Solid electrolytic capacitors

By forming a rough surface with an unfolded area ratio of 0.4 or higher at the contact surface between the lead terminals and the outer casing, the problem of insufficient sealing between the lead terminals and the outer casing is solved, achieving effective isolation from oxygen and moisture and improving the long-term reliability of the capacitor.

CN116601730BActive Publication Date: 2026-11-17PANASONIC INTELLECTUAL PROPERTY MANAGEMENT CO LTD
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202180079287.X
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2020-11-30
Filing Date
2021-11-25
Publication Date
2026-11-17
Estimated Expiration
2041-11-25

AI Technical Summary

Technical Problem

Existing solid electrolytic capacitors have insufficient sealing between the lead terminals and the outer casing, which makes it easy for oxygen and moisture to penetrate and cause capacitor deterioration.

Method used

By forming a rough surface with an unfolded area ratio of 0.4 or higher on the contact surface of the lead terminal, the tightness between the lead terminal and the outer casing can be improved. Specific methods include sandblasting, roughening plating, and roughening etching to form a rough surface to increase the unfolded area ratio of the interface.

Benefits of technology

It effectively inhibits the intrusion of oxygen and other substances, improves the long-term reliability and sealing of solid electrolytic capacitors, and slows down the degradation process of capacitors.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116601730B_ABST
    Figure CN116601730B_ABST
Patent Text Reader

Abstract

A solid electrolytic capacitor includes: at least one capacitor element comprising an anode portion and a cathode portion, an anode lead terminal, a cathode lead terminal, and an outer casing covering the at least one capacitor element. The anode lead terminal and the cathode lead terminal each include an embedded portion embedded in the outer casing. The embedded portion of the anode lead terminal has a first contact surface that contacts the outer casing, and the embedded portion of the cathode lead terminal has a second contact surface that contacts the outer casing. At least one contact surface selected from the first and second contact surfaces has a rough surface with an interface unfolded area ratio of 0.4 or higher.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to solid electrolytic capacitors. Background Technology

[0002] Solid electrolytic capacitors include: capacitor elements with a solid electrolyte layer, lead terminals electrically connected to the capacitor elements, and an outer casing that seals the capacitor elements.

[0003] The outer casing prevents oxygen and moisture from the atmosphere from reaching the capacitor elements and causing them to deteriorate. However, if the seal between the lead terminals and the outer casing is poor, oxygen and moisture can easily penetrate through this interface, leading to the deterioration of the solid electrolytic capacitor.

[0004] Japanese Patent Document 1 (Japanese Patent Application Publication No. 4-253314) discloses "a solid electrolytic capacitor, wherein an oxide film, a conductive material layer, a conductive polymer film, and a conductor layer are sequentially formed on the surface of a valve metal to form a capacitor element, and a lead frame, which serves as a lead terminal, is connected to the valve metal portion and the conductor layer portion of the capacitor element, and then the capacitor element and a portion of the lead frame are externally packaged with molding resin. The solid electrolytic capacitor is characterized in that the lead frame has a copper metal layer on its surface, and its surface is roughened."

[0005] Existing technical documents

[0006] Patent documents

[0007] Patent Document 1: Japanese Patent Application Publication No. 4-253314 Summary of the Invention

[0008] A solid electrolytic capacitor according to one aspect of the present invention includes: at least one capacitor element comprising an anode portion and a cathode portion, an anode lead terminal electrically connected to the anode portion, a cathode lead terminal electrically connected to the cathode portion, and an outer casing covering the at least one capacitor element. Each of the anode lead terminal and the cathode lead terminal includes an embedded portion embedded in the outer casing and an exposed portion connected to the embedded portion and exposed from the outer casing. The embedded portion of the anode lead terminal has a first contact surface that contacts the outer casing, and the embedded portion of the cathode lead terminal has a second contact surface that contacts the outer casing. At least one of the first contact surface and the second contact surface has a rough surface with an interface unfolded area ratio of 0.4 or more.

[0009] According to the present invention, a solid electrolytic capacitor capable of particularly suppressing deterioration caused by the intrusion of oxygen, etc., can be obtained. Attached Figure Description

[0010] Figure 1This is a cross-sectional view of a solid electrolytic capacitor, schematically illustrating an example of an embodiment of the present invention.

[0011] Figure 2 This is an image representing an example of the state of the rough surface of capacitor C2.

[0012] Figure 3 This is an image representing an example of the state of the rough surface of capacitor A2. Detailed Implementation

[0013] Before describing the implementation methods, the issues in the prior art are briefly shown below.

[0014] There is now a need to further suppress degradation caused by the intrusion of oxygen and the like. In this context, one object of the present invention is to provide a novel solid electrolytic capacitor capable of particularly suppressing degradation caused by the intrusion of oxygen and the like.

[0015] In view of the above-mentioned problems, the present invention provides a paste for forming an electrolytic capacitor and an electrolytic capacitor that can particularly suppress the deterioration caused by the intrusion of oxygen, etc.

