Friction stir additive manufacturing method and friction stir additive manufacturing device for metal components with variable path width
By using metal rods of different diameters combined with friction stir additive manufacturing, the overlap problem caused by inconsistent path widths in additive manufacturing is solved, and efficient and defect-free metal component manufacturing is achieved, and production efficiency and printing quality are improved.
Patent Information
- Application Number
- CN202310434068.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-04-21
- Publication Date
- 2024-11-01
- Estimated Expiration
- 2043-04-21
AI Technical Summary
The existing metal additive manufacturing technology has overlapping problems for metal components of different path widths during the printing process, resulting in low manufacturing efficiency and cumbersome replacement of the print head.
Using metal rods of different diameters combined with friction stir additive manufacturing technology, the path width variability is achieved by adjusting the diameter of metal rods on the stirring head, and metal components with different path widths are directly obtained to avoid overlaps, improve printing quality and efficiency.
The full-position defect-free connection of additive objects is achieved, the quality and manufacturing efficiency of parts are improved, the operation is simplified, and the need for manual replacement of raw materials and mixing heads is reduced.
Smart Images

Figure CN116652361B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of friction stir additive manufacturing, and in particular to a friction stir additive manufacturing method and a friction stir additive manufacturing device for a metal component with a variable path width. Background Art
[0002] Additive manufacturing technology, commonly known as 3D printing technology, is a digital manufacturing technology that achieves precise moldless forming of components by adding and stacking materials layer by layer. Contrary to the traditional subtractive processing concept, additive manufacturing technology uses a high-energy source to melt the material point by point, stack it layer by layer, and directly form it. Since its emergence, additive manufacturing technology has attracted widespread attention due to its advantages such as short processing cycle, high production efficiency, and high flexible production. The main preparation methods include 3D printing, magnetron sputtering, and directional solidification.
[0003] Commonly used metal additive manufacturing methods include arc, electron beam and laser additive manufacturing. These three technologies have their own advantages and scope of use, and can all achieve good additive manufacturing of materials. However, for some parts with special sizes, such as metal sheets with different widths of reinforcing ribs on the surface used in the construction field, or cylindrical connectors with different wall thicknesses, there are defects caused by overlaps in the printing process for different path widths, which affects manufacturing efficiency; the overlap problem can be solved by replacing the print head with the corresponding width, but the operation is cumbersome and still affects manufacturing efficiency. Summary of the invention
[0004] The purpose of the present invention is to provide a stir friction additive manufacturing method and a stir friction additive manufacturing device for metal components with variable path widths, by using metal bars of different diameters as raw materials and combining the stir friction additive manufacturing process, metal components with different path widths can be directly obtained, thereby improving printing quality and efficiency.
[0005] According to a first aspect of the present invention, there is provided a friction stir additive manufacturing method for a metal component with a variable path width, comprising:
[0006] Using a plurality of metal rods with different diameters as raw materials, a stir friction additive manufacturing process is adopted, and deposition is performed layer by layer on a substrate in an upward growth manner starting from the first layer according to a preset program until the deposition of the last layer is completed, thereby obtaining the desired metal component; the metal component is a metal plate with a reinforcing rib structure of different widths or a cylindrical part with different wall thicknesses;
[0007] The stirring needle is inserted into the substrate or the previous deposition layer, and the end face of the stirring head is in contact with the surface of the substrate or the previous deposition layer for preheating. Then, the stirring head is retracted to keep a certain distance between the end face of the stirring head and the surface of the substrate or the previous deposition layer. The metal rod enters and extends out of the stirring head until it contacts the surface of the substrate or the previous deposition layer, and is driven by the stirring head to perform synchronous rotation and plasticization to deposit a new deposition layer, so that the width of the deposition layer is equal to the diameter of the metal rod.
[0008] When the width of the deposition layer needs to be changed, a metal rod with a diameter equal to the required deposition layer width is directly selected as the raw material to obtain the required path width; during the printing process, different metal rods are switched for stir friction additive manufacturing for reinforcing rib structures of different widths or different wall thicknesses of cylindrical parts.
[0009] In an optional embodiment, the metal component is a metal plate with reinforcing rib structures of different widths, and the preparation process includes the following:
[0010] Using metal bars as raw materials and the stir friction additive manufacturing process, a reinforcing rib structure is formed on the surface of the metal plate in a single pass in a horizontal and vertical orthogonal cross-section according to a preset program, and there is a spacing between adjacent single passes in the same direction;
[0011] Among them, two metal bars with different diameters are used as raw materials to print transverse reinforcement ribs and longitudinal reinforcement ribs respectively, so that the widths of the transverse reinforcement ribs and the longitudinal reinforcement ribs are not equal, and metal plates with reinforcement rib structures of different widths are obtained.
[0012] In an optional embodiment, the spacing range between adjacent single passes can be set according to the strength and rigidity requirements of the metal sheet.
