Ultra-flexible polyphenylene sulfide fiber aerogel elastomer and preparation method and application thereof
By using a combination of island melt composite spinning technology and organosiloxane in polyphenylene sulfide fiber aerogels, the problems of insufficient molding and performance of polyphenylene sulfide fiber aerogels are solved, and high porosity is achieved , airgel materials with low thermal conductivity and excellent resilience, suitable for a variety of high-performance applications.
Patent Information
- Application Number
- CN202310237953.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2022-09-28
- Filing Date
- 2023-03-10
- Publication Date
- 2024-10-08
- Estimated Expiration
- 2043-03-10
AI Technical Summary
Traditional polyphenylene sulfide fiber aerogels are difficult to mold, have high thermal conductivity, and poor resilience and flexibility, which limits their application in high-performance flexible fields.
By dispersing 0.5-5mm polyphenylene sulfide ultrafine fibers into a hydroxymethylcellulose aqueous solution, combining an organosiloxane containing hydrophobic groups with an acid-containing aqueous solution, hydrolyzing and stirring, and freeze-drying, an ultra-flexible polyester is produced. Phenyl sulfide fiber aerogel elastomer uses island melt composite spinning technology to improve the flexibility and resilience of the fiber.
The prepared ultra-flexible polyphenylene sulfide fiber airgel elastomer has excellent resilience, flexibility, high porosity, low thermal conductivity and thermal stability, and is suitable for a variety of applications, including thermal insulation, sound insulation, and vibration. Absorbent and catalytic materials.
Smart Images

Figure CN116575240B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of fiber manufacturing, and in particular to an ultra-flexible polyphenylene sulfide fiber aerogel elastomer and a preparation method and application thereof. Background Art
[0002] As a solid material with a three-dimensional porous network structure, aerogel has the characteristics of low density, high porosity and large specific surface area, which makes it possible to be used in flame retardant insulation, filtration adsorption, shock absorption, sound absorption and other fields. In order to meet the needs of aerogel in the fields of national defense, aerospace and civil use, aerogel not only needs excellent comprehensive performance, thermal stability and low thermal conductivity, but also should pursue flexibility, high elasticity, simple and convenient preparation methods, large-scale production, etc. Traditional inorganic aerogels have poor mechanical strength, high brittleness and easy breakage under force, which greatly limits their application in the field of high-performance flexibility. Organic aerogels (polyurethane, polyurea, chitosan aerogels) have the disadvantage of poor thermal stability. Therefore, designing a new type of aerogel with excellent mechanical properties, good thermal stability, low thermal conductivity, good flexibility and good resilience is still a challenging problem in this field.
[0003] Polyphenylene sulfide (PPS) is a polymer containing repeating structural units of p-phenylene sulfide in the main chain. It is a new functional engineering plastic with good heat resistance, excellent chemical corrosion resistance and flame retardancy. It can be widely used in high-temperature filtration, special protective clothing, thermal insulation materials, battery separators and other fields. At present, there is no report on polyphenylene sulfide fiber aerogel. The main reason is that the aerogel made of polyphenylene sulfide fiber is not easy to form, or after forming, the thermal conductivity is high, and the resilience and flexibility are poor, which leads to limited application and cannot meet application requirements. Summary of the invention
[0004] Based on this, the present invention provides an ultra-flexible polyphenylene sulfide fiber aerogel elastomer and a preparation method and application thereof to solve the technical problem that the prior art cannot well use polyphenylene sulfide materials to make micro / nano fibers and use them as aerogels.
[0005] To achieve the above object, the present invention provides a method for preparing an ultra-flexible polyphenylene sulfide fiber aerogel elastomer, which comprises the following steps:
[0006] S1. Dispersing 0.5-5 mm polyphenylene sulfide superfine fibers into a hydroxymethyl cellulose aqueous solution in proportion to obtain a polyphenylene sulfide superfine fiber dispersion, wherein the mass fraction of the polyphenylene sulfide superfine fibers with a length of 0.5-1 mm is 0-30%, the mass fraction of the polyphenylene sulfide superfine fibers with a length of 1-2 mm is 50-100%, and the mass fraction of the polyphenylene sulfide superfine fibers with a length of 2-5 mm is 0-30%;
[0007] S2. The organic siloxane containing hydrophobic groups is mixed with an acid-containing aqueous solution for hydrolysis, and then mixed with a polyphenylene sulfide ultrafine fiber aqueous dispersion, stirred, frozen, and vacuum freeze-dried. After drying, the ultra-flexible polyphenylene sulfide fiber aerogel elastomer is obtained by dehydration and polycondensation.
