Antibacterial and wear-resistant antistatic composite fabric and preparation method thereof
Through the reaction of nano titanium dioxide with γ-glycidoxypropyltrimethoxysilane and lauryl amide, combined with ultrasonic dispersion technology, an antibacterial and antistatic finishing agent was prepared, which solved the poor antibacterial performance and static electricity problems of nylon yarn and linen yarn composite fabrics. , improves the antibacterial and antistatic properties, and maintains the wear resistance and breathability of the fabric.
Patent Information
- Application Number
- CN202310801618.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-07-03
- Publication Date
- 2024-10-01
- Estimated Expiration
- 2043-07-03
AI Technical Summary
In the existing technology, composite fabrics made from nylon yarn and linen yarn as raw materials have poor antibacterial performance, are prone to generate static electricity, and have poor breathability after the waterproof performance is improved.
Epoxy-modified nano-titanium dioxide is prepared by reacting nano-titanium dioxide with γ-glycidoxypropyltrimethoxysilane. It is combined with lauryl amide and dimethyl sulfate for quaternization treatment to form an antibacterial and antistatic finishing agent, which is dispersed by ultrasonic The composite fabric base fabric twisted with linen yarn and nylon yarn is impregnated to improve the antibacterial and antistatic properties.
It significantly improves the antibacterial, wear-resistant and antistatic properties of composite fabrics, ensuring the wear-resistant properties of the fabrics while avoiding a reduction in breathability.
Smart Images

Figure CN116676772B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of textile fabrics, and in particular to an antibacterial, wear-resistant, antistatic composite fabric and a preparation method thereof. Background Art
[0002] With the continuous improvement of living standards, people have higher and higher requirements for the functionality of clothing fabrics, especially the wear resistance and antibacterial properties of fabrics. Clothing is often worn out due to friction during wearing and use, which affects the functionality and aesthetics of clothing. Therefore, there are higher requirements for the wear resistance of clothing fabrics. Nylon (polyamide fiber) in synthetic fibers has high wear resistance. Linen yarn made from linen fiber in natural plant fibers not only has good wear resistance, but also has good antibacterial properties. Chinese patent application CN110257998A discloses a process for making a fabric containing linen yarn. Through the combination of nylon yarn and linen yarn, the fabric has both wear resistance and antibacterial properties. At the same time, the presence of nylon yarn can also improve the poor touch of pure linen yarn fabric. However, the antibacterial property of the fabric only depends on the antibacterial property of the linen yarn itself, and the antibacterial effect is poor. In addition, due to the lack of hydrophilic groups in the molecular structure of nylon, the surface resistivity of nylon fiber is extremely large, and static electricity is easily generated during processing and wearing. Chinese patent application CN114055873A discloses an antistatic wear-resistant fabric, which includes a wear-resistant layer, a tensile layer, an antistatic layer, an anti-radiation layer, an antibacterial layer and a thermal insulation layer from the outside to the inside, and has good antistatic effect, radiation protection effect and antibacterial effect, but the comprehensive performance of the fabric can only be achieved by the joint action of the multi-layer structure. Chinese patent application CN115354502A discloses a wear-resistant and water-resistant composite fabric, which twists nylon fiber, polyamide fiber and polyester fiber into composite yarn in a twisting machine, weaves the composite yarn to obtain a fabric body, and then immerses the fabric body in a pretreatment liquid to obtain a pretreated fabric, and coats the pretreated fabric with a coating rubber of a wear-resistant and waterproof coating to obtain a wear-resistant and water-resistant composite fabric. The fabric has good wear resistance and waterproof performance, but with the realization of waterproof performance, the air permeability of the fabric will be relatively poor. Chinese patent application CN109610075A discloses an antibacterial cotton nylon graphene twill fabric, which is a two-up-one-down twill structure woven from warp yarn and weft yarn, wherein the warp yarn is cotton yarn made of combed cotton and spun by ring spinning, and the weft yarn is nylon and nylon containing graphene, wherein the pure nylon and the nylon containing graphene are distributed at intervals, and 0.5-5% of graphene material is added to the spinning solution of the graphene-containing nylon during the nylon spinning process. Due to the presence of the graphene material, the fabric has good antibacterial, UV protection, antistatic and other characteristics, but the dispersion uniformity of graphene in the spinning solution is difficult to ensure, which in turn affects the stability of the performance. Summary of the invention
[0003] In view of the deficiencies in the prior art, the present invention provides an antibacterial, wear-resistant and antistatic composite fabric and a preparation method thereof, so as to solve the problems in the prior art that the composite fabric made of nylon yarn and linen yarn as raw materials has poor antibacterial performance and is prone to static electricity.