[0013] In an optional embodiment, the metal component is a cylindrical part with different wall thicknesses, and the preparation process includes the following:
[0014] Using a metal rod with a first diameter as a raw material, a stir friction additive manufacturing process is used to deposit layer by layer starting from a first layer on the surface of the substrate in an upward growth manner according to a preset program to obtain a cylindrical part with a first wall thickness, wherein the first wall thickness is equal to the first diameter;
[0015] Using a metal rod having a second diameter as a raw material, a stir friction additive manufacturing process is used to continue to deposit layer by layer in an upward growth manner on the cylindrical part having a first wall thickness according to a preset program to obtain a cylindrical part having a second wall thickness, wherein the second wall thickness is equal to the second diameter;
[0016] And so on, until the required cylindrical parts with different wall thicknesses are obtained.
[0017] In an optional embodiment, the metal type is an aluminum alloy, a magnesium alloy, a copper alloy or a titanium alloy.
[0018] In an optional embodiment, the friction stir additive manufacturing process is configured to determine the feed speed of the metal bar and the process parameters of the friction stir treatment according to the printing structure parameters, and set the printing program accordingly to print and form the part.
[0019] In an optional embodiment, the friction stir additive manufacturing method further includes annealing the printed parts.
[0020] According to a second aspect of the present invention, there is provided a variable diameter continuous feeding friction stir additive manufacturing device, comprising:
[0021] The material feeding system comprises a raw material container, wherein the raw material container is provided with a plurality of through holes for placing metal bars of different diameters;
[0022] The upper end of the raw material container is provided with a pushing mechanism for pushing the metal rod, and the lower end of the raw material container is sleeved with a feeding mechanism, and the feeding mechanism is provided with a first channel for only one metal rod to pass through;
[0023] The raw material container is also provided with a transmission mechanism, and the raw material container is pushed and pulled by the transmission mechanism so that the position of the metal rod placed in the through hole corresponds to the position of the first channel on the feeding mechanism, and the pushing mechanism pushes the metal rod of the required diameter, and the metal rod is transported to the friction stir additive manufacturing system through the first channel;
[0024] A friction stir additive manufacturing system disposed below the feeding system comprises a stirring head, wherein the stirring head comprises a connecting portion, a shaft shoulder portion and a stirring needle connected in sequence;
[0025] A second channel is provided in the connecting part, and the metal bar passing through the first channel is transported to the second channel through a traction mechanism. A gathering mechanism is provided in the second channel, and the diameter of the second channel and the metal bar are matched by the gathering mechanism, and the metal bar is further transported to the shaft shoulder.
[0026] A third channel is provided in the shoulder portion, the third channel is connected with the second channel, the metal rod enters the third channel from the second channel, and is transported to the surface of the area to be added along the third channel;
[0027] The stirring needle is arranged on the end surface of the shaft shoulder away from the connecting part to promote the flow of surrounding materials;
[0028] The friction stir additive manufacturing system is connected to a control drive system, and the control drive system is configured to perform friction stir additive manufacturing on the metal rod output from the shaft shoulder;
[0029] Among them, when printing metal plates with reinforcing rib structures of different widths or cylindrical parts with different wall thicknesses, the metal rods placed in different through holes are pushed by the pushing mechanism for reinforcing rib structures of different widths or different wall thickness parts of the cylindrical parts, and different metal rods are switched for stir friction additive manufacturing.
[0030] In an optional embodiment, the gathering mechanism includes multiple sets of clamping devices, which include an inner ring, an outer ring and multiple pre-tensioning mechanisms arranged between the inner ring and the outer ring, and the pre-tensioning mechanisms keep the inner ring and the outer ring tending to move away from each other.
[0031] In an optional embodiment, the preload mechanism is a spring with preload force.
[0032] In an optional embodiment, the top of the inner ring is funnel-shaped with a larger top and a smaller bottom, so as to facilitate the entry of bars of different diameters.
[0033] In an optional embodiment, the traction mechanism is a set of adjustable roller wheels, which pull the metal bar to move downward at a constant speed into the second channel.
[0034] It can be seen from the above technical solution of the present invention that the friction stir additive manufacturing method for metal components with variable path width proposed in the present invention adopts metal bars of different diameters as raw materials and combines the friction stir additive manufacturing process to directly obtain metal components with different path widths, thereby avoiding the cold overlap generated in the overlap additive manufacturing process, achieving defect-free connection of additive objects in all positions, and improving the quality of parts and manufacturing efficiency.
[0035] The variable diameter continuous feeding friction stir additive manufacturing device proposed in the present invention adopts a continuous feeding method to feed materials, thereby realizing continuous additive manufacturing without stopping the machine. It can work continuously for a long time and does not require manual replacement of additive raw materials and stirring heads during the working process, which greatly improves production efficiency and ease of operation. BRIEF DESCRIPTION OF THE DRAWINGS
[0036] Figure 1 It is a schematic diagram of the manufacturing process of the friction stir additive manufacturing method of the metal component with variable path width of the present invention.