[0016] Hereinafter, examples of embodiments of the present invention will be described. It should be noted that the following description illustrates embodiments of the present invention by way of example, but the present invention is not limited to the examples described below. In the following description, specific numerical values ​​and materials are illustrated, but other numerical values ​​and materials can be applied as long as the effects of the present invention can be obtained. In this specification, when referred to as "numerical value A to numerical value B," the range includes both numerical value A and numerical value B.

[0017] (Solid electrolytic capacitor)

[0018] The solid electrolytic capacitor of this embodiment includes: at least one capacitor element comprising an anode portion and a cathode portion, an anode lead terminal electrically connected to the anode portion, a cathode lead terminal electrically connected to the cathode portion, and an outer casing covering the at least one capacitor element. Each of the anode lead terminal and the cathode lead terminal includes an embedded portion embedded in the outer casing and an exposed portion connected to the embedded portion and protruding from the outer casing. The embedded portion of the anode lead terminal has a contact surface p (first contact surface) that contacts the outer casing. The embedded portion of the cathode lead terminal has a contact surface n (second contact surface) that contacts the outer casing. At least one contact surface selected from contact surface p and contact surface n has a rough surface with an interface unfolded area ratio of 0.4 or more. Hereinafter, a rough surface with an interface unfolded area ratio of 0.4 or more is sometimes referred to as a "rough surface (R)". The interface unfolded area ratio can be measured by the method described later.

[0019] Conventional methods for improving the fit between lead terminals and the outer casing have involved roughening the surface of the lead terminals using methods such as sandblasting. However, as a result of research, the inventors of this application have recently discovered that even when roughening the surface of the lead terminals using conventional methods, sometimes insufficient results are not achieved. This invention is based on this new insight.

[0020] If the adhesion between the contact surface and the outer casing is poor, oxygen and other contaminants can easily penetrate from the interface between the contact surface and the outer casing. Although previously unknown, as shown in the embodiments, by having a rough surface (R) on the contact surface, it is possible to suppress the penetration of oxygen and other contaminants from the interface between the contact surface and the outer casing. This is believed to be because having a rough surface (R) on the contact surface improves the adhesion between the contact surface and the outer casing.

[0021] Oxygen and other substances in the atmosphere can penetrate from the surface of the outer casing into its interior. Therefore, the rough surface (R) is preferably formed extending from the boundary between the embedded part and the exposed part into the interior of the outer casing.

[0022] A rough surface (R) can also be formed from the embedded portion to the exposed portion, thus also forming on at least a portion of the exposed portion. When sealing is achieved using an outer casing, the outer surface of the outer casing may sometimes be offset relative to the lead terminal. By forming the rough surface (R) in a manner that extends from the embedded portion to the exposed portion, the embedded portion can reliably have a rough surface (R).

[0023] When a rough surface (R) is also formed on the exposed portion, there is no particular limitation on the extent to which the rough surface (R) is formed. The length L of the rough surface (R) from the boundary between the embedded portion and the exposed portion (i.e., the contact portion between the exposed portion and the outer casing) is preferably 0.3 mm or more, and may also be 0.5 mm or more. Here, the length L is the length along the surface of the exposed portion, and is the apparent length assuming the surface of the exposed portion is smooth. There is no particular upper limit to the length L, and the entire surface of the exposed portion may be rough surface (R).

[0024] At least one of the contact surfaces p and n has a rough surface (R). In a preferred example, both contact surfaces p and n have a rough surface (R).

[0025] The effectiveness of the present invention can be improved by increasing the proportion of the rough surface (R) in the contact surface. The area of ​​the rough surface (R) in the area of ​​the contact surface p is preferably 50% or more, more preferably 80% or more (e.g., 90% or more). The area of ​​the rough surface (R) in the area of ​​the contact surface n is preferably 50% or more, more preferably 80% or more (e.g., 90% or more). Alternatively, both the contact surfaces p and n may be entirely rough surfaces (R). It should be noted that the area referred to here is the apparent area, and is the area assuming a smooth surface.

[0026] It should be noted that the surface of the lead terminal may also have a rough surface (R) other than the contact surface that contacts the outer casing. For example, the surface of the cathode lead terminal that is electrically connected to the cathode portion may also be a rough surface (R) with an interface unfolded area ratio of 0.4 or more. The area of ​​the rough surface (R) may account for 50% or more, 80% or more, or 90% or more of the area of ​​the embedded portion. Alternatively, the entire surface of the embedded portion may be a rough surface (R).

[0027] As described above, the unfolded area ratio of the rough surface (R) interface is 0.4 or higher. There is no particular upper limit to the unfolded area ratio of the rough surface (R) interface, but by setting this unfolded area ratio below a certain value, lead terminals can be easily manufactured. The unfolded area ratio of the rough surface (R) interface can be 10.0 or lower, 6.0 or lower, 4.0 or lower, 2.0 or lower, 1.0 or lower, or 0.6 or lower. This unfolded area ratio can be within the range specified by either the upper limit or the lower limit (0.4 or higher) described herein. For example, the unfolded area ratio of the rough surface (R) interface can be in the range of 0.4 to 10.0, 0.4 to 6.0, 0.4 to 4.0, 0.4 to 2.0, 0.4 to 1.0, or 0.4 to 0.6.

[0028] A preferred example of the solid electrolytic capacitor of the present invention satisfies the following conditions (1) and (2), and can further satisfy condition (3).