[0004] In order to achieve the above object, the technical solution adopted by the present invention is as follows:
[0005] A method for preparing an antibacterial, wear-resistant and antistatic composite fabric comprises the following steps:
[0006] Step 1, adding nano titanium dioxide and γ-glycidyloxypropyltrimethoxysilane to an ethanol aqueous solution, reacting, filtering, and drying after the reaction to obtain epoxy-modified nano titanium dioxide;
[0007] Step 2, adding lauramide and epoxy-modified nano titanium dioxide into ethanol, adding triethylamine at a pH value of 9.5-10.5, reacting, filtering, washing, and drying after the reaction to obtain nano titanium dioxide grafted with lauroyl diethanolamide;
[0008] Step 3, adding nano titanium dioxide grafted with lauroyl diethanolamine and dimethyl sulfate to isopropanol for reaction, and then rotary evaporating to obtain an antibacterial and antistatic finishing agent;
[0009] Step 4, adding the antibacterial and antistatic finishing agent into deionized water, and ultrasonically dispersing the mixture to obtain an antibacterial and antistatic finishing liquid;
[0010] The linen yarn and the nylon yarn are twisted and plied to obtain a composite yarn, and the composite yarn is used as a warp yarn and a weft yarn respectively to manufacture a composite fabric base cloth, and the composite fabric base cloth is immersed in an antibacterial and antistatic finishing liquid, double immersed and double rolled, and dried to obtain an antibacterial and wear-resistant antistatic composite fabric.
[0011] Preferably, in step 1, the mass ratio of nano-titanium dioxide, γ-glycidyloxypropyltrimethoxysilane and ethanol aqueous solution is 80:(250-270):(1500-2000), and the reaction conditions are 70-80° C. for 4-5 hours.
[0012] Preferably, the ethanol aqueous solution comprises 90wt%-95wt% ethanol aqueous solution.
[0013] Preferably, in step 2, the mass ratio of lauramide, epoxy-modified nano-titanium dioxide and ethanol is 200:(630-660):(3000-5000), and the reaction conditions are 75-85° C. for 3-5 hours.
[0014] Preferably, in step three: the mass ratio of nano-titanium dioxide grafted with lauroyl diethanolamine, dimethyl sulfate and isopropanol is 850:(130-150):(1000-1500), and the reaction conditions are 80-90° C. for 2.5-3.5 hours.
[0015] Preferably, in step 4: the mass ratio of the antibacterial and antistatic finishing agent to deionized water is (1-10):(90-99).
[0016] Preferably, the frequency of ultrasonic dispersion is 20-40 KHz, and the time of ultrasonic dispersion is 10-20 min.
[0017] Preferably, in step 4: the ratio of the number of linen yarns to the number of nylon yarns is (2-4):(10-20), and the density of the composite fabric base cloth is that the total number of warp yarns and weft yarns per square inch of fabric is not less than 200.
[0018] Preferably, in step 4: the bath ratio of the immersion treatment is 1:(20-30), the immersion temperature is 50-60° C., and the immersion time is 20-30 min.
[0019] Preferably, the present invention provides an antibacterial, wear-resistant and antistatic composite fabric prepared by the above-mentioned method for preparing the antibacterial, wear-resistant and antistatic composite fabric.
[0020] Compared with the prior art, the present invention has the following beneficial effects:
[0021] In the present invention, the composite fabric base fabric is prepared by using linen yarn and nylon yarn as raw materials. Both the linen yarn and the nylon yarn have good wear resistance, and the prepared composite fabric has good wear resistance. Then, the composite fabric base fabric is immersed in an antibacterial and antistatic finishing liquid to obtain an antibacterial and wear-resistant antistatic composite fabric.