[0037] Figure 2 It is a structural schematic diagram of a raw material container of a variable diameter continuous feeding and stirring friction additive manufacturing device of the present invention.
[0038] Figure 3 It is a structural schematic diagram of a stirring head of a variable diameter continuous feeding friction stir additive manufacturing device of the present invention.
[0039] Figure 4 It is a structural schematic diagram of the gathering mechanism of the variable diameter continuous feeding stir friction additive manufacturing device of the present invention.
[0040] Figure 5 It is a structural schematic diagram of the clamping device of the variable diameter continuous feeding friction stir additive manufacturing device of the present invention.
[0041] Figure 6 It is a schematic structural diagram of a metal plate with reinforcing ribs of different widths according to an example of the present invention.
[0042] Figure 7 It is a schematic structural diagram of a cylindrical part with different wall thicknesses according to an example of the present invention. DETAILED DESCRIPTION
[0043] In order to better understand the technical content of the present invention, specific embodiments are given and described as follows in conjunction with the accompanying drawings.
[0044] Various aspects of the present invention are described in this disclosure with reference to the accompanying drawings, in which many illustrative embodiments are shown. The embodiments of the present disclosure are not necessarily intended to include all aspects of the present invention. It should be understood that the various concepts and embodiments introduced above, as well as those described in more detail below, can be implemented in any of many ways.
[0045] Friction stir additive manufacturing is a solid-phase non-melting additive manufacturing method derived from friction stir welding technology. Due to its large plastic deformation and self-heating behavior, it brings strong dynamic recovery and recrystallization and second-phase crushing and redistribution characteristics. It can achieve high-strength and high-toughness design of additive parts with ultrafine grain and dense structure and uniform dispersion of the second phase. It is particularly suitable for the manufacture of aluminum and aluminum alloys, magnesium and magnesium alloys, lightweight metal composites, etc.
[0046] Based on this, the present invention provides a friction stir additive manufacturing method and a friction stir additive manufacturing device for metal components with variable path widths. By using metal bars of different diameters as raw materials and combining them with the friction stir additive manufacturing process, metal components with different path widths can be directly obtained, thereby improving printing quality and efficiency.
[0047] Combination Figures 1 to 5 The variable diameter continuous feeding friction stir additive manufacturing device of the exemplary embodiment shown includes:
[0048] The feeding system 100 is provided with a raw material container 110, such as Figure 2 As shown, the raw material container 110 is provided with a plurality of through holes 111 for placing metal bars 300 of different diameters.
[0049] It should be understood that the diameter of each through hole is different, for example, 4.2mm, 6.2mm, 8.2mm, 10.2mm, respectively for placing metal bars with diameters of 4mm, 6mm, 8mm, 10mm; or the diameter of each through hole is equal, with the maximum diameter of the required metal bar as a reference, for example, if the maximum diameter of the required metal bar is 10mm, the diameter of the through holes is set to 10.2mm. It can be understood that the through holes are for placing metal bars, and it is only necessary to ensure that the metal bars can be pushed by the pushing mechanism and enter the friction stir additive manufacturing system.
[0050] In one of the embodiments, after a metal rod of a certain diameter is delivered to the friction stir additive manufacturing system, an automated system may be used to supply metal rods of the same diameter into corresponding through holes to ensure uninterrupted raw material supply.
[0051] The upper end of the raw material container 110 is provided with a pushing mechanism 120 for pushing the metal rod, and the lower end of the raw material container 110 is sleeved with a feeding mechanism 130, and the feeding mechanism 130 is provided with a first channel 131 for only one metal rod to pass through.
[0052] It can be understood that the diameter of the first channel 131 is set to ensure that the metal rod with the largest diameter can pass through.
[0053] A transmission mechanism 140 is also provided on the raw material container 110. The raw material container 110 pushes and pulls the transmission mechanism 140 so that the position of the metal rod placed in the through hole 111 corresponds to the position of the first channel 131 on the unloading mechanism. The pushing mechanism 120 pushes the metal rod of the required diameter, and the metal rod is transported to the friction stir additive manufacturing system through the first channel 131.
[0054] The friction stir additive manufacturing system 200 disposed below the feeding system 100 includes a stirring head, wherein the stirring head includes a connecting portion 210 , a shoulder portion 220 , and a stirring needle 230 that are sequentially connected.
[0055] like Figure 3 As shown, a second channel 211 is provided in the connecting portion 210, and the metal rod passing through the first channel 131 is transported to the second channel 211 through the traction mechanism 212. A gathering mechanism 2110 is provided in the second channel 211, and the second channel is matched with the diameter of the metal rod through the gathering mechanism 2110, and the metal rod is further transported to the shoulder portion 220.
[0056] A third channel 221 is provided in the shoulder portion 220 , and the third channel 221 is connected to the second channel 211 . The metal rod enters the third channel 221 from the second channel 211 and is transported to the surface of the area to be added along the third channel 221 .
