A wear-resistant charging pile cable and its preparation method
By employing a protective sheath structure consisting of a high-temperature resistant layer, a waterproof layer, and a wear-resistant insulating sheath in the charging pile cable, and by covering the conductor cable core with specific materials, the problem of external surface damage caused by torsion and bending during the use of the charging pile cable is solved, thereby improving the cable's wear resistance and signal transmission stability and extending its service life.
Patent Information
- Application Number
- CN202310775620.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-06-28
- Publication Date
- 2026-11-10
- Estimated Expiration
- 2043-06-28
AI Technical Summary
During use, charging pile cables are prone to damage to their outer surface due to twisting, bending, and dragging on the ground, which affects the stability of signal transmission and service life.
The cable adopts a protective sheath structure that includes a high-temperature resistant layer, a waterproof layer, and a wear-resistant insulating sheath. It uses materials such as thermoplastic polyurethane elastomer, modified basalt fiber, and surface-modified crab shell powder to encapsulate the conductor core through an extruder, forming a wear-resistant charging pile cable.
It improves the cable's abrasion resistance and mechanical properties, prevents damage to the outer surface, ensures signal transmission stability, and extends service life.
Abstract
Description
Technical Field
[0001] This application relates to the technical field of cable processing, and in particular to a wear-resistant charging pile cable and its preparation method. Background Technology
[0002] With the rapid development of new energy sources, new energy vehicles have been widely promoted due to their advantages such as low energy consumption, low noise, low carbon emissions, and high safety, and have broad market prospects. Correspondingly, charging piles for new energy vehicles have also begun to be built. With the construction of charging piles and other infrastructure, there is an urgent need for charging pile cable products that can be used in conjunction with new energy vehicles.
[0003] Charging piles connect to charging heads via cables to charge vehicles. Currently, there are various types of charging pile cables on the market, with different performance levels. High-quality charging pile cables need to have advantages such as good safety, strong adaptability, durability, and energy efficiency.
[0004] During use, car charging pile cables are frequently twisted, bent, or dragged on the ground, which can easily damage the outer surface of the cable, causing unstable signal transmission and shortening the cable's lifespan. Summary of the Invention
[0005] To address the issue of easily damaged outer surfaces of electric vehicle charging pile cables, which shortens their service life, this application provides a wear-resistant charging pile cable and its preparation method.
[0006] This application provides a wear-resistant charging pile cable, which adopts the following technical solution: It includes a conductor cable core and a protective sleeve, wherein the protective sleeve covers the conductor cable core, and the protective sleeve includes a high-temperature resistant layer, a waterproof layer and a wear-resistant insulating sheath arranged in sequence, wherein the high-temperature resistant layer covers the conductor cable core; The wear-resistant insulating sheath comprises the following raw materials in parts by weight: Thermoplastic polyurethane elastomer 35-55 parts, maleic anhydride grafted ethylene-vinyl acetate copolymer 25-30 parts, epoxidized natural rubber 15-25 parts, hydrogenated castor oil 11-20 parts, dioctyl phthalate 15-25 parts, surface-modified crab shell powder 22-38 parts, modified basalt fiber 8-15 parts, titanate coupling agent 2-5 parts, antioxidant 2-4 parts, lubricant 1-3 parts.
[0007] By adopting the above technical solution, the protective sleeve is used to protect the conductor cable core. The high-temperature resistant layer covers the conductor cable core, and the high-temperature resistant layer has excellent flame resistance and fire retardant properties, protecting the conductor cable core from high temperatures so that it can continue to operate. The waterproof layer increases the durability of the protective sleeve and prevents moisture from penetrating the protective sleeve and entering the conductor cable core, thereby affecting the service life of the conductor cable core. The wear-resistant insulating sleeve can not only effectively prevent electric shock accidents caused by human contact with the previously exposed wiring terminals due to various reasons, but also effectively avoid damage to the outer surface of the cable during use, thereby preventing unstable signal transmission and shortening the service life of the cable.
[0008] Thermoplastic polyurethane elastomers possess excellent comprehensive properties such as high strength, high toughness, wear resistance, and oil resistance, and have good processing performance. Epoxidized natural rubber exhibits excellent air tightness, oil resistance, adhesion, anti-slip properties, and low rolling resistance. Maleic anhydride-grafted ethylene-vinyl acetate copolymer has excellent viscosity, which helps to increase the adhesion between the components in the system, making the prepared wear-resistant insulating sheath more robust. Hydrogenated castor oil helps to adjust the consistency of the system, dioctyl phthalate is used to adjust the plasticity of the system, and titanate coupling agents play a reinforcing role in the components of the system, improving the overall wear resistance, anti-aging ability, and gloss of the system. Antioxidants delay the decomposition of the wear-resistant insulating sheath due to oxidation, extending the life of plastic products. Lubricants improve the fluidity of the system, prevent the polymer from sticking to the barrel, inhibit frictional heat generation, reduce mixing torque and load, and thus prevent the thermal degradation of the polymer material. At the same time, during extrusion molding, it can improve the fluidity of the system, improve the adhesion of the polymer material to the barrel and die, and facilitate the extrusion molding of the polymer.