[0022] In the present invention, when preparing the antibacterial and antistatic finishing agent, nano titanium dioxide with antibacterial effect is firstly reacted with γ-glycidyloxypropyltrimethoxysilane to obtain epoxy-modified nano titanium dioxide, and then the epoxy-modified nano titanium dioxide is reacted with lauramide to obtain non-ionic antistatic agent nano titanium dioxide grafted with lauryl diethanolamine, and finally the nano titanium dioxide grafted with lauryl diethanolamine is subjected to a quaternization reaction with dimethyl sulfate to obtain a quaternary ammonium salt type antibacterial and antistatic finishing agent, that is, a cationic antibacterial and antistatic finishing agent, which can improve the adsorption effect on the surface of the composite fabric and improve the antistatic performance; at the same time, the quaternary ammonium salt has a good antibacterial effect, and on the basis of the nano titanium dioxide, the antibacterial performance of the antibacterial and antistatic finishing agent is further improved. BRIEF DESCRIPTION OF THE DRAWINGS
[0023] Figure 1The flowchart is a process for preparing the antibacterial and wear-resistant antistatic composite fabric of the present invention;
[0024] Figure 2 The figure is a flow chart of the preparation process of the antibacterial and antistatic finishing agent of the present invention;
[0025] Figure 3 The schematic diagram of the reaction of lauryl amide and epoxy-modified nano-titanium dioxide to prepare nano-titanium dioxide grafted with lauroyl diethanolamide in the present invention. DETAILED DESCRIPTION
[0026] The technical solutions in the embodiments of the present invention will be clearly and completely described below in conjunction with the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, rather than all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present invention.
[0027] Example 1
[0028] A method for preparing an antibacterial, wear-resistant and antistatic composite fabric comprises the following steps:
[0029] Step 1, adding nano titanium dioxide and γ-glycidyloxypropyltrimethoxysilane to a 90wt% ethanol aqueous solution, the mass ratio of nano titanium dioxide, γ-glycidyloxypropyltrimethoxysilane, and 90wt% ethanol aqueous solution is 80:250:1500, reacting at 70°C for 5h, filtering after the reaction, and drying at 55°C for 15h to obtain epoxy-modified nano titanium dioxide;
[0030] Step 2: adding lauramide and epoxy-modified nano titanium dioxide to ethanol, wherein the mass ratio of lauramide, epoxy-modified nano titanium dioxide and ethanol is 200:630:3000, adding triethylamine at a pH value of 9.5, reacting at 75° C. for 5 h, filtering after the reaction, washing with ethanol, and drying at 55° C. for 15 h to obtain nano titanium dioxide grafted with lauroyl diethanolamide;
[0031] Step 3: adding nano titanium dioxide grafted lauroyl diethanolamine and dimethyl sulfate to isopropanol, wherein the mass ratio of nano titanium dioxide grafted lauroyl diethanolamine, dimethyl sulfate and isopropanol is 850:130:1000, reacting at 80° C. for 2.5 hours, and after the reaction, rotary evaporating at 75° C. to obtain an antibacterial and antistatic finishing agent;
[0032] Step 4: adding the antibacterial and antistatic finishing agent to deionized water, wherein the mass ratio of the antibacterial and antistatic finishing agent to deionized water is 10:90, and performing ultrasonic dispersion at 40KHz for 10 minutes to obtain an antibacterial and antistatic finishing liquid;
[0033] The linen yarn and the nylon yarn are twisted and plied at a root ratio of 2:10 with a twist of 80 twists / 10cm to obtain a composite yarn. The composite yarn is used as warp yarn and weft yarn respectively to manufacture a composite fabric base cloth. The density of the composite fabric base cloth is 236 warp yarns and 116 weft yarns per square inch. The composite fabric base cloth is immersed in an antibacterial and antistatic finishing liquid with a bath ratio of 1:10, an immersion temperature of 50°C, an immersion time of 30min, two immersions and two rollings, and dried at 65°C for 2.5h to obtain an antibacterial and wear-resistant antistatic composite fabric.