[0057] The stirring pin 230 is disposed on the end surface of the shoulder portion 220 away from the connecting portion 210 to promote the flow of surrounding materials.
[0058] The friction stir additive manufacturing system 200 is connected to a control drive system, and the control drive system is configured to perform friction stir additive manufacturing on the metal rod output from the shaft shoulder.
[0059] When printing metal plates with rib structures of different widths or cylindrical parts with different wall thicknesses, the pushing mechanism 120 pushes metal rods placed in different through holes 111 for rib structures of different widths or different wall thicknesses of cylindrical parts, and switches different metal rods for stir friction additive manufacturing.
[0060] like Figure 4 , Figure 5 As shown, in an optional embodiment, the gathering mechanism 2110 includes at least one set of clamping devices 2111, and the clamping device 2111 includes an inner ring 2111A, an outer ring 2111B and a plurality of pre-tightening mechanisms 2111C, such as springs, which are arranged between the inner ring 2111A and the outer ring 2111B.
[0061] In the illustrated example, the gathering mechanism 2110 includes a plurality of clamping devices 2111 arranged in parallel along the conveying direction of the metal bar, and is used to make the second channel 211 fit the diameter of the metal bar so that the metal bar can be conveyed downward smoothly.
[0062] The inner ring 2111A is made of flexible material, so it has a certain elasticity, for example, it is made of rubber, and the top is set to be a funnel shape with a larger top and a smaller bottom, so that metal bars of different diameters can enter more easily; the outer ring 2111B is made of rigid material, so as to ensure the stability of the clamping device.
[0063] After the metal rod is squeezed into the inner ring 2111A, the inner ring generates an outward force to squeeze the spring, and the spring makes the second channel fit with the diameter of the metal rod through the reaction force.
[0064] In a more optional embodiment, the original diameter of the inner ring 2111A is smaller than the diameter of the metal rod with the smallest diameter, and the diameter of the metal rod with the smallest diameter is smaller than the maximum diameter of the inner ring 2111A after stretching, thereby ensuring that the second channel fits the diameter of the metal rod through the reaction force of the spring.
[0065] It should be understood that the gathering mechanism is detachably mounted, so that the size of the inner ring can be changed according to actual needs to adapt to different sizes of metal bars.
[0066] In another optional embodiment, the clamping device adopts an automated tightening system, and controls the electric actuator through a control system to extrude the inner ring, so as to achieve the purpose of making the second channel fit the diameter of the metal rod.
[0067] In an optional embodiment, the traction mechanism 212 is a set of adjustable roller wheels, which pull the metal bar to move downward at a constant speed into the second channel 211.
[0068] In an optional embodiment, the pushing mechanism 120 is a hydraulic push rod, which cooperates with the transmission mechanism on the raw material container to directly push the metal bar to contact the previous metal bar when pushing the metal bar, thereby completing the raw material supply.
[0069] In combination with the variable diameter continuous feeding friction stir additive manufacturing device of the aforementioned embodiment of the present invention, it is utilized to carry out an additive manufacturing process of a metal component with a variable path width.
[0070] Combination Figure 1 As shown, an exemplary friction stir additive manufacturing method for a metal component with a variable path width of the present invention comprises:
[0071] Using multiple metal rods with different diameters as raw materials and adopting the friction stir additive manufacturing process, they are deposited layer by layer on the substrate in an upward growth manner starting from the first layer according to a preset program until the deposition of the last layer is completed, thereby obtaining the required metal components; the metal components are metal plates with reinforcing rib structures of different widths or cylindrical parts with different wall thicknesses.
[0072] The stirring needle is inserted into the substrate or the previous deposition layer, and the end face of the stirring head is in contact with the surface of the substrate or the previous deposition layer for preheating. Then, the stirring head is retracted to keep a certain distance between the end face of the stirring head and the surface of the substrate or the previous deposition layer. The metal rod enters and extends out of the stirring head until it contacts the surface of the substrate or the previous deposition layer, and is driven by the stirring head to perform synchronous rotation and plasticization to deposit a new deposition layer, so that the width of the deposition layer is equal to the diameter of the metal rod.
[0073] When the width of the deposition layer needs to be changed, a metal rod with a diameter equal to the required deposition layer width is directly selected as the raw material to obtain the required path width; during the printing process, different metal rods are switched for stir friction additive manufacturing for reinforcing rib structures of different widths or different wall thicknesses of cylindrical parts.
[0074] In a typical example, the specific deposition process of a single-pass deposition layer and the raw material switching process are completed by using the above-mentioned device as follows:
[0075] Select a metal rod of corresponding diameter according to the required path width, and place the rod into the corresponding through hole of the raw material container.