[0009] Surface-modified crab shell powder has a loose and porous structure with a rough surface and a large specific surface area. It exhibits good adsorption and wear resistance, and can be loaded onto modified basalt fibers to increase their mechanical properties and wear resistance. Simultaneously, it ensures uniform mixing of all components in the system, resulting in good density and increased mechanical strength and wear resistance. Modified basalt fiber is a reinforcing material with excellent mechanical properties, stability, insulation, durability, wear resistance, and corrosion resistance. The combination of modified basalt fiber and surface-modified crab shell powder enhances the wear resistance and mechanical properties of the modified basalt fiber. When mixed with other components in the system, it further strengthens the mechanical properties and wear resistance of the system. In subsequent applications, it provides wear-resistant insulating sheaths for cables, exhibiting good wear resistance, tear resistance, and mechanical strength.
[0010] Preferably, the preparation method of the surface-modified crab shell powder includes the following steps: (1) Wash the crab shell powder with deionized water, then soak it in anhydrous ethanol for 1-3 hours, dry it, ball mill it, pass it through an 80-mesh sieve, and then add 0.01-0.03 g / mL of KOH solution and activate it at 100-120℃ for 2-3 hours. (2) Wash the crab shell powder treated in step (1) with deionized water, then disperse it in anhydrous ethanol, add graphene oxide, sonicate at 35-45℃ for 20-35 min, filter, and dry. (3) Disperse chitosan in malic acid, add the crab shell powder treated in step (2), stir at 65-75℃ for 3-5 hours, then filter and dry to obtain surface-modified crab shell powder.
[0011] By adopting the above technical solution, the crab shell powder is first cleaned with anhydrous ethanol to remove organic stains and sterilize it. Then, it is ball-milled to refine the crab shell powder. Next, it is mixed with KOH solution for deproteinization. The crab shell powder itself has a dense matrix structure composed of chitin and protein. After removing the protein, the crab shell powder exhibits a porous cross-linked network structure. Then, it is activated at a temperature of 100-120℃ to further remove organic impurities from the crab shell powder and expand the pore size in the porous structure, which is conducive to the loading of subsequent components.
[0012] Graphene oxide is mainly composed of a graphene substrate with carbon-carbon double bonds and aromatic rings combined with oxygen atom groups. It has good compatibility, surface activity, wear resistance, and mechanical properties. Graphene oxide can be loaded on the surface of crab shell powder and partially loaded into the porous structure of crab shell powder, thereby improving the wear resistance and mechanical properties of crab shell powder. Chitosan has good biocompatibility, degradability, and antibacterial properties. Chitosan dispersed in malic acid has good adhesion and film-forming properties. It can coat graphene oxide and crab shell powder, forming a film on the surface of crab shell powder, further increasing the adhesion between graphene oxide and crab shell powder. This allows graphene oxide to be loaded on the surface and in the porous structure of crab shell powder, further increasing the mechanical properties and wear resistance of crab shell powder.
[0013] Preferably, the mass ratio of crab shell powder, graphene oxide and chitosan in step (1) is 1g:0.02-0.06mg:0.3-0.6g.
[0014] By adopting the above technical solution, the mass ratio of crab shell powder, graphene and chitosan in step (1) is further limited to obtain surface-modified crab shell powder with better mechanical properties and wear resistance. Graphene oxide can be loaded on the surface of crab shell powder, and chitosan can coat crab shell powder, which further increases the adhesion between crab shell powder and graphene oxide, thereby improving the mechanical properties and wear resistance of crab shell powder, which helps to improve the mechanical properties and wear resistance of subsequent wear-resistant insulating sheaths.
[0015] A preferred method for preparing modified basalt fibers includes the following steps: (1) Soak basalt fiber in citric acid for 1-2 hours, wash with water until neutral, and dry; (2) Disperse the basalt fibers treated in step (1) in anhydrous ethanol, then add ceramic micro powder, sonicate for 1-3 hours, wash with water, and dry. (3) Disperse glass fiber in silane coupling agent and stir for 1-3 hours. Then add basalt fiber treated in step (2) and stir for 3-5 hours. Wash with water and dry to obtain modified basalt fiber.