[0008] As a further preferred technical solution of the present invention, the polyphenylene sulfide ultrafine fibers described in step S1 are made from a mixture of polyphenylene sulfide and alkali-soluble polyester, are formed by sea-island melt spinning, followed by stretching and heat setting, and then are alkaline hydrolyzed and cut.
[0009] As a further preferred technical solution of the present invention, the diameter of the polyphenylene sulfide ultrafine fiber prepared in step S1 is 0.5-1.5 μm, and the fiber is round.
[0010] As a further preferred technical solution of the present invention, the organosiloxane containing a hydrophobic group in step S2 is at least one of methyltrimethoxysilane, ethyltrimethoxysilane, vinyltrimethoxysilane, and propyltrimethoxysilane; and the acid-containing aqueous solution is acetic acid, oxalic acid, or hydrochloric acid with a concentration of 0.01 to 6 mmol / L.
[0011] As a further preferred technical solution of the present invention, in step S2, the hydrolysis time is 15 to 30 minutes; the stirring time is 1 to 3 hours; the freezing is freezing in liquid nitrogen; the process conditions of vacuum freeze drying are: freeze drying polymerization in a vacuum environment with a vacuum degree lower than 30 Pa for 2 to 3 days; the drying, dehydration and condensation process is performed at a temperature of 40 to 90°C for 8 to 48 hours.
[0012] As a further preferred technical solution of the present invention, in step S2, in the mixture after adding the polyphenylene sulfide ultrafine fiber aqueous dispersion: the mass fraction of polyphenylene sulfide ultrafine fiber is 35%-90%, the mass fraction of organic polysiloxane is 9%-64%, and the mass fraction of hydroxymethyl cellulose is 0.1%-1%.
[0013] According to another aspect of the present invention, the present invention also provides an ultra-flexible polyphenylene sulfide fiber aerogel elastomer, which is prepared by the preparation method of an ultra-flexible polyphenylene sulfide fiber aerogel elastomer. The ultra-flexible polyphenylene sulfide fiber aerogel elastomer is an organic-inorganic hybrid fiber with polyphenylene sulfide ultrafine fibers as a base material and an organic polysiloxane nanolayer as a coating layer.
[0014] According to another aspect of the present invention, the present invention also provides an application of an ultra-flexible polyphenylene sulfide fiber aerogel elastomer, wherein the ultra-flexible polyphenylene sulfide fiber aerogel elastomer is applied to thermal insulation materials, sound insulation materials, vibration absorption materials, catalytic materials, oil absorption materials, three-dimensional skeletons of flexible functional materials, pressure sensing materials or magnetic response materials.
[0015] The ultra-flexible polyphenylene sulfide fiber aerogel elastomer of the present invention and its preparation method and application can achieve the following beneficial effects by adopting the above technical scheme:
[0016] 1) The present invention utilizes the good heat resistance, excellent chemical corrosion resistance and flame retardancy of polyphenylene sulfide (PPS), and obtains the sea-island type polyphenylene sulfide fiber aerogel by melt-spinning, alkaline hydrolysis, dispersion and sufficient stirring with organic siloxane, and finally freezing and freeze drying. The aerogel has excellent resilience, flexibility, thermal stability, chemical stability and other properties, and the preparation process of the present invention is simple and convenient, does not require the use of organic solvents, and is suitable for large-scale production;
[0017] 2) The present invention can prepare polyphenylene sulfide ultrafine fibers with a diameter of 0.5-1.5 um through sea-island melt composite spinning, and improve the flexibility and resilience of polyphenylene sulfide fiber aerogel by hybridizing organic siloxane with polyphenylene sulfide ultrafine fibers;
[0018] 3) The ultra-flexible polyphenylene sulfide fiber aerogel elastomer of the present invention has excellent resilience, flexibility, high porosity, low thermal conductivity and other properties, and also has excellent thermal stability and flame retardancy, which can meet the use requirements of aerogels in various environments. Compared with the aerogel elastomers in the prior art, it has better flexibility and can be folded repeatedly without breaking or cracking, making it more applicable and can be applied to more fields.