[0029] (1) The proportion of the area of ​​the rough surface (R) in the area of ​​the contact surface p and the proportion of the area of ​​the rough surface (R) in the area of ​​the contact surface n are each 50% or more, and can be 80% or more (e.g., 90% or more). Alternatively, both the contact surface p and the contact surface n can be rough surfaces (R). In this condition (1), the area of ​​the contact surface p and the area of ​​the contact surface n can be renamed as the area of ​​the embedded part of the anode lead terminal and the area of ​​the embedded part of the cathode lead terminal, respectively.

[0030] (2) The unfolded area ratio of the rough surface (R) is 0.4 or more. The unfolded area ratio of this interface can be 10.0 or less, or it can be within the range shown above.

[0031] (3) A rough surface (R) is formed extending from the boundary between the embedded part and the exposed part into the interior of the outer body. The rough surface (R) may also be formed by crossing from the embedded part to the exposed part, and thus also formed on at least a portion of the exposed part.

[0032] At least one substrate selected from the substrates of the anode lead terminal and the cathode lead terminal can be a copper substrate. In this case, at least a portion of the copper substrate in the exposed portion can be coated with a copper plating layer. In a preferred embodiment, both the substrates of the anode lead terminal and the substrates of the cathode lead terminal are copper substrates. In this case, at least a portion of the copper substrates of both can be coated with a copper plating layer. The entire surface of the exposed portion can be coated with a copper plating layer.

[0033] Rolled copper sheets can be used as the copper substrate (lead frame). However, rolled copper sheets have a metallic structure that extends along the rolling direction. When making the lead frame by punching the rolled copper sheet, depending on the direction of punching the rolled copper sheet, the direction of the ridge line at the bending position of the lead terminal can be approximately parallel to the direction of the metallic structure's extension. In this case, at the peak side of the bending position, the spacing between the metallic structures widens due to bending, sometimes resulting in cracking. As a result, the plating formed on the copper substrate (e.g., tin plating) is sometimes subjected to tensile stress, causing cracking in the plating and reducing the wettability of the solder.

[0034] When a tin plating layer is directly applied to the surface of a copper substrate, an alloy layer of copper and tin is formed between the copper substrate and the tin plating layer due to the heat during installation. This copper-tin alloy layer is harder than copper and tin alone and is less malleable, thus failing to alleviate the stress caused by cracking in the copper substrate and easily leading to cracking in the alloy layer. Consequently, cracking also occurs in the tin plating layer, potentially reducing solder wettability. Forming a copper plating layer on the copper substrate, however, allows for the mitigation of stress caused by cracking in the copper substrate through its excellent ductility. Furthermore, the copper plating layer has good affinity with the copper substrate, which is also primarily composed of copper, and easily fills in the unevenness caused by cracks in the copper substrate. Therefore, the formation of cracks in both the copper plating layer and the coating layer is suppressed, and the reduction in solder wettability is also prevented. Thus, the reliability of the electrical connection between the solid electrolytic capacitor and the external substrate can be improved. It should be noted that, because the copper plating layer has a metallic structure perpendicular to the extension direction of the copper substrate, it is possible to distinguish the copper substrate from the copper plating layer covering the copper substrate by means of observation, for example, under a microscope, and to identify the boundary between the copper substrate and the copper plating layer.

[0035] The thickness of the copper plating layer is preferably 2 μm or more. By setting the thickness to 2 μm or more, the tensile stress caused by cracking of the copper substrate can be effectively mitigated, and the formation of cracks in the copper plating layer and the coating layer can be effectively suppressed. As a result, the effect of suppressing the reduction of solder wettability can be improved. The thickness of the copper plating layer can be, for example, 10 μm or less or 15 μm or less.

[0036] The copper substrate may have a curved portion in the exposed portion that bends along the outer surface of the outer casing. In this case, the outer surface of the curved portion may be coated with a copper plating layer. Due to the high stress applied to the curved portion, it is preferable to coat this portion with a copper plating layer.

[0037] The solid electrolytic capacitor (more specifically, the lead terminal) of this embodiment may further include a tin plating layer covering the copper plating layer described above. In this case, the solid electrolytic capacitor (more specifically, the lead terminal) may further include other layers disposed between the copper plating layer and the tin plating layer. These other layers may be an alloy layer of copper and tin or a nickel plating layer. The tin plating layer improves the wettability of the solder and enhances the reliability of the electrical connection between the solid electrolytic capacitor and the external substrate. It should be noted that when a tin plating layer is formed on the copper plating layer, sometimes the tin (Sn) in the tin plating layer diffuses into the copper plating layer due to heat during installation, forming an alloy layer of copper and tin between the copper plating layer and the tin plating layer. Alternatively, a nickel plating layer may be formed between the copper plating layer and the tin plating layer.

[0038] The solid electrolytic capacitor (more specifically, the lead terminals) of this embodiment may further include a noble metal plating layer covering the copper plating layer described above. The noble metal plating layer may include at least one selected from gold, platinum, and palladium.

[0039] The solid electrolytic capacitor (more specifically, lead terminals) of this embodiment may further include a nickel plating layer disposed between the copper plating layer and the noble metal plating layer.