[0076] Start the friction stir additive manufacturing system, the stirring head rotates at high speed, and the stirring needle penetrates into the substrate or the previous deposition layer until the end face of the stirring head contacts the upper surface of the additive manufacturing substrate. After the rotation preheating is maintained for a period of time, the stirring head is retracted so that the end face of the stirring head maintains a certain distance from the substrate or the surface of the previous deposition layer.
[0077] With the cooperation of the transmission mechanism, the pushing mechanism pushes the metal rod to the friction stir additive manufacturing system, and the metal rod is transported to the second channel through the traction of the traction mechanism. At this time, the gathering mechanism gathers the metal rod so that the metal rod is smoothly transported downward until it extends out of the stirring head and contacts the surface of the substrate or the surface of the previous deposition layer.
[0078] The stirring head starts to move according to the preset program. At the same time, the traction mechanism operates continuously to ensure that the metal rod is continuously transported downward. The metal rod rotates synchronously with the stirring head. The metal rod extending out of the stirring head is thermoplasticized and deposited on the substrate or the previous deposition layer to form a deposition layer with a width equal to the diameter of the metal rod, completing the deposition of a single deposition layer.
[0079] When it is necessary to switch to another diameter of metal rod, the transmission mechanism pushes and pulls the raw material container to align the metal rod of the required diameter with the first channel. At this time, the pushing mechanism pushes the metal rod of the required diameter to transport it to the friction stir additive manufacturing system.
[0080] In one of the optional embodiments, the above method is used to manufacture a metal plate with reinforcing rib structures of different widths, including the following preparation process:
[0081] According to the above process, metal rods are used as raw materials and the stir friction additive manufacturing process is adopted. According to the preset program, a single pass is printed on the surface of the metal plate in a horizontal and vertical orthogonal cross manner to form a reinforcing rib structure, and there is a spacing between adjacent single passes in the same direction.
[0082] Among them, two metal bars with different diameters are used as raw materials to print transverse reinforcement ribs and longitudinal reinforcement ribs respectively, so that the widths of the transverse reinforcement ribs and the longitudinal reinforcement ribs are not equal, and metal plates with reinforcement rib structures of different widths are obtained.
[0083] In an optional embodiment, the spacing range between adjacent single passes can be set according to the strength and rigidity requirements of the metal sheet.
[0084] In another optional embodiment, the above method is used to manufacture cylindrical parts with different wall thicknesses, including the following preparation process:
[0085] According to the above process, a metal rod having a first diameter is used as a raw material, and a stir friction additive manufacturing process is adopted to deposit layer by layer on the surface of the substrate starting from the first layer in an upward growth manner according to a preset program to obtain a cylindrical part having a first wall thickness, wherein the first wall thickness is equal to the first diameter.
[0086] According to the above process, a metal rod having a second diameter is used as a raw material, a stir friction additive manufacturing process is adopted, and layer-by-layer deposition is continued in an upward growth manner on the cylindrical part having a first wall thickness according to a preset procedure to obtain a cylindrical part having a second wall thickness, wherein the second wall thickness is equal to the second diameter.
[0087] And so on, until the required cylindrical parts with different wall thicknesses are obtained.
[0088] In an optional embodiment, the metal type is an aluminum alloy, a magnesium alloy, a copper alloy or a titanium alloy.
[0089] In an optional embodiment, the friction stir additive manufacturing process is configured to determine the feed speed of the metal bar and the process parameters of the friction stir treatment according to the printing structure parameters, and set the printing program accordingly to print and form the part.
[0090] In one of the preferred embodiments, the feeding speed of the traction mechanism is 1 to 5 times the travel speed of the stirring head; especially for low melting point materials such as aluminum / magnesium, the feeding speed of the traction mechanism is 3 to 5 times the travel speed of the stirring head; for higher melting point materials such as copper / titanium, the feeding speed of the traction mechanism is 2 to 3 times the travel speed of the stirring head.
[0091] In another preferred embodiment, the stirring head is withdrawn at a speed of 0.5-1 mm / min, and the withdrawal distance is 0.5-2.5 mm.
[0092] In another preferred embodiment, the rotation speed of the stirring head is 100-8000 rpm, the travel speed range is 10-1000 mm / min, the downward pressure of the friction stir additive manufacturing is 10-100 kN, and the downward pressure is 0.1-4 mm.
[0093] In an optional embodiment, the friction stir additive manufacturing method further includes annealing the printed part, and the annealing process is as follows:
[0094] Heat to 350~450℃ at a rate of 10-15℃ / s, keep warm for 2~4h, then cool with the furnace at a cooling temperature of less than 10℃ per hour, cool to 200℃, take out of the furnace, and cool in air to room temperature.
[0095] For better understanding, the present invention is further described below in conjunction with several specific examples, but the processing technology is not limited thereto, and the content of the present invention is not limited thereto.