[0019] In summary, the preparation method of the ultra-flexible polyphenylene sulfide fiber aerogel elastomer provided by the present invention has a simple and convenient preparation process, does not require the use of organic solvents, is suitable for large-scale production, and regulates the polyphenylene sulfide fiber aerogel to improve the flexibility and resilience of the aerogel. The obtained ultra-flexible polyphenylene sulfide fiber aerogel elastomer has excellent resilience, flexibility, high porosity, low thermal conductivity, thermal stability and flame retardancy.
[0020] In addition, the ultra-flexible polyphenylene sulfide fiber aerogel elastomer prepared by the preparation method of the present invention is suitable for the fields of heat insulation, sound absorption, oil absorption, warmth preservation, etc. BRIEF DESCRIPTION OF THE DRAWINGS
[0021] The present invention will be further described in detail below in conjunction with the accompanying drawings and specific embodiments.
[0022] Figure 1 This is a scanning electron microscope image of the island-in-sea type polyphenylene sulfide ultrafine fiber prepared in Example 1 of the present invention;
[0023] Figure 2 This is a scanning electron microscope image of the ultra-flexible polyphenylene sulfide fiber aerogel elastomer prepared in Example 1 of the present invention;
[0024] Figure 3The actual object and flexibility performance test diagram of the ultra-flexible polyphenylene sulfide fiber aerogel elastomer prepared in Example 1 of the present invention;
[0025] Figure 4 This is the elastic deformation curve of the ultra-flexible polyphenylene sulfide fiber aerogel elastomer prepared in Example 1 of the present invention;
[0026] Figure 5 The contact angle of the ultra-flexible polyphenylene sulfide fiber aerogel elastomer prepared in Example 1 of the present invention;
[0027] Figure 6 Curve showing the change in mass of the ultra-flexible polyphenylene sulfide fiber aerogel elastomer prepared in an embodiment of the present invention as a function of temperature.
[0028] The purpose, features and advantages of the present invention will be further described with reference to the accompanying drawings in conjunction with the embodiments. DETAILED DESCRIPTION
[0029] The present invention will be further described below in conjunction with the accompanying drawings and specific embodiments. The terms such as "upper", "lower", "left", "right", "middle" and "one" cited in the preferred embodiments are only for the convenience of description, and are not used to limit the scope of the present invention. The change or adjustment of the relative relationship shall also be regarded as the scope of the present invention without substantially changing the technical content.
[0030] Examples 1-6
[0031] Examples 1-6 are respectively methods for preparing ultra-flexible polyphenylene sulfide fiber aerogel elastomers. The process parameters in the preparation process are shown in Table 1. The specific preparation process includes the following steps:
[0032] S1. Preparation of polyphenylene sulfide ultrafine fibers:
[0033] First, polyphenylene sulfide particles / powder (PPS) and alkali-soluble polyester (PET) with a melt index of 10-50g / 10min are dried at a temperature of 80-160°C for 12-24h, and then mixed at a mass ratio of 2:8-8:2, and subjected to sea island melt spinning to obtain circular polyphenylene sulfide ultrafine fiber filaments with a diameter of 0.5-1.5μm; during the melt spinning process, the screw extrusion temperature is 315-325°C, the screw melt pressure is 60-120bar, the spinning box temperature is 315-325°C, the spinning assembly pressure is less than 60kgf / cm2, the spinning speed is 600-1000m / min, and the draft multiple is 3.6-4.3 times;
[0034] Then, the polyphenylene sulfide ultrafine fiber filaments are dissolved in a sodium hydroxide solution to remove the PET component, the dissolution concentration is 5-15%, the time is 60-300 minutes, the temperature is 60-90° C., and then the fibers are cut into short pieces to obtain polyphenylene sulfide ultrafine fibers with a fiber length of 0.5-5 mm;
[0035] S2. Preparation of polyphenylene sulfide ultrafine fiber dispersion:
[0036] The polyphenylene sulfide ultrafine fibers cut into 0.5-5 mm lengths are dispersed in a hydroxymethyl cellulose aqueous solution according to different length distribution ratios to obtain a polyphenylene sulfide ultrafine fiber dispersion, wherein the polyphenylene sulfide ultrafine fiber solid content is 0.2-0.6% and the hydroxymethyl cellulose dispersant concentration is 0.1-1%.