[0040] Hereinafter, the layer (such as the aforementioned plating layer) formed on the substrate of the lead terminal is sometimes referred to as the "coating layer".

[0041] (Examples of the components that make up a capacitor element)

[0042] The following describes examples of the constituent components of a capacitor element (solid electrolytic capacitor element). For constituent components other than the characteristic parts of this invention, known constituent components can be used. It should be noted that there is no particular limitation on the capacitor element as long as the effects of this invention can be obtained, and other capacitor elements besides those described below (e.g., known capacitor elements) can also be used.

[0043] (Anode section)

[0044] The anode portion includes an anode body. The anode body may contain a valve-acting metal, an alloy containing a valve-acting metal, or a compound containing a valve-acting metal. These materials may be used alone or in combination of two or more. For example, aluminum, tantalum, niobium, and titanium are preferred as valve-acting metals. An anode body with porous surfaces can be obtained, for example, by roughening the surface of a metal foil containing a valve-acting metal. Roughening can be performed by electrolytic etching or the like. The anode body may be entirely porous. However, from a strength point of view, the anode body preferably includes porous portions disposed on two main surfaces and a core disposed between these porous portions. The porosity of the core is lower than that of the porous portions. The porous portions are regions having many fine pores. The core is, for example, a region that has not been electrolytically etched.

[0045] (Dielectric layer)

[0046] A capacitor element includes a dielectric layer disposed between an anode and a cathode. The dielectric layer is an insulating layer that functions as a dielectric. The dielectric layer is formed by anodizing a valve-operated metal on the surface of an anode body (e.g., a metal foil). The dielectric layer is formed to cover at least a portion of the anode body (anode portion). The dielectric layer is typically formed on the surface of the anode body. The dielectric layer is formed on the surface of the porous portion of the anode body, thus forming along the inner walls of pores and recesses (also called pits) on the surface of the anode body.

[0047] A typical dielectric layer contains an oxide of the valve-acting metal. For example, a typical dielectric layer when tantalum is used as the valve-acting metal contains Ta₂O₅, and a typical dielectric layer when aluminum is used as the valve-acting metal contains Al₂O₃. It should be noted that the dielectric layer is not limited to these, as long as it functions as a dielectric.

[0048] (Cathode section)

[0049] The cathode portion includes a solid electrolyte layer covering at least a portion of the dielectric layer, and may further include a cathode lead-out layer covering at least a portion of the solid electrolyte layer. The solid electrolyte layer and the cathode lead-out layer will be described below.

[0050] (Solid electrolyte layer)

[0051] The solid electrolyte layer may, for example, be a layer comprising a conductive polymer. Depending on the need, in addition to the conductive polymer, the solid electrolyte layer may also contain at least one selected from dopants and other additives. Examples of dopants include, but are not limited to, p-toluenesulfonic acid, naphthalenesulfonic acid, and polystyrenesulfonic acid (PSS).

[0052] As conductive polymers, π-conjugated polymers can be used, for example. Examples of conductive polymers include those with a basic backbone of polypyrrole, polythiophene, polyaniline, polyfuran, polyacetylene, polyphenylene, polyphenylene vinylidene, polyphenylene oxide, and polythiophene vinylidene. These polymers also include homopolymers, copolymers of two or more monomers, and their derivatives (substitutes with substituents, etc.). For example, polythiophene includes poly(3,4-ethylidene dioxythiophene). However, these are merely examples, and conductive polymers are not limited to these examples.

[0053] (Cathode lead-out layer)

[0054] The cathode lead-out layer can use a conductive layer. For example, the cathode lead-out layer can use a layer containing conductive particles or a metal foil layer. Examples of conductive particles include conductive carbon and metal particles. The cathode lead-out layer can comprise a first layer and a second layer stacked sequentially from the side of the solid electrolyte layer. In one example, a layer containing conductive carbon can be used as the first layer, and a layer containing metal particles or a metal foil can be used as the second layer. Examples of conductive carbon include graphite (artificial graphite, natural graphite, etc.). Examples of metal particles include silver particles. The layer containing conductive particles can be formed using a composition containing conductive particles and a resin (adhesive resin), or it can be formed using a metal paste (e.g., silver paste).

[0055] (Solid electrolytic capacitor)

[0056] The solid electrolytic capacitor of this embodiment includes at least one capacitor element. The number of capacitor elements included in the solid electrolytic capacitor can be in the range of 1 to 20 (e.g., 2 to 10).

[0057] In electrolytic capacitors comprising multiple capacitor elements, these elements can be stacked. Typically, the ends of the anodes of the stacked capacitor elements are electrically connected to each other. For example, the ends of these anodes can be joined by welding. Anode lead terminals can be connected to the ends of these anodes.

[0058] Typically, the cathode lead layers of stacked capacitor elements are electrically connected to each other. Cathode lead terminals may be bonded to the cathode lead layer of at least one capacitor element. The cathode lead terminals may be bonded to the cathode lead layer via a conductive adhesive or solder. Alternatively, the cathode lead terminals may be bonded to the cathode lead layer by welding (resistance welding, laser welding, etc.). The conductive adhesive is, for example, a mixture of curable resin and carbon particles or metal particles.