[0096] Unless otherwise specified, the raw materials used in the present invention are all commercially available. Example 1
[0097] Print the rib structure on a 60×60mm 2060 aluminum plate. The horizontal ribs are 8mm wide, with a 20mm interval between adjacent ribs. There are 2 ribs in total. The vertical ribs are 4mm wide, with a 20mm interval between adjacent ribs. There are 2 ribs in total. The part structure is as follows: Figure 6 shown.
[0098] Step 1: Select 2060 aluminum-based bars with diameters of 4mm and 8mm, soak them in a dilute acid solution, rinse them with clean water to remove the surface oxide layer, use anhydrous ethanol to clean the surface oil stains, and then put them into the corresponding receiving through holes.
[0099] Step 2: Place the 2060 aluminum plate at the bottom.
[0100] Step 3: Start the stirring head, and the stirring needle penetrates into the substrate, so that the stirring head contacts the substrate. After rotating and preheating for 30 seconds, it is retracted. At the same time, the metal rod enters the stirring head and contacts the substrate, and stirring additive manufacturing begins until the component is completely formed. When printing a horizontal single channel, the rod diameter used is 8mm. After the horizontal printing is completed and the vertical single channel is turned, the rod diameter is changed to 4mm and the layer thickness is 0.4mm.
[0101] The parameters of the friction stir treatment are as follows: the stirring head speed is 1500 r / min, the travel speed is 100 mm / min, the stirring head penetrates 2 mm into the substrate, retracts 1.5 mm, the retraction speed is 1 mm / min, and the downward pressure of the stirring head is 200 N.
[0102] Step 4: Wait for the print to cool down and remove it.
[0103] Step 5: The obtained print is annealed by heating to 400°C at a rate of 15°C / s, keeping warm for 2h, and then cooling with the furnace at a cooling temperature of less than 10°C per hour. It is cooled to 200°C and taken out of the furnace, and placed in the air to cool to room temperature to eliminate residual stress. Example 2
[0104] 2195 aluminum-based material is used to manufacture cylindrical parts with different upper and lower wall thicknesses. The parts are two cylinders with the same inner diameter and different wall thicknesses connected together. The inner diameter of the upper cylinder is 4mm and the height is 60mm; the inner diameter of the lower cylinder is 10mm and the height is 60mm. Figure 7 shown.
[0105] Step 1: Select 2195 aluminum rods with diameters of 4mm and 10mm, soak them in a dilute acid solution, rinse them with clean water to remove the surface oxide layer, use anhydrous ethanol to clean the surface oil stains, and then put them into the corresponding receiving through holes.
[0106] Step 2: Place the 2195 aluminum plate at the bottom.
[0107] Step 3: Start the stirring head, and the stirring needle penetrates into the substrate, so that the stirring head contacts the substrate. After rotating and preheating for 30 seconds, it is retracted. At the same time, the metal rod enters the stirring head and contacts the substrate, and stirring additive manufacturing begins until the component is completely formed. When printing the thicker cylinder at the bottom, the rod diameter used is 10mm. After the bottom printing is completed and the upper part is printed, the rod diameter changes to 4mm, and the layer thickness is 0.4mm.
[0108] The parameters of the friction stir treatment are as follows: the stirring head speed is 1500 r / min, the travel speed is 100 mm / min, the stirring head penetrates 2 mm into the substrate, retracts 1.5 mm, the retraction speed is 1 mm / min, and the downward pressure of the stirring head is 200 N.
[0109] Step 4: Wait for the print to cool down and remove it.
[0110] Step 5: The obtained print is annealed by heating to 400°C at a rate of 15°C / s, keeping warm for 2h, and then cooling with the furnace at a cooling temperature of less than 10°C per hour. It is cooled to 200°C and taken out of the furnace, and placed in the air to cool to room temperature to eliminate residual stress. Comparative Example 1
[0111] The printed parts are the same as in Example 1.
[0112] Step 1: Select a 2060 aluminum-based rod with a diameter of 4 mm, soak it in a dilute acid solution, rinse it with clean water to remove the surface oxide layer, use anhydrous ethanol to clean the surface oil stains, and then put it into the corresponding receiving through hole.
[0113] Step 2: Place the 2060 aluminum plate at the bottom.
[0114] Step 3: Start the stirring head, insert the stirring needle into the substrate, make the stirring head contact with the substrate, rotate and preheat for 30 seconds, then retract. At the same time, the metal rod enters the stirring head and contacts with the substrate, and stirring additive manufacturing begins until the component is completely formed. During the printing process, a rod with a diameter of 4mm is always used. When printing a single-channel reinforcement with a width of 8mm, the overlap rate is 50% and the layer thickness is 0.4mm.
[0115] The parameters of the friction stir treatment are as follows: the stirring head speed is 1500 r / min, the travel speed is 100 mm / min, the stirring head penetrates 2 mm into the substrate, retracts 1.5 mm, the retraction speed is 1 mm / min, and the downward pressure of the stirring head is 200 N.
[0116] Step 4: Wait for the print to cool down and remove it.