[0034] Example 2
[0035] A method for preparing an antibacterial, wear-resistant and antistatic composite fabric comprises the following steps:
[0036] Step 1, adding nano titanium dioxide and γ-glycidyloxypropyltrimethoxysilane to a 95wt% ethanol aqueous solution, the mass ratio of nano titanium dioxide, γ-glycidyloxypropyltrimethoxysilane, and 95wt% ethanol aqueous solution is 80:270:2000, reacting at 80°C for 4h, filtering after the reaction, and drying at 65°C for 10h to obtain epoxy-modified nano titanium dioxide;
[0037] Step 2: adding lauramide and epoxy-modified nano titanium dioxide to ethanol, wherein the mass ratio of lauramide, epoxy-modified nano titanium dioxide and ethanol is 200:660:5000, adding triethylamine at a pH value of 10.5, reacting at 85° C. for 3 h, filtering after the reaction, washing with ethanol, and drying at 65° C. for 10 h to obtain nano titanium dioxide grafted with lauroyl diethanolamide;
[0038] Step 3: adding nano titanium dioxide grafted with lauroyl diethanolamine and dimethyl sulfate to isopropanol, wherein the mass ratio of nano titanium dioxide grafted with lauroyl diethanolamine, dimethyl sulfate and isopropanol is 850:150:1500, reacting at 90° C. for 3.5 hours, and after the reaction, rotary evaporating at 75° C. to obtain an antibacterial and antistatic finishing agent;
[0039] Step 4: adding the antibacterial and antistatic finishing agent to deionized water at a mass ratio of 1:99, and dispersing by ultrasonic at 20KHz for 20min to obtain an antibacterial and antistatic finishing liquid;
[0040] The linen yarn and the nylon yarn are twisted and plied at a root ratio of 4:20 with a twist of 120 twists / 10cm to obtain a composite yarn, and the composite yarn is used as warp yarn and weft yarn respectively to manufacture a composite fabric base cloth. The density of the composite fabric base cloth is 140 warp yarns and 110 weft yarns per square inch. The composite fabric base cloth is immersed in an antibacterial and antistatic finishing liquid with a bath ratio of 1:20, an immersion temperature of 60°C, an immersion time of 20min, two immersions and two rollings, and dried at 70°C for 2h to obtain an antibacterial and wear-resistant antistatic composite fabric.
[0041] Example 3
[0042] A method for preparing an antibacterial, wear-resistant and antistatic composite fabric comprises the following steps:
[0043] Step 1, adding nano titanium dioxide and γ-glycidyloxypropyltrimethoxysilane to a 90wt% ethanol aqueous solution, the mass ratio of nano titanium dioxide, γ-glycidyloxypropyltrimethoxysilane, and 90wt% ethanol aqueous solution is 80:254:1600, reacting at 75°C for 4.5h, filtering after the reaction, and drying at 60°C for 12h to obtain epoxy-modified nano titanium dioxide;
[0044] Step 2: adding lauramide and epoxy-modified nano titanium dioxide to ethanol, wherein the mass ratio of lauramide, epoxy-modified nano titanium dioxide and ethanol is 200:636:3400, adding triethylamine at a pH value of 10, reacting at 80° C. for 4 h, filtering after the reaction, washing with ethanol, and drying at 60° C. for 13 h to obtain nano titanium dioxide grafted with lauroyl diethanolamide;
[0045] Step 3: adding nano titanium dioxide grafted lauryl diethanolamine and dimethyl sulfate to isopropanol, wherein the mass ratio of nano titanium dioxide grafted lauryl diethanolamine, dimethyl sulfate and isopropanol is 850:134:1100, reacting at 85° C. for 2 h, and after the reaction, rotary evaporating at 75° C. to obtain an antibacterial and antistatic finishing agent;
[0046] Step 4: adding the antibacterial and antistatic finishing agent to deionized water, wherein the mass ratio of the antibacterial and antistatic finishing agent to deionized water is 8.5:91.5, and performing ultrasonic dispersion at 30KHz for 15 minutes to obtain an antibacterial and antistatic finishing liquid;
[0047] The linen yarn and the nylon yarn are twisted and plied at a root ratio of 3:12 and a twist of 100 twists / 10cm to obtain a composite yarn. The composite yarn is used as warp yarn and weft yarn respectively to manufacture a composite fabric base cloth. The density of the composite fabric base cloth is 172 warp yarns and 143 weft yarns per square inch. The composite fabric base cloth is immersed in an antibacterial and antistatic finishing liquid with a bath ratio of 1:15, an immersion temperature of 55°C, an immersion time of 25min, two immersions and two rollings, and dried at 60°C for 3h to obtain an antibacterial and wear-resistant antistatic composite fabric.