[0059] As described above, a solid electrolytic capacitor includes an outer casing covering the capacitor elements. The outer casing also covers a portion of the anode lead terminals (embedded portion) and a portion of the cathode lead terminals (embedded portion). The outer casing preferably comprises a cured form of a curable resin composition, but may also contain a thermoplastic resin or a composition containing the same. The curable resin composition may comprise a curable resin and fillers. A thermosetting resin is preferred as the curable resin.

[0060] In addition to the curable resin, curable resin compositions may also contain fillers, curing agents, polymerization initiators, and catalysts. Examples of curable resins include epoxy resins, phenolic resins, urea resins, polyimides, polyamide-imides, polyurethanes, diallyl phthalate, and unsaturated polyesters. Curable resin compositions can contain a variety of curable resins.

[0061] Examples of fillers include insulating particles (inorganic particles, organic particles), insulating fibers, etc. Examples of insulating materials constituting fillers include insulating compounds (oxides, etc.) such as silica and alumina, glass, and mineral materials (talc, mica, clay, etc.). The outer casing may contain only one type of filler or two or more types. The filler content in the outer casing can range from 10% to 90% by mass.

[0062] Examples of thermoplastic resins include polyphenylene sulfide (PPS) and polybutylene terephthalate (PBT). In addition to the thermoplastic resin, compositions containing thermoplastic resins may also contain the aforementioned fillers.

[0063] The solid electrolytic capacitor of this embodiment may further include a housing disposed on the outside of the outer casing (resin composition). Examples of resin materials constituting the housing include thermoplastic resins or compositions containing them. Examples of metal materials constituting the housing include metals such as aluminum, copper, and iron, or their alloys (including stainless steel and brass).

[0064] (Lead terminal)

[0065] As described above, both the anode and cathode leads include an embedded portion and an exposed portion. Except for the roughened surface (R), the anode and cathode leads can be formed using known materials and methods. As described above, both the anode and cathode leads can be formed by processing a metal sheet (including metal plate and metal foil) made of metal (copper, copper alloy, etc.). That is, examples of materials for the substrate of the anode and cathode leads include copper, copper alloys, etc.

[0066] One end of the anode lead terminal (the end of the embedded portion) is connected to the anode portion. One end of the cathode lead terminal (the end of the embedded portion) is connected to the cathode portion (e.g., the cathode lead-out layer). The exposed portions of the anode lead terminal and the exposed portions of the cathode lead terminal can each function as terminal portions for brazing or other applications when mounting a solid electrolytic capacitor.

[0067] (Solid electrolytic capacitor elements and manufacturing methods of solid electrolytic capacitors)

[0068] The manufacturing method of the solid electrolytic capacitor in this embodiment is not particularly limited. Among these manufacturing methods, known manufacturing methods can be used, except for the method of forming a rough surface (R), or a portion of a known manufacturing method can be modified for application.

[0069] The following describes an example of a method for manufacturing a solid electrolytic capacitor according to this embodiment. However, the solid electrolytic capacitor of this embodiment can also be manufactured using methods other than those described below. The matters described for the solid electrolytic capacitor can also be applied to the manufacturing method described below, therefore, some repeated descriptions may be omitted. Furthermore, the matters described for the manufacturing method described below can also be applied to the solid electrolytic capacitor of this embodiment.

[0070] First, capacitor elements, anode leads, and cathode leads are fabricated (step (i)). The method for fabricating the capacitor elements is not particularly limited and can be formed using known methods. In the case of manufacturing a solid electrolytic capacitor comprising multiple stacked capacitor elements, the multiple capacitor elements are stacked. In this case, the anode portions of the multiple capacitor elements are connected to each other by welding or the like, if necessary. Additionally, the cathode portions of the multiple capacitor elements are connected to each other by a conductive paste or the like, if necessary.

[0071] Next, the anode lead terminal is electrically connected to the anode portion of the capacitor element, and the cathode lead terminal is electrically connected to the cathode portion of the capacitor element (step (ii)). The connection method is not particularly limited, and known connection methods can be used. For example, the anode portion and the anode lead terminal can be connected by soldering or the like. The cathode portion and the cathode lead terminal can be connected by a conductive paste or the like.

[0072] Next, the capacitor element, the embedded portion of the anode lead terminal, and the embedded portion of the cathode lead terminal are covered with an outer casing (step (iii)). The outer casing can be formed using molding techniques such as injection molding, insert molding, and compression molding.

[0073] The manufacturing method includes a step (I) of fabricating lead terminals (anode lead terminals and / or cathode lead terminals) having a rough surface (R). Step (I) includes a step (a) of processing a metal sheet (substrate) into a specified shape by stamping or the like, and a step (b) of forming the rough surface (R). Step (I) may also include a step (c) of forming a coating layer (plating layer, etc.) on the substrate. Either step (a) or step (b) may be performed first.