[0016] By adopting the above technical solution, basalt fibers are soaked in citric acid. Citric acid has a certain abrasive effect on the surface of basalt fibers, making the surface of basalt fibers rough and creating a microporous structure, which increases the specific surface area of the basalt fiber surface and helps the loading of subsequent components. The ceramic micro powder itself has a porous structure and has good adsorption, corrosion resistance, high temperature resistance and wear resistance. The ceramic micro powder loaded on the surface of basalt fibers and in the microporous structure increases the specific surface area of basalt fibers and improves the structural strength, mechanical properties and wear resistance of basalt fibers.
[0017] Glass fiber possesses high tensile strength, is non-flammable, has good insulation, excellent chemical resistance, and strong heat resistance. Mixing glass fiber with a silane coupling agent further enhances its tensile strength. Adding treated basalt fiber creates a cross-linked network structure between the basalt and glass fibers. The silane coupling agent, acting as a bridge, further increases the cross-linking structure between the glass and basalt fibers, thereby improving the mechanical and abrasion resistance of the basalt fiber. In subsequent applications in abrasion-resistant insulating sheaths, this further improves the mechanical properties and abrasion resistance of the sheath.
[0018] Preferably, the mass ratio of basalt fiber, ceramic micro powder and glass fiber in step (1) is 1:0.1-0.3:0.5-0.8.
[0019] By adopting the above technical solution, the mass ratio of basalt fiber, ceramic micro powder and glass fiber in step (1) is further limited to obtain modified basalt fiber with better mechanical properties and wear resistance. Ceramic micro powder is loaded on the surface of basalt fiber, and glass fiber is cross-linked with basalt fiber and loaded on the surface of basalt fiber, which further improves the mechanical properties and wear resistance of basalt fiber.
[0020] Preferably, the particle size of the ceramic micro powder is 1-3 μm.
[0021] By adopting the above technical solution, the particle size of ceramic micro powder is further limited, and the obtained ceramic micro powder has better comprehensive performance, with good adsorption, weather resistance, durability, wear resistance, corrosion resistance and high temperature resistance. When applied to wear-resistant insulating sheaths, it not only helps to disperse the components in the system evenly, but also helps to improve the mechanical properties and wear resistance of the system.
[0022] Preferably, the high-temperature resistant layer is made of polytetrafluoroethylene, polyester, kaolin and graphite.
[0023] By adopting the above technical solutions, the high-temperature resistant layer has superior high-temperature resistance, which helps protect the conductor core and prevents it from becoming unusable due to high temperatures. Polytetrafluoroethylene has good high-temperature resistance and corrosion resistance, polyester has strong mechanical strength, flexibility and tear resistance, kaolin can improve the tensile strength, elongation at break and insulation performance of the system, and graphite has good strength, toughness, heat resistance and antibacterial properties. The combination of various raw materials together improves the high-temperature resistance and long-term performance of the high-temperature resistant layer.
[0024] Preferably, the waterproof layer is made of polyethylene, antioxidant 1010, and pentaerythritol triallyl ether.
[0025] By adopting the above technical solution, the waterproof layer has excellent waterproof performance, preventing the conductor core from coming into contact with water and thus affecting the service life of the conductor core. Polyethylene has good toughness, waterproofness and wear resistance. Antioxidant 1010 increases the antioxidant performance of the system, and pentaerythritol triallyl ether increases the plasticity of the system. The various raw materials in the system work together to improve the waterproof performance of the waterproof layer.
[0026] Preferably, the antioxidant is bisphenol A; the lubricant is lubricant G60.
[0027] By adopting the above technical solutions, antioxidants can delay the decomposition of wear-resistant insulating sheaths due to oxidation and extend the life of plastic products; lubricants improve the fluidity of the system, improve the adhesion of the polymer material to the barrel and mold, and help the polymer extrusion molding of the system.
[0028] Secondly, this application also provides a method for preparing a wear-resistant charging pile cable, comprising the following steps: extruding a high-temperature resistant layer on the outside of the conductor core using an extruder, covering the outside of the high-temperature resistant layer with a waterproof layer, and covering the outside of the waterproof layer with a wear-resistant insulating sheath to obtain a wear-resistant charging pile cable.
[0029] By adopting the above technical solution and the above steps to prepare wear-resistant charging pile cables, the raw materials are mixed evenly, which makes them easy to process and simple to operate. This improves the strength and wear resistance of the wear-resistant charging pile cables and is conducive to subsequent industrial production.