[0037] S3. Preparation of ultra-flexible polyphenylene sulfide fiber aerogel:
[0038] The organic siloxane containing a hydrophobic group is mixed with an acid-containing aqueous solution with a concentration of 0.01 to 6 mmol / L for hydrolysis, and then mixed with a polyphenylene sulfide ultrafine fiber aqueous dispersion, wherein the mass fraction of the polyphenylene sulfide ultrafine fiber is 35%-90%, the mass fraction of the organic polysiloxane is 9%-64%, and the mass fraction of hydroxymethyl cellulose is 0.1%-1%. The mixture is then stirred, frozen, freeze-dried, and subjected to dehydration and polycondensation treatment to obtain an ultra-flexible polyphenylene sulfide fiber aerogel elastomer.
[0039] Table 1. Process parameters for preparing ultra-flexible polyphenylene sulfide fiber aerogel elastomers in Examples 1-6
[0040]
[0041] The specific performance indicators of the ultra-flexible polyphenylene sulfide fiber aerogel elastomer prepared by the above preparation method are shown in Table 2.
[0042] Table 2. Performance indicators of ultra-flexible polyphenylene sulfide fiber aerogel elastomers prepared in Examples 1-6
[0043]
[0044] As shown in Table 2, the porosity of the ultra-flexible polyphenylene sulfide fiber aerogel elastomers prepared in Examples 1-6 is 90-95%, the contact angle is 140-164°, the thermal conductivity is lower than 0.032W / (m·K), the recovery elastic deformation is 86-96%, and the thermal stability is greater than 320°C. The high porosity of the aerogel is conducive to its application in the fields of heat insulation, sound absorption, and warmth preservation, and the super-hydrophobicity is conducive to the oil absorption of the aerogel. In addition, the polyphenylene sulfide fiber aerogel can be folded repeatedly, indicating excellent flexibility.
[0045] Polyphenylene sulfide ultrafine fibers are used as aerogel skeleton materials, and their surface is coated with an organic polysiloxane nano-inorganic layer. The high aspect ratio of polyphenylene sulfide ultrafine fibers gives the aerogel good flexibility, and the inorganic hybrid layer and surface coating give the aerogel excellent heat resistance, which can greatly improve the flame retardant properties of the aerogel.
[0046] Taking the product of Example 1 as an example, the following tests were carried out respectively:
[0047] The scanning electron microscope image of the polyphenylene sulfide ultrafine fiber prepared in Example 1 is as follows: Figure 1 As shown, the diameter of the polyphenylene sulfide ultrafine fibers was measured to be between 0.5 and 1.5 μm. Figure 2 This is a scanning electron microscope image of the ultra-flexible polyphenylene sulfide fiber aerogel elastomer in Example 1, and its structure is: the organic siloxane forms a sheet layer, and the fiber is coated or interspersed therein, which is conducive to improving the resilience of the polyphenylene sulfide fiber aerogel; Figure 3 This is a physical picture of the ultra-flexible polyphenylene sulfide fiber aerogel elastomer of Example 1, Figure 3 It can be seen that the aerogel elastomers of various shapes in (a) are repeatedly folded according to the method of (b). It can be seen that the polyphenylene sulfide aerogel elastomer can be completely folded without breaking, indicating that the polyphenylene sulfide fiber aerogel elastomer has good flexibility; Figure 4 This is the elastic deformation curve of the ultra-flexible polyphenylene sulfide fiber aerogel elastomer of Example 1, from which it can be seen that the polyphenylene sulfide aerogel can still fully recover after being compressed by 30%, 60%, and 80%, indicating that it has excellent resilience; Figure 5 is the contact angle of the ultra-flexible polyphenylene sulfide fiber aerogel elastomer of Example 1, which is greater than 150°, indicating that it has super-hydrophobic properties; Figure 6 is the curve of the mass change of the ultra-flexible polyphenylene sulfide fiber aerogel elastomer of Example 1 with temperature, Figure 6 It can be seen that after exceeding 500°C, the quality of the ultra-flexible polyphenylene sulfide fiber aerogel elastomer begins to decline significantly, showing excellent thermal stability.