[0074] When step (I) includes step (c), the order of steps (a), (b), and (c) is not particularly limited as long as a rough surface (R) is ultimately formed in the specified area. However, if a coating is formed on the surface having the rough surface (R) after it has been formed, the unfolded area ratio of the interface of the rough surface (R) may decrease. In this case, step (b) can be performed after step (c). Alternatively, step (c) can be performed after the rough surface (R) has been formed in step (b), and only in areas that may not be rough surfaces (R) can the coating be formed. Step (c) can be performed before step (iii) of covering the embedded portion of the capacitor element and the lead terminals with the outer casing. Alternatively, step (c) can be performed after step (iii), and the coating can be formed only on the exposed portion of the lead terminals.

[0075] The process (a) of processing a metal sheet (substrate) into a specified shape by means of stamping or the like can be carried out by known methods.

[0076] The process (b) for forming a rough surface (R) can be performed, for example, by sandblasting, roughening plating, or roughening etching. Sandblasting is preferred due to its rapid processing speed and cost-effectiveness. Roughening plating is preferred due to its low cost. Roughening etching is preferred due to its low non-uniformity and ability to create a fine roughness. Furthermore, unlike sandblasting, roughening plating and roughening etching have the advantage of not leaving any residue (blasted material).

[0077] Conventional methods involve roughening the surface of lead terminals using techniques such as sandblasting. However, under conventional conditions, the fit between the outer casing and the lead terminals is insufficient. In the method of this invention, roughening is performed when the unfolded area ratio of the roughened surface interface is 0.4 or higher.

[0078] By reducing the particle size (e.g., increasing the grade number) of the particles (blasting material), it is possible to increase the developed area ratio of the interface of the surface subjected to blasting treatment. Therefore, in this method, blasting is generally performed using particles smaller than the particles conventionally used for roughening lead terminals. In addition, by increasing the blasting shot count, it is also possible to increase the developed area ratio of the interface of the surface subjected to blasting treatment to a certain extent. Although there are cases where the developed area ratio of the interface decreases when the particle size of the particles (blasting material) is excessively small, the condition for the developed area ratio of the interface of the rough surface to be 0.4 or more can be easily determined through experiments. The particles (blasting material) used for blasting are not particularly limited, and alumina particles and garnet particles can be used.

[0079] In the case where the rough surface (R) is formed by a roughening plating method, the developed area ratio Sdr of the interface can be made 0.4 or more by, for example, forming acicular or particulate plating to increase the surface area. For example, the proportion of acicular or particulate plating can be increased.

[0080] In the case where the rough surface (R) is formed by a roughening etching method, a roughened shape is formed by utilizing the difference between the etching rate of grain boundaries and the etching rate of crystal grains (the etching rate of grain boundaries is higher), for example, so that the surface area can be increased, and as a result, the developed area ratio Sdr of the interface can be made 0.4 or more. For example, the ratio of grain boundaries to crystal grains in the metal can be changed by selecting the metal that serves as the material of the lead terminal, or the difference in etching rate can be varied by changing the etching conditions.

[0081] As described above, the rough surface (R) having a developed area ratio of the interface of 0.4 or more is formed on the lead terminal. The coating layer (the layer on the base material) formed in step (c) can be formed by a known method (e.g., a known plating method). In this manner, the solid electrolytic capacitor can be manufactured.

[0082] Examples of the embodiments of the present invention will be specifically described below with reference to the accompanying drawings. The above-described constituent elements can be applied to the constituent elements of the examples described below. In addition, the examples described below can be modified based on the above description. Further, the matters described below can also be applied to the above embodiments. Furthermore, in the embodiments described below, non-essential constituent elements of the solid electrolytic capacitor of the present invention may be omitted. The solid electrolytic capacitor described below can be manufactured by the above method.

[0083] (Embodiment 1)

[0084] Figure 1 is a schematic cross-sectional view showing the solid electrolytic capacitor according to Embodiment 1. Figure 1The solid electrolytic capacitor 10 shown includes a capacitor element 100, lead terminals 20, and an outer casing 30. The lead terminals 20 include an anode lead terminal 21 electrically connected to the anode portion (anode body) 111 of the capacitor element 100, and a cathode lead terminal 22 electrically connected to the cathode portion 113 of the capacitor element 100.

[0085] The capacitor element 100 includes an anode portion (anode body) 111, a dielectric layer 112 covering at least a portion of the anode portion 111, and a cathode portion 113 covering at least a portion of the dielectric layer 112. The cathode portion 113 includes a solid electrolyte layer 113a covering at least a portion of the dielectric layer 112, and a cathode lead-out layer 113b covering at least a portion of the solid electrolyte layer 113a.

[0086] The anode lead terminal 21 includes an embedded portion 21a embedded in the outer casing 30 and an exposed portion 21b protruding from the outer casing 30. The cathode lead terminal 22 includes an embedded portion 22a embedded in the outer casing 30 and an exposed portion 22b protruding from the outer casing 30. Figure 1 The boundary 21x between the embedded part 21a and the exposed part 21b, and the boundary 22x between the embedded part 22a and the exposed part 22b are shown.

[0087] One end of the anode portion 111 is electrically connected to the embedded portion 21a of the anode lead terminal 21 by welding or the like. The cathode portion 113 (specifically the cathode lead-out layer 113b) of the capacitor element 100 is electrically connected to the embedded portion 22a of the cathode lead terminal 22 by a conductive paste 23.