[0030] In summary, this application has the following beneficial effects: 1. In this application, the protective sleeve is used to protect the conductor cable core. The high-temperature resistant layer covers the conductor cable core and has excellent flame retardant and fireproof properties, protecting the conductor cable core from high temperatures so that it can continue to operate. The waterproof layer increases the durability of the protective sleeve and prevents moisture from penetrating the protective sleeve into the conductor cable core, thereby affecting the service life of the conductor cable core. The wear-resistant insulating sleeve can not only effectively prevent electric shock accidents caused by human contact with the originally exposed wiring terminals due to various reasons, but also effectively avoid damage to the outer surface of the cable during use, thereby preventing unstable signal transmission and shortening the service life of the cable.
[0031] 2. The thermoplastic polyurethane elastomer in this application has excellent comprehensive properties such as high strength, high toughness, wear resistance, and oil resistance, and good processing performance. The epoxidized natural rubber has excellent air tightness, oil resistance, adhesion, anti-slip properties, and low rolling resistance. The maleic anhydride-grafted ethylene-vinyl acetate copolymer has excellent adhesion, which is beneficial to increasing the adhesion between the components in the system, making the prepared wear-resistant insulating sheath more robust.
[0032] 3. The surface-modified crab shell powder in this application has a loose and porous structure, a rough surface, and a large specific surface area. It has good adsorption and wear resistance, and can be loaded onto modified basalt fibers to increase the mechanical properties and wear resistance of the modified basalt fibers. At the same time, it can make the components in the system mix evenly, with good density, increasing the mechanical strength and wear resistance of the system. The modified basalt fibers combined with the surface-modified crab shell powder increase the wear resistance and mechanical properties of the modified basalt fibers. When mixed with other components in the system, it further enhances the mechanical properties and wear resistance of the system. When subsequently applied to the wear-resistant insulating sheath of cables, it has good wear resistance, tear resistance, and mechanical strength. Detailed Implementation
[0033] The present application will be further described in detail below with reference to the embodiments.
[0034] The raw materials used in the examples and comparative examples are all commercially available; the antioxidant is bisphenol A; and the lubricant is lubricant G60.
[0035] Preparation example of surface-modified crab shell powder Preparation Example 1-1 The preparation method of surface-modified crab shell powder includes the following steps: (1) Wash 1.2 kg of crab shell powder with deionized water, then soak it in 2 L of anhydrous ethanol for 3 h, dry it, ball mill it, pass it through an 80 mesh sieve, and then add 0.02 g / mL of KOH solution and activate it at 110 °C for 3 h. (2) Wash the crab shell powder treated in step (1) with deionized water, then disperse it in 2.1L of anhydrous ethanol, add graphene oxide, sonicate at 40℃ for 30min, filter, and dry. (3) Chitosan was dispersed in 2.5L of malic acid, and the crab shell powder treated in step (2) was added. The mixture was stirred at 70℃ for 5 hours, then filtered and dried to obtain surface-modified crab shell powder. The mass ratio of crab shell powder, graphene oxide and chitosan in step (1) was 1g:0.02mg:0.6g.
[0036] Preparation Examples 1-2 The difference from preparation example 1-1 is that graphene oxide is not added in step (2).
[0037] Preparation Examples 1-3 The difference from preparation example 1-1 is that chitosan is not added in step (1).
[0038] Preparation Examples 1-4 The difference from Preparation Example 1-1 is that the mass ratio of crab shell powder, graphene oxide and chitosan in step (1) is 1g:0.06mg:0.3g.
[0039] Preparation Examples 1-5 The difference from Preparation Example 1-1 is that the mass ratio of crab shell powder, graphene oxide and chitosan in step (1) is 1g:0.09mg:0.1g.
[0040] Preparation Examples 1-6 The difference from preparation example 1-1 is that step (1) is not performed.
[0041] Preparation example of modified basalt fiber Preparation Example 2-1 The preparation method of modified basalt fiber includes the following steps: (1) Soak 1.2 kg of basalt fiber in 2 L of 1.5 mol / L citric acid for 2 h, wash with water until neutral, and dry; (2) Disperse the basalt fibers treated in step (1) in 2.5L of anhydrous ethanol, then add ceramic micro powder, sonicate for 3 hours, wash with water and dry; (3) Disperse glass fiber in 1.5L silane coupling agent, stir for 3h, then add basalt fiber treated in step (2), stir for 5h, wash with water, dry, and obtain modified basalt fiber; wherein, the mass ratio of basalt fiber, ceramic micro powder and glass fiber in step (1) is 1:0.1:0.8.
[0042] Preparation Example 2-2 The difference from preparation example 2-1 is that ceramic powder is not added in step (2).
[0043] Preparation Examples 2-3 The difference from preparation example 2-1 is that glass fiber is not added in step (3).
[0044] Preparation Examples 2-4 The difference from preparation example 2-1 is that the mass ratio of basalt fiber, ceramic micro powder and glass fiber in step (1) is 1:0.3:0.5.