[0048] In order to further study the properties of the ultra-flexible polyphenylene sulfide fiber aerogel elastomer of the present invention, Examples 7-10 were proposed according to the same preparation method and process parameters as Example 1, except that the distribution of the length of the polyphenylene sulfide ultrafine fibers was different (i.e., the content of polyphenylene sulfide ultrafine fibers of different lengths was different). The specific process parameters and the corresponding product performance indicators are shown in Table 3.
[0049] According to the different fiber lengths, when the fiber length is 100% distributed in the range of 0.5-1mm, as in Example 7, the fibers are well dispersed and easy to form, but due to the poor entanglement force between the fibers, the flexibility of the aerogel is poor and the resilience effect is not good; when the fiber length is 100% distributed in the range of 1-2mm, as in Example 8, the entanglement force between the fibers is enhanced, the resilience and flexibility are improved, and the thermal conductivity is reduced; when the fiber length is 100% distributed in the range of 2-5mm, as in Example 9, the fibers are severely entangled, cannot be evenly dispersed in the dispersion, and cannot be formed to prepare aerogel, and ultimately no aerogel elastomer is obtained; when the fiber distribution is 0.5-1mm (25%), 1-2mm (50%), 2-5mm (25%), as in Example 10, short fibers are conducive to dispersion, long fibers are conducive to entanglement, and the intermediate length fibers are used as the skeleton of the aerogel, with better resilience and flexibility, and the thermal conductivity is further reduced (the smaller the thermal insulation effect, the better), indicating that its structure is more reasonable and the various properties of the prepared aerogel are excellent. In addition, the following test was conducted. When the fiber length was 100% distributed below 0.5 mm, the prepared aerogel did not show flexibility and resilience effects; and when the fiber length was 100% distributed above 5 mm, aerogel could not be formed and prepared.
[0050] Table 3 Process parameters for preparing ultra-flexible polyphenylene sulfide fiber aerogel elastomers in Examples 7-9
[0051]
[0052] It can be seen that the content distribution of polyphenylene sulfide ultrafine fibers of different lengths mainly affects resilience, flexibility, and thermal conductivity, and the aerogel prepared by mixing the three is better than that of single-component length fibers. The aerogel elastomer prepared by mixing polyphenylene sulfide ultrafine fibers of different lengths has better resilience and higher thermal conductivity. The reason is that too many long fibers have poor dispersion and poor molding, resulting in poor performance; although too many short fibers have good dispersion, their entanglement ability is poor, resulting in poor resilience. Through many experiments, it was concluded that the best choice is to mix and match three types of polyphenylene sulfide ultrafine fibers of different lengths.
[0053] In order to explore the effect of the component content of organic polysiloxane on product performance, Examples 10-12 were proposed according to the same preparation method and process parameters as Example 1, only the content of the components of polyphenylene sulfide ultrafine fibers and organic polysiloxane was changed. The specific process parameters and corresponding product performance indicators are shown in Table 4.
[0054] Table 4 Process parameters for preparing ultra-flexible polyphenylene sulfide fiber aerogel elastomers in Examples 10-12
[0055]
[0056] It can be seen that the concentration of organosiloxane is crucial to the stability of the aerogel structure. When its concentration decreases, its resilience becomes worse, the structure collapses, and the thermal conductivity increases (the thermal insulation effect becomes worse).
[0057] The present invention also provides an ultra-flexible polyphenylene sulfide fiber aerogel elastomer, which is prepared by the preparation method of the ultra-flexible polyphenylene sulfide fiber aerogel elastomer described in any of the above embodiments. The ultra-flexible polyphenylene sulfide fiber aerogel elastomer is an organic-inorganic hybrid fiber with polyphenylene sulfide ultrafine fibers as a substrate and an organic polysiloxane nanolayer as a coating layer. The polyphenylene sulfide ultrafine fibers and the organic polysiloxane are connected by hydrogen bond interaction and chemical bonding.
[0058] The present invention also provides an application of an ultra-flexible polyphenylene sulfide fiber aerogel elastomer, wherein the ultra-flexible polyphenylene sulfide fiber aerogel elastomer is applied to thermal insulation materials, sound insulation materials, vibration absorption materials, catalytic materials, oil absorption materials, three-dimensional skeletons of flexible functional materials, pressure sensing materials or magnetic response materials.