[0088] The embedded portion 21a has a contact surface p that contacts the outer casing 30. The embedded portion 22a has a contact surface n that contacts the outer casing 30. The contact surface p and / or the contact surface n have the aforementioned rough surface (R). In the rough surface (R) portion, the sealing between the outer casing 30 and the lead terminal 20 is improved. Therefore, it is possible to suppress the intrusion of oxygen and the like from the interface between the outer casing 30 and the lead terminal 20. As a result, it is possible to suppress the deterioration of the capacitor element 100 and improve the long-term reliability of the solid electrolytic capacitor 10.

[0089] The anode lead terminal 21 and / or the cathode lead terminal 22 may include the aforementioned coating. The coating is preferably formed in such a way as to cover the curved portions 21d and 22d of the exposed portions 21b and 22b that are curved along the outer surface of the outer casing 30.

[0090] An example of this embodiment of the electrolytic capacitor may include a plurality of stacked capacitor elements 100. In this case, one end of the anode portion 111 of the plurality of capacitor elements 100 is joined by welding or the like, and at least one anode portion 111 is connected to an anode lead terminal 21. The cathode portions 113 of the plurality of capacitor elements 100 are connected by a conductive paste or the like, and at least one cathode portion 113 is connected to a cathode lead terminal 22 by a conductive paste or the like. That is, the plurality of capacitor elements 100 are connected in parallel. In this case, the contact surface p and / or the contact surface n also have a rough surface (R).

[0091] Example

[0092] The solid electrolytic capacitor of the present invention will be further described in detail through embodiments.

[0093] [Fabrication and Evaluation of Solid Electrolytic Capacitors]

[0094] Various solid electrolytic capacitors are fabricated using the methods described below. Each solid electrolytic capacitor contains one capacitor element. The solid electrolytic capacitor and the capacitor element each have the following characteristics: Figure 1 The solid electrolytic capacitor 10 shown has a similar structure to the capacitor element 100.

[0095] First, the two surfaces of an aluminum foil (thickness: 100 μm) are roughened by etching to create the anode body (anode portion). Next, anodizing is performed while a portion of the anode body is immersed in a chemical conversion solution, thereby forming a dielectric layer (alumina layer) on the anode body.

[0096] Next, a solid electrolyte layer is formed on the dielectric layer using the following method. First, an aqueous solution containing pyrrole monomer and p-toluenesulfonic acid is prepared. The anode and counter electrode, on which the dielectric layer is formed, are immersed in the obtained aqueous solution for electrolytic polymerization. Through this electrolytic polymerization, a solid electrolyte layer is formed.

[0097] Next, graphite particles and a dispersion material (such as a cellulose derivative) are wet-milled with water using a bead mill to obtain a dispersion. This dispersion is then coated onto the surface of a solid electrolyte layer and dried. This forms a carbon layer on the surface of the solid electrolyte layer. Next, a silver paste containing silver particles and a binder resin (epoxy resin) is coated onto the surface of the carbon layer, and the mixture is heated to form a metal paste layer. Through these processes, a cathode lead-out layer comprising the carbon layer and the metal paste layer is formed. Thus, a capacitor element is manufactured.

[0098] A copper sheet (thickness: 100 μm) for forming the anode and cathode leads is prepared. Next, the portions forming the anode and cathode leads are roughened to create rough surfaces. Subsequently, the metal sheet is processed to form the shapes of the anode and cathode leads.

[0099] Roughening is achieved through sandblasting, roughening plating, and roughening etching. In sandblasting, the average particle size of the blasted beads (alumina particles, garnet particles, etc.) is varied to change the unfolded area ratio Sdr of the interface. In roughening plating and roughening etching, the unfolded area ratio Sdr of the interface is increased using the methods described above. To evaluate the roughness of the formed rough surface, the arithmetic mean height Sa and the unfolded area ratio Sdr of the interface are measured for the formed rough surface. It should be noted that in the unroughened capacitor C1, the surface roughness of the lead terminals is determined by measuring the arithmetic mean height Sa and the unfolded area ratio Sdr of the interface.

[0100] The unfolded area ratio Sdr of the interface was measured according to ISO 25178. Similarly, the arithmetic mean height Sa was measured according to ISO 25178.

[0101] Next, one end of the anode portion of the capacitor element is connected to the anode lead terminal. Additionally, the cathode portion of the capacitor element is connected to the cathode lead terminal using a conductive paste. Then, the capacitor element, a portion of the anode lead terminal (embedded portion), and a portion of the cathode lead terminal (embedded portion) are covered by molding. In this way, a capacitor with [missing information - likely referring to a specific structure or feature] is manufactured. Figure 1 An electrolytic capacitor with a structure similar to the electrolytic capacitor shown.

[0102] In this embodiment, 100 of each of seven types of solid electrolytic capacitors (capacitors C1, C2, A1 to A5) were fabricated by changing the method for forming the roughened surface (roughening method). The roughening methods used are shown in Table 1. In the sandblasting of capacitors C2 and A1 to A3, the average particle size of the sprayed beads (sprayed material) used was changed as shown in Table 1 below, thereby changing the ratio of the unfolded area of ​​the interface. Specifically, the ratio of the average particle size to the average particle size was changed based on the average particle size of the sprayed beads used in the sandblasting of capacitor C2, as shown in Table 1. For example, the average particle size of the sprayed beads used in the sandblasting of capacitor A1 was half the average particle size of the sprayed beads used in the sandblasting of capacitor C2. It should be noted that the sandblasting conditions for capacitor C2 were the conventional sandblasting conditions.