[0045] Preparation Examples 2-5 The difference from preparation example 2-1 is that the mass ratio of basalt fiber, ceramic micro powder and glass fiber in step (1) is 1:0.05:0.95.
[0046] Preparation Examples 2-6 The difference from preparation example 2-1 is that step (1) is not performed. Example
[0047] Example 1 A wear-resistant charging pile cable includes a conductor core and a protective sheath. The protective sheath covers the conductor core and includes a high-temperature resistant layer, a waterproof layer, and a wear-resistant insulating sheath arranged sequentially. The high-temperature resistant layer covers the conductor core. The high-temperature resistant layer is made of 30 kg of polytetrafluoroethylene, 20 kg of polyester, 5 kg of kaolin, and 2 kg of graphite. The waterproof layer is made of 40 kg of polyethylene, 2 kg of antioxidant 1010, and 1 kg of pentaerythritol triallyl ether.
[0048] The wear-resistant insulating sheath comprises the following raw materials by weight: 40 kg of thermoplastic polyurethane elastomer, 28 kg of maleic anhydride-grafted ethylene-vinyl acetate copolymer, 20 kg of epoxidized natural rubber, 16 kg of hydrogenated castor oil, 20 kg of dioctyl phthalate, 30 kg of surface-modified crab shell powder, 12 kg of modified basalt fiber, 4 kg of titanate coupling agent, 3 kg of antioxidant, and 2 kg of lubricant.
[0049] The above-mentioned method for preparing wear-resistant charging pile cables includes the following steps: extruding a high-temperature resistant layer on the outside of the conductor core using an extruder, covering the outside of the high-temperature resistant layer with a waterproof layer, and covering the outside of the waterproof layer with a wear-resistant insulating sheath to obtain the wear-resistant charging pile cable.
[0050] The surface-modified crab shell powder was prepared using Preparation Example 1-1; the modified basalt fiber was prepared using Preparation Example 2-1.
[0051] Example 2 A wear-resistant charging pile cable differs from Example 1 in that the surface-modified crab shell powder is prepared using Preparation Examples 1-2.
[0052] Example 3 A wear-resistant charging pile cable differs from Example 1 in that the surface-modified crab shell powder is prepared using Preparation Examples 1-3.
[0053] Example 4 A wear-resistant charging pile cable differs from Example 1 in that the surface-modified crab shell powder is prepared using Preparation Examples 1-4.
[0054] Example 5 A wear-resistant charging pile cable differs from Example 1 in that the surface-modified crab shell powder is prepared using Preparation Examples 1-5.
[0055] Example 6 A wear-resistant charging pile cable differs from Example 1 in that the surface-modified crab shell powder is prepared using Preparation Examples 1-6.
[0056] Example 7 A wear-resistant charging pile cable differs from Example 1 in that the modified basalt fiber is prepared using Preparation Example 2-2.
[0057] Example 8 A wear-resistant charging pile cable, which differs from Example 1 in that the modified basalt fiber is prepared using Preparation Examples 2-3.
[0058] Example 9 A wear-resistant charging pile cable differs from Example 1 in that the modified basalt fiber is prepared using Preparation Examples 2-4.
[0059] Example 10 A wear-resistant charging pile cable, which differs from Example 1 in that the modified basalt fiber is prepared using Preparation Examples 2-5.
[0060] Example 11 A wear-resistant charging pile cable differs from Example 1 in that the modified basalt fiber is prepared using Preparation Examples 2-6.
[0061] Example 12 A wear-resistant charging pile cable, differing from Embodiment 1 in that the wear-resistant insulating sheath comprises the following raw materials by weight: 35 kg of thermoplastic polyurethane elastomer, 25 kg of maleic anhydride-grafted ethylene-vinyl acetate copolymer, 15 kg of epoxidized natural rubber, 11 kg of hydrogenated castor oil, 15 kg of dioctyl phthalate, 38 kg of surface-modified crab shell powder, 8 kg of modified basalt fiber, 2 kg of titanate coupling agent, 4 kg of antioxidant, and 3 kg of lubricant.
[0062] Example 13 A wear-resistant charging pile cable, differing from Embodiment 1 in that the wear-resistant insulating sheath comprises the following raw materials by weight: 55 kg of thermoplastic polyurethane elastomer, 30 kg of maleic anhydride-grafted ethylene-vinyl acetate copolymer, 25 kg of epoxidized natural rubber, 20 kg of hydrogenated castor oil, 25 kg of dioctyl phthalate, 22 kg of surface-modified crab shell powder, 15 kg of modified basalt fiber, 5 kg of titanate coupling agent, 2 kg of antioxidant, and 1 kg of lubricant.