[0059] Although specific embodiments of the present invention are described above, those skilled in the art should understand that these are merely examples and that various changes or modifications may be made to the embodiments without departing from the principles and essence of the present invention. The scope of protection of the present invention is limited only by the appended claims.
Claims
1. A method for preparing an ultra-flexible polyphenylene sulfide fiber aerogel elastomer, characterized in that: The following steps are involved: S1. Dispersing 0.5-5 mm polyphenylene sulfide superfine fibers into a hydroxymethyl cellulose aqueous solution in proportion to obtain a polyphenylene sulfide superfine fiber dispersion, wherein the mass fraction of the polyphenylene sulfide superfine fibers with a length of 0.5-1 mm is 10-30%, the mass fraction of the polyphenylene sulfide superfine fibers with a length of greater than 1 mm and less than 2 mm is 50-80%, and the mass fraction of the polyphenylene sulfide superfine fibers with a length of 2-5 mm is 10-30%; S2, mixing the organosiloxane containing a hydrophobic group with an acid-containing aqueous solution for hydrolysis, and then mixing it with a polyphenylene sulfide ultrafine fiber aqueous dispersion, stirring, freezing, vacuum freeze drying, and drying and dehydrating and polycondensing to obtain an ultra-flexible polyphenylene sulfide fiber aerogel elastomer; In step S2, in the mixture after adding the polyphenylene sulfide ultrafine fiber aqueous dispersion, the mass fraction of the polyphenylene sulfide ultrafine fiber is 35%-90%, the mass fraction of the organopolysiloxane is 9%-64%, and the mass fraction of the hydroxymethyl cellulose is 0.1%-1%.
2. The method for preparing the ultra-flexible polyphenylene sulfide fiber aerogel elastomer according to claim 1, characterized in that: The polyphenylene sulfide ultrafine fibers described in step S1 are made from a mixture of polyphenylene sulfide and alkali-soluble polyester, are produced by sea-island melt spinning, stretching and heat setting, and then alkaline hydrolysis and shortening.
3. The method for preparing the ultra-flexible polyphenylene sulfide fiber aerogel elastomer according to claim 1, characterized in that: The diameter of the polyphenylene sulfide ultrafine fiber prepared in step S1 is 0.5-1.5 μm, and the fiber is round.
4. The method for preparing the ultra-flexible polyphenylene sulfide fiber aerogel elastomer according to claim 1, characterized in that: In step S2, the organosiloxane containing a hydrophobic group is at least one of methyltrimethoxysilane, ethyltrimethoxysilane, vinyltrimethoxysilane, and propyltrimethoxysilane; and the acid-containing aqueous solution is acetic acid, oxalic acid, or hydrochloric acid with a concentration of 0.01 to 6 mmol / L.
5. The method for preparing the ultra-flexible polyphenylene sulfide fiber aerogel elastomer according to claim 1, characterized in that: In step S2, the hydrolysis time is 15 to 30 minutes; the stirring time is 1 to 3 hours; the freezing is performed in liquid nitrogen; the process conditions of vacuum freeze drying are: freeze drying polymerization for 2 to 3 days in a vacuum environment with a vacuum degree lower than 30 Pa; the drying, dehydration and condensation process is performed at a temperature of 40 to 90° C. for 8 to 48 hours.
6. An ultra-flexible polyphenylene sulfide fiber aerogel elastomer, characterized in that: The ultra-flexible polyphenylene sulfide fiber aerogel elastomer is prepared by the preparation method of any one of claims 1 to 5. The ultra-flexible polyphenylene sulfide fiber aerogel elastomer is an organic-inorganic hybrid fiber with polyphenylene sulfide ultrafine fibers as a base material and an organic polysiloxane nanolayer as a coating layer.
7. An application of the ultra-flexible polyphenylene sulfide fiber aerogel elastomer according to claim 6, characterized in that: The ultra-flexible polyphenylene sulfide fiber aerogel elastomer is applied to thermal insulation materials, sound insulation materials, vibration absorption materials, catalytic materials, oil absorption materials, three-dimensional skeletons of flexible functional materials, pressure sensing materials or magnetic response materials.