[0117] Step 5: Anneal the printed parts, heat them to 400 degrees at a rate of 15 degrees / second, keep them warm for 2 hours, and then cool them in the furnace at a cooling rate of less than 10 degrees per hour. Cool them to 200 degrees and take them out of the furnace, and cool them in the air to room temperature to eliminate residual stress. Comparative Example 2
[0118] The printed parts are the same as in Example 2.
[0119] Step 1: Select a 2195 aluminum rod with a diameter of 4 mm, soak it in a dilute acid solution, rinse it with clean water to remove the surface oxide layer, use anhydrous ethanol to clean the surface oil stains, and then put it into the corresponding receiving through hole.
[0120] Step 2: Place the 2195 aluminum plate at the bottom.
[0121] Step 3: Start the stirring head, insert the stirring needle into the substrate, make the stirring head contact with the substrate, rotate and preheat for 30 seconds, then retract. At the same time, the metal rod enters the stirring head and contacts with the substrate, and the stirring additive manufacturing starts until the component is completely formed. During the printing process, a rod with a diameter of 4mm is always used. When printing a thicker cylinder at the bottom, the overlap rate is 50% and the layer thickness is 0.4mm.
[0122] The parameters of the friction stir treatment are as follows: the stirring head speed is 1500 r / min, the travel speed is 100 mm / min, the stirring head penetrates 2 mm into the substrate, retracts 1.5 mm, the retraction speed is 1 mm / min, and the downward pressure of the stirring head is 200 N.
[0123] Step 4: Wait for the print to cool down and remove it.
[0124] Step 5: The obtained print is annealed by heating to 400°C at a rate of 15°C / s, keeping warm for 2h, and then cooling with the furnace at a cooling temperature of less than 10°C per hour. It is cooled to 200°C and taken out of the furnace, and placed in the air to cool to room temperature to eliminate residual stress.
[0125] Performance Testing
[0126] The performance tests were carried out on the components of Examples 1-2 and Comparative Examples 1-2, and the results are shown in the following table.
[0127]
[0128] It can be seen from the test results that the surface quality of the components prepared by the method of the present invention is better, the mechanical properties are improved to a certain extent, and the preparation time is shortened by at least 33%, thereby improving the production efficiency.
[0129] Although the present invention has been disclosed as above with preferred embodiments, it is not intended to limit the present invention. A person with ordinary knowledge in the technical field to which the present invention belongs may make various changes and modifications without departing from the spirit and scope of the present invention. Therefore, the protection scope of the present invention shall be determined by the definition of the claims.
Claims
1. A friction stir additive manufacturing method for a metal component with a variable path width, characterized in that: include: Using a plurality of metal rods with different diameters as raw materials, a stir friction additive manufacturing process is adopted, and deposition is performed layer by layer on a substrate in an upward growth manner starting from the first layer according to a preset program until the deposition of the last layer is completed, thereby obtaining the desired metal component; the metal component is a metal plate with a reinforcing rib structure of different widths or a cylindrical part with different wall thicknesses; The stirring needle is inserted into the substrate or the previous deposition layer, and the end face of the stirring head is in contact with the surface of the substrate or the previous deposition layer for preheating. Then, the stirring head is retracted to keep a certain distance between the end face of the stirring head and the surface of the substrate or the previous deposition layer. The metal rod enters and extends out of the stirring head until it contacts the surface of the substrate or the previous deposition layer, and is driven by the stirring head to perform synchronous rotation and plasticization to deposit a new deposition layer, so that the width of the deposition layer is equal to the diameter of the metal rod. When the width of the deposition layer needs to be changed, a metal rod with a diameter equal to the required deposition layer width is directly selected as the raw material to obtain the required path width; during the printing process, different metal rods are switched for stir friction additive manufacturing for reinforcing rib structures of different widths or different wall thicknesses of cylindrical parts.
2. The friction stir additive manufacturing method for a metal component with a variable path width according to claim 1, characterized in that: The metal component is a metal plate with reinforcing rib structures of different widths, including the following preparation process: Using metal bars as raw materials and the stir friction additive manufacturing process, a reinforcing rib structure is formed on the surface of the metal plate in a single pass in a horizontal and vertical orthogonal cross-section according to a preset program, and there is a spacing between adjacent single passes in the same direction; Among them, two metal bars with different diameters are used as raw materials to print transverse reinforcement ribs and longitudinal reinforcement ribs respectively, so that the widths of the transverse reinforcement ribs and the longitudinal reinforcement ribs are not equal, and metal plates with reinforcement rib structures of different widths are obtained.
3. The friction stir additive manufacturing method for a metal component with a variable path width according to claim 2, characterized in that: The spacing range between adjacent single passes can be set according to the strength and rigidity requirements of the metal sheet.