[0063] Comparative Example Comparative Example 1 A wear-resistant charging pile cable, differing from Embodiment 1 in that the wear-resistant insulating sheath comprises the following raw materials by weight: 30 kg of thermoplastic polyurethane elastomer, 20 kg of maleic anhydride-grafted ethylene-vinyl acetate copolymer, 35 kg of epoxidized natural rubber, 8 kg of hydrogenated castor oil, 10 kg of dioctyl phthalate, 15 kg of surface-modified crab shell powder, 5 kg of modified basalt fiber, 1 kg of titanate coupling agent, 1 kg of antioxidant, and 0.5 kg of lubricant.
[0064] Comparative Example 2 A wear-resistant charging pile cable, differing from Embodiment 1 in that the wear-resistant insulating sheath comprises the following raw materials in parts by weight: 60 kg of thermoplastic polyurethane elastomer, 35 kg of maleic anhydride-grafted ethylene-vinyl acetate copolymer, 10 kg of epoxidized natural rubber, 30 kg of hydrogenated castor oil, 35 kg of dioctyl phthalate, 45 kg of surface-modified crab shell powder, 20 kg of modified basalt fiber, 8 kg of titanate coupling agent, 6 kg of antioxidant, and 5 kg of lubricant.
[0065] Comparative Example 3 A wear-resistant charging pile cable differs from Example 1 in that it does not contain surface-modified crab shell powder.
[0066] Comparative Example 4 A wear-resistant charging pile cable differs from Example 1 in that it does not contain modified basalt fiber.
[0067] Comparative Example 5 A wear-resistant charging pile cable differs from Example 1 in that it uses an equal amount of basalt fiber instead of modified basalt fiber.
[0068] Performance testing The wear-resistant charging pile cables prepared in Examples 1-13 and Comparative Examples 1-5 were subjected to mechanical property tests and wear resistance tests. The tensile strength and elongation at break were measured according to GB / T2951.12, and the tear strength was measured according to GB / T529. The results are shown in Table 1.
[0069] Table 1 Test data for the examples and comparative examples Testing items Tensile strength / MPa Elongation at break / % Tear strength N / mm Abrasion resistance (with an additional 0.2kg weight) Example 1 35 550 165 Belt travel 2532mm Example 2 22 520 130 Belt travel 2030mm Example 3 28 535 145 Belt travel 2256mm Example 4 34 549 165 Belt travel 2532mm Example 5 30 540 152 Belt travel 2356mm Example 6 32 542 158 Belt travel 2412mm Example 7 25 526 138 Belt travel 2120mm Example 8 20 515 125 Belt travel 2010mm Example 9 33 550 164 Belt travel 2532mm Example 10 27 534 142 Belt travel 2210mm Example 11 31 540 156 Belt travel 2400mm Example 12 34 550 164 Belt travel 2532mm Example 13 35 549 163 Belt travel 2532mm Comparative Example 1 15 500 120 Belt travel 1752mm Comparative Example 2 16 495 119 Belt travel 1742mm Comparative Example 3 11 463 101 Belt travel 1602mm Comparative Example 4 9 450 92 Belt travel 1432mm Comparative Example 5 18 499 121 Belt travel 1830mm As can be seen from Table 1, the wear-resistant charging pile cables prepared in Examples 1, 4, 9 and 12-13 of this application have good mechanical properties and wear resistance. The tensile strength reaches 35MPa, the elongation at break reaches 550%, and the tear strength reaches 165N / mm. In the wear resistance test, with an additional weight of 0.2kg and a sand belt walking 2532mm, it is shown that the wear-resistant charging pile cables prepared in this application have superior mechanical properties and wear resistance. When applied to wear-resistant insulating sheaths, they can improve the mechanical properties, wear resistance and service life of the wear-resistant insulating sheaths.
[0070] In Example 2, no graphene oxide was added during the preparation of surface-modified crab shell powder. As shown in Table 1, compared with Example 1, the mechanical properties and wear resistance were significantly reduced. The tensile strength was 22 MPa, the elongation at break was 520%, and the tear strength was 130 N / mm. Wear resistance testing was conducted with an additional 0.2 kg weight and a sanding belt travel of 2030 mm, indicating that graphene oxide improved the wear resistance and mechanical properties of the crab shell powder. In Example 3, no chitosan was added during the preparation of surface-modified crab shell powder. As shown in Table 1, the mechanical properties and wear resistance were significantly reduced, indicating that chitosan has good adhesion and film-forming properties, capable of coating graphene oxide and crab shell powder, further increasing the adhesion between graphene oxide and crab shell powder, and increasing the mechanical properties and wear resistance of the crab shell powder.