[0103] The manufactured capacitors were heat-treated under the same conditions as the solder reflow process (peak temperature of 260°C for 10 seconds). Then, the hermeticity defect rate was evaluated for the heat-treated capacitors.

[0104] The airtightness failure rate was evaluated using a total leakage test. Specifically, a capacitor was placed inside a small capsule, and the minute pressure drop caused by leakage of internal pressure from the small capsule to the capacitor's outer casing was measured. Capacitors with large pressure changes were then identified as having airtightness failures. A portion of the capacitor manufacturing conditions and the evaluation results are shown in Table 1.

[0105] [Table 1]

[0106]

[0107] As shown in Table 1, by making the unfolded area ratio Sdr of the interface greater than 0.4, the airtightness failure rate after heat treatment can be significantly reduced. Compared with capacitor C1, capacitor C2, which underwent sandblasting, showed a significant increase in the arithmetic mean height Sa of its surface, indicating that roughening occurred through sandblasting. However, the airtightness failure rate of capacitor C2 after heat treatment remained high. Although the arithmetic mean height Sa of the roughened surfaces of capacitors A1 to A5 was lower than that of capacitor C2, the airtightness failure rates of capacitors A1 to A5 were significantly lower than those of capacitor C2. This indicates that the previously used evaluation methods could not provide a proper evaluation.

[0108] An image showing an example of the unevenness of a portion representing the rough surface of capacitor C2 is provided. Figure 2 An image showing an example of the unevenness of a portion of the rough surface of capacitor A2 is provided. Figure 3 .like Figure 2 As shown, on the rough surface of capacitor C2, the areas of one concave portion and one convex portion are large, and the concave and convex portions are not uniform. On the other hand, in the rough surface of capacitor A2, the fine concave and convex portions are uniformly distributed.

[0109] Industrial availability

[0110] This invention can be used for solid electrolytic capacitor elements and solid electrolytic capacitors.

[0111] Explanation of reference numerals in the attached figures

[0112] 10: Solid electrolytic capacitors

[0113] 20: Lead terminal

[0114] 21: Anode lead terminal

[0115] 21a, 22a: embedded part

[0116] 21b, 22b: Exposed areas

[0117] 22: Cathode lead terminal

[0118] 22a: Buried part

[0119] 22b: Exposed area

[0120] 30: Exterior body

[0121] 100: Capacitor element

[0122] 111: Anode section

[0123] 112: Dielectric layer

[0124] 113: Cathode section

[0125] 113a: Solid electrolyte layer

[0126] 113b: Cathode lead-out layer

[0127] p, n: contact surfaces.

Claims

1. A solid electrolytic capacitor, comprising: At least one capacitor element comprising an anode and a cathode The anode lead terminal electrically connected to the anode section, The cathode lead terminal electrically connected to the cathode section, and The outer casing covering the at least one capacitor element, Each of the anode lead terminal and the cathode lead terminal includes an embedded portion embedded in the outer casing and an exposed portion connected to the embedded portion and protruding from the outer casing. At least one of the substrates selected from the substrates of the anode lead terminal and the substrates of the cathode lead terminal is a copper substrate. At least a portion of the copper substrate in the exposed portion is covered with a copper plating layer. The copper plating is covered by a tin plating. An alloy layer of copper and tin is disposed between the copper plating layer and the tin plating layer. The embedded portion of the anode lead terminal has a first contact surface that contacts the outer casing. The embedded portion of the cathode lead terminal has a second contact surface that contacts the outer casing. At least one of the first contact surface and the second contact surface has a rough surface with an unfolded area ratio of 0.4 or more.

2. The solid electrolytic capacitor according to claim 1, wherein, The rough surface formed extends across the embedded portion and the exposed portion, and is thus also formed on at least a portion of the exposed portion.

3. The solid electrolytic capacitor according to claim 1 or 2, wherein, The first contact surface and the second contact surface each have the rough surface.

4. The solid electrolytic capacitor according to claim 1 or 2, wherein, The unfolded area ratio of the rough surface interface is less than 10.

0.

5. The solid electrolytic capacitor according to claim 1, wherein, The copper substrate has a curved portion at the exposed portion that bends along the outer surface of the outer casing. The outer surface of the curved portion is covered by the copper plating layer.

6. The solid electrolytic capacitor according to claim 1 or 5, further comprising a noble metal plating covering the copper plating. The precious metal coating comprises at least one selected from gold, platinum, and palladium.

7. The solid electrolytic capacitor of claim 6, further comprising a nickel plating layer disposed between the copper plating layer and the noble metal plating layer.

Citation Information

Patent Citations

  • Solid electrolytic capacitor

    JP1992253314A

  • Solid-state electrolytic capacitor

    JP2000049056A

  • Lead frame material, manufacturing method of the same, and semiconductor package

    JP2019207905A