4. The friction stir additive manufacturing method for a metal component with a variable path width according to claim 1, characterized in that: The metal component is a cylindrical part with different wall thicknesses, and the preparation process includes the following steps: Using a metal rod with a first diameter as a raw material, a stir friction additive manufacturing process is used to deposit layer by layer starting from a first layer on the surface of the substrate in an upward growth manner according to a preset program to obtain a cylindrical part with a first wall thickness, wherein the first wall thickness is equal to the first diameter; Using a metal rod having a second diameter as a raw material, a stir friction additive manufacturing process is used to continue to deposit layer by layer in an upward growth manner on the cylindrical part having a first wall thickness according to a preset program to obtain a cylindrical part having a second wall thickness, wherein the second wall thickness is equal to the second diameter; And so on, until the required cylindrical parts with different wall thicknesses are obtained.
5. The friction stir additive manufacturing method for a metal component with a variable path width according to any one of claims 1 to 4, characterized in that: The metal type is aluminum alloy, magnesium alloy, copper alloy or titanium alloy.
6. The friction stir additive manufacturing method for a metal component with a variable path width according to any one of claims 1 to 4, characterized in that: The friction stir additive manufacturing process is configured to determine the feed speed of the metal bar and the process parameters of the friction stir treatment according to the printing structure parameters, and to set the printing program accordingly to print and form the parts.
7. The friction stir additive manufacturing method for a metal component with a variable path width according to any one of claims 1 to 4, characterized in that: The friction stir additive manufacturing method also includes annealing the printed parts.
8. A variable diameter continuous feeding friction stir additive manufacturing device, characterized in that: include: A material feeding system (100) comprises a raw material container (110), wherein the raw material container (110) is provided with a plurality of through holes (111) for accommodating metal bars of different diameters; The upper end of the raw material container (110) is provided with a pushing mechanism (120) for pushing the metal bar, and the lower end of the raw material container (110) is sleeved with a feeding mechanism (130), wherein the feeding mechanism (130) is provided with a first passage (131) for only one metal bar to pass through; The raw material container (110) is also provided with a transmission mechanism (140). The raw material container (110) is pushed and pulled by the transmission mechanism (140) so that the position of the metal bar placed in the through hole (111) corresponds to the position of the first channel (131) on the feeding mechanism. The pushing mechanism (120) pushes the metal bar of a required diameter, and the metal bar is transported to the friction stir additive manufacturing system through the first channel (131). A friction stir additive manufacturing system (200) disposed below the material feeding system (100), comprising a stirring head, wherein the stirring head comprises a connecting portion (210), a shaft shoulder portion (220), and a stirring needle (230) which are connected in sequence; A second channel (211) is provided in the connecting portion (210) and is passed through. The metal bar passing through the first channel (131) is transported to the second channel (211) via a traction mechanism (212). A gathering mechanism (2110) is provided in the second channel (211). The gathering mechanism (2110) allows the diameter of the second channel to match that of the metal bar, and the metal bar is further transported to the shaft shoulder portion (220). A third channel (221) is provided in the shaft shoulder portion (220) and is connected to the second channel (211). The metal rod enters the third channel (221) from the second channel (211) and is transported along the third channel (221) to the surface of the area to be added. The stirring needle (230) is arranged on the end surface of the shaft shoulder (220) away from the connecting portion (210) and is used to promote the flow of surrounding materials; The friction stir additive manufacturing system (200) is connected to a control drive system, and the control drive system is configured to perform friction stir additive manufacturing on the metal rod output from the shaft shoulder; When printing metal plates with reinforcing rib structures of different widths or cylindrical parts with different wall thicknesses, the pushing mechanism (120) is used to push metal rods placed in different through holes (111) for reinforcing rib structures of different widths or different wall thickness parts of the cylindrical parts, and different metal rods are switched to perform friction stir additive manufacturing.
9. The variable diameter continuous feeding friction stir additive manufacturing device according to claim 8, characterized in that: The gathering mechanism (2110) comprises a plurality of clamping devices (2111), wherein the clamping devices (2111) comprise an inner ring (2111A), an outer ring (2111B) and a plurality of pre-tightening mechanisms (2111C) arranged between the inner ring (2111A) and the outer ring (2111B), and the pre-tightening mechanisms (2111C) enable the inner ring (2111A) and the outer ring (2111B) to maintain a tendency to move away from each other.
10. The variable diameter continuous feeding friction stir additive manufacturing device according to claim 8, characterized in that: The preload mechanism (2111C) is a spring with preload force.
11. The variable diameter continuous feeding friction stir additive manufacturing device according to claim 9, characterized in that: The top of the inner ring (2111A) is in the shape of a funnel with a larger top and a smaller bottom, so as to facilitate the entry of bars of different diameters.
12. The variable diameter continuous feeding friction stir additive manufacturing device according to claim 8, characterized in that: The traction mechanism (212) is a set of adjustable roller wheels, which pull the metal bar to move downward at a constant speed into the second channel (211).
Citation Information
Cited By
Impeller type stirring friction deposition additive stirring head and using method thereof
CN118060702A