[0071] Example 5 changed the mass ratio of crab shell powder, graphene oxide and chitosan in step (1). As shown in Table 1, compared with Example 1, the mechanical properties and wear resistance decreased significantly. However, the data test results were significantly better than the corresponding data of Examples 2-3, but worse than the corresponding data of Examples 1 and 4. This indicates that there is a synergistic effect between crab shell powder, graphene and chitosan, which together improves the mechanical properties and wear resistance of the wear-resistant insulating sheath.
[0072] In Example 6, step (1) was omitted in the preparation of surface-modified crab shell powder. As shown in Table 1, compared with Example 1, the mechanical properties and wear resistance were significantly reduced. This indicates that the crab shell powder was mixed with KOH solution for deproteinization treatment. After removing the protein, the crab shell powder exhibited a porous cross-linked network structure. Then, it was activated at a certain temperature to further remove organic impurities in the crab shell powder and expand the pore size in the porous structure of the crab shell powder. This helps the loading of subsequent components and thus improves the corresponding performance of the subsequent cable.
[0073] In Example 7, no ceramic powder was added during the preparation of modified basalt fiber. As shown in Table 1, compared with Example 1, the mechanical properties and wear resistance were significantly reduced. The tensile strength was 25 MPa, the elongation at break was 526%, and the tear strength was 138 N / mm. The wear resistance test was conducted with an additional 0.2 kg weight and a sanding belt traveled 2120 mm. This indicates that the ceramic powder was loaded on the surface and within the microporous structure of the basalt fiber, increasing the specific surface area of the basalt fiber and improving its structural strength, mechanical properties, and wear resistance.
[0074] In Example 8, no glass fiber was added during the preparation of modified basalt fiber. As shown in Table 1, the mechanical properties and abrasion resistance decreased significantly. The tensile strength was 20 MPa, the elongation at break was 515%, and the tear strength was 125 N / mm. Abrasion resistance tests were conducted with an additional 0.2 kg weight and a sanding belt traveled for 2010 mm. This indicates that the basalt fiber and glass fiber form a cross-linked network structure, thereby improving the mechanical properties and abrasion resistance of the basalt fiber. In subsequent applications in abrasion-resistant insulating sheaths, this will further improve the mechanical properties and abrasion resistance of the abrasion-resistant insulating sheaths.
[0075] Example 10 changed the mass ratio of basalt fiber, ceramic powder and glass fiber in step (1). As can be seen from Table 1, compared with Example 1, the mechanical properties and wear resistance decreased significantly. However, the data test was significantly better than the corresponding data of Examples 7-8, but worse than the corresponding data of Examples 1 and 9. This indicates that there is a synergistic effect between basalt fiber, ceramic powder and glass fiber, which together improves the mechanical properties and wear resistance of the wear-resistant insulating sheath.
[0076] In Example 11, step (1) was not performed in the preparation of modified basalt fiber. As can be seen from Table 1, compared with Example 1, the mechanical properties and wear resistance decreased significantly, indicating that citric acid has a certain erosion effect on the surface of basalt fiber, making the surface of basalt fiber rough and microporous structure appear on the surface, which helps the subsequent components to be loaded.
[0077] Comparative Examples 1-2 showed changes in the amount of raw materials used in the wear-resistant insulating sheath. As shown in Table 1, compared to Example 1, the tensile strength, elongation at break, and tear strength all decreased significantly. Abrasion resistance tests were conducted with an additional 0.2 kg weight and a sand belt running for 1752 mm. This indicates that the proportions of each raw material component in a certain ratio give the charging pile cable better mechanical and abrasion resistance properties. Changes in the amount of each raw material affect the corresponding performance of the charging pile cable.
[0078] Comparative Example 3, without the addition of surface-modified crab shell powder, shows, as per Table 1, a significant decrease in mechanical and heat resistance compared to Example 1. The tensile strength was 11 MPa, the elongation at break was 463%, and the tear strength was 101 N / mm. Abrasion resistance testing was conducted with an additional 0.2 kg weight and a sanding belt travel of 1602 mm. This indicates that the surface-modified crab shell powder has a loose, porous structure and a rough surface, exhibiting good adsorption and abrasion resistance. It can be loaded onto modified basalt fibers, increasing their mechanical properties and abrasion resistance.
[0079] Comparative Example 4, without the addition of modified basalt fiber, shows, as per Table 1, a significant decrease in mechanical and heat resistance compared to Example 1. The tensile strength is 9 MPa, the elongation at break is 450%, and the tear strength is 90 N / mm. Abrasion resistance testing was conducted with a 0.2 kg weight added and a sand belt traveled 1432 mm. This indicates that the modified basalt fiber possesses excellent mechanical properties, stability, insulation, durability, abrasion resistance, and corrosion resistance. In subsequent applications as abrasion-resistant insulating sheaths for cables, it exhibits good abrasion resistance, tear resistance, and mechanical strength.
[0080] Comparative Example 5 uses an equal amount of basalt fiber instead of modified basalt fiber. As shown in Table 1, compared with Example 1 and Comparative Example 4, the mechanical properties and heat resistance are significantly worse than those of Example 1, but better than those of Comparative Example 4. This indicates that the modified basalt fiber prepared in this application has better mechanical properties and wear resistance, which can further improve the corresponding performance of the charging pile cable.
[0081] This specific embodiment is merely an explanation of this application and is not intended to limit it. After reading this specification, those skilled in the art can make modifications to this embodiment without contributing any inventive step, but such modifications are protected by patent law as long as they fall within the scope of the claims of this application.
Claims
1. A wear-resistant charging pile cable, characterized in that, It includes a conductor cable core and a protective sleeve, wherein the protective sleeve covers the conductor cable core, and the protective sleeve includes a high-temperature resistant layer, a waterproof layer and a wear-resistant insulating sheath arranged in sequence, wherein the high-temperature resistant layer covers the conductor cable core; The wear-resistant insulating sheath comprises the following raw materials in parts by weight: Thermoplastic polyurethane elastomer 35-55 parts, maleic anhydride grafted ethylene-vinyl acetate copolymer 25-30 parts, epoxidized natural rubber 15-25 parts, hydrogenated castor oil 11-20 parts, dioctyl phthalate 15-25 parts, surface modified crab shell powder 22-38 parts, modified basalt fiber 8-15 parts, titanate coupling agent 2-5 parts, antioxidant 2-4 parts, lubricant 1-3 parts; The preparation method of the surface-modified crab shell powder includes the following steps: (1) Wash the crab shell powder with deionized water, then soak it in anhydrous ethanol for 1-3 hours, dry it, ball mill it, pass it through an 80-mesh sieve, and then add 0.01-0.03 g / mL of KOH solution and activate it at 100-120℃ for 2-3 hours. (2) Wash the crab shell powder treated in step (1) with deionized water, then disperse it in anhydrous ethanol, add graphene oxide, sonicate at 35-45℃ for 20-35 min, filter, and dry. (3) Disperse chitosan in malic acid, add crab shell powder treated in step (2), stir at 65-75℃ for 3-5 hours, then filter and dry to obtain surface-modified crab shell powder. The method for preparing the modified basalt fiber includes the following steps: (1) Soak basalt fibers in citric acid for 1-2 hours, wash with water until neutral, and dry; (2) Disperse the basalt fibers treated in step (1) in anhydrous ethanol, then add ceramic micro powder, sonicate for 1-3 hours, wash with water, and dry; (3) Disperse glass fiber in silane coupling agent and stir for 1-3 hours. Then add basalt fiber treated in step (2) and stir for 3-5 hours. Wash with water and dry to obtain modified basalt fiber.
2. The wear-resistant charging pile cable according to claim 1, characterized in that, The mass ratio of crab shell powder, graphene oxide, and chitosan is 1g:0.02-0.06mg:0.3-0.6g.
3. The wear-resistant charging pile cable according to claim 1, characterized in that, The mass ratio of basalt fiber, ceramic micro powder and glass fiber is 1:0.1-0.3:0.5-0.
8.
4. The wear-resistant charging pile cable according to claim 1, characterized in that, The ceramic micro powder has a particle size of 1-3 μm.
5. The wear-resistant charging pile cable according to claim 1, characterized in that, The high-temperature resistant layer is made of polytetrafluoroethylene, polyester, kaolin and graphite.
6. The wear-resistant charging pile cable according to claim 1, characterized in that, The waterproof layer is made of polyethylene, antioxidant 1010, and pentaerythritol triallyl ether.
7. The wear-resistant charging pile cable according to claim 1, characterized in that, The antioxidant is bisphenol A; the lubricant is lubricant G60.
8. A method for preparing a wear-resistant charging pile cable according to any one of claims 1-7, characterized in that, The process includes the following steps: extruding a high-temperature resistant layer onto the outside of the conductor core using an extruder, covering the outside of the high-temperature resistant layer with a waterproof layer, and covering the outside of the waterproof layer with a wear-resistant insulating sheath to obtain a wear-resistant charging pile cable.
Citation Information
Patent Citations
Heat-resistant reinforced polypropylene cable material and manufacturing method thereof
CN106633377A
Tensile and wear-resistant carbon fiber cable
CN108630344A