[0048] Example 4
[0049] A method for preparing an antibacterial, wear-resistant and antistatic composite fabric comprises the following steps:
[0050] Step 1, adding nano titanium dioxide and γ-glycidyloxypropyltrimethoxysilane to a 90wt% ethanol aqueous solution, the mass ratio of nano titanium dioxide, γ-glycidyloxypropyltrimethoxysilane, and 90wt% ethanol aqueous solution is 80:258:1700, reacting at 75°C for 4.5h, filtering after the reaction, and drying at 60°C for 12h to obtain epoxy-modified nano titanium dioxide;
[0051] Step 2: adding lauramide and epoxy-modified nano titanium dioxide to ethanol, wherein the mass ratio of lauramide, epoxy-modified nano titanium dioxide and ethanol is 200:642:3800, adding triethylamine at a pH value of 10, reacting at 80° C. for 4 h, filtering after the reaction, washing with ethanol, and drying at 55° C. for 15 h to obtain nano titanium dioxide grafted with lauroyl diethanolamide;
[0052] Step 3: adding nano titanium dioxide grafted with lauroyl diethanolamine and dimethyl sulfate to isopropanol, wherein the mass ratio of nano titanium dioxide grafted with lauroyl diethanolamine, dimethyl sulfate and isopropanol is 850:138:1200, reacting at 85° C. for 3 h, and after the reaction, rotary evaporating at 75° C. to obtain an antibacterial and antistatic finishing agent;
[0053] Step 4: adding the antibacterial and antistatic finishing agent to deionized water, wherein the mass ratio of the antibacterial and antistatic finishing agent to deionized water is 6:94, and performing ultrasonic dispersion at 30KHz for 15 minutes to obtain an antibacterial and antistatic finishing liquid;
[0054] The linen yarn and the nylon yarn are twisted and plied at a root ratio of 3:14 and a twist of 100 twists / 10cm to obtain a composite yarn. The composite yarn is used as warp yarn and weft yarn respectively to manufacture a composite fabric base cloth. The density of the composite fabric base cloth is 172 warp yarns and 143 weft yarns per square inch. The composite fabric base cloth is immersed in an antibacterial and antistatic finishing liquid with a bath ratio of 1:15, an immersion temperature of 55°C, an immersion time of 25min, two immersions and two rollings, and dried at 60°C for 3h to obtain an antibacterial and wear-resistant antistatic composite fabric.
[0055] Example 5
[0056] A method for preparing an antibacterial, wear-resistant and antistatic composite fabric comprises the following steps:
[0057] Step 1, adding nano titanium dioxide and γ-glycidyloxypropyltrimethoxysilane to a 90wt% ethanol aqueous solution, the mass ratio of nano titanium dioxide, γ-glycidyloxypropyltrimethoxysilane, and 90wt% ethanol aqueous solution is 80:262:1800, reacting at 75°C for 4.5h, filtering after the reaction, and drying at 60°C for 12h to obtain epoxy-modified nano titanium dioxide;
[0058] Step 2: adding lauramide and epoxy-modified nano titanium dioxide to ethanol, wherein the mass ratio of lauramide, epoxy-modified nano titanium dioxide and ethanol is 200:652:4200, adding triethylamine at a pH value of 10, reacting at 80°C for 4 hours, filtering, washing with ethanol, and drying at 55°C for 15 hours to obtain nano titanium dioxide grafted with lauroyl diethanolamide;
[0059] Step 3: adding nano titanium dioxide grafted lauroyl diethanolamine and dimethyl sulfate to isopropanol, wherein the mass ratio of nano titanium dioxide grafted lauroyl diethanolamine, dimethyl sulfate and isopropanol is 850:146:1300, reacting at 80° C. for 2.5 hours, and after the reaction, rotary evaporating at 75° C. to obtain an antibacterial and antistatic finishing agent;
[0060] Step 4: adding the antibacterial and antistatic finishing agent to deionized water, wherein the mass ratio of the antibacterial and antistatic finishing agent to deionized water is 4.5:96.5, and performing ultrasonic dispersion at 30KHz for 15 minutes to obtain an antibacterial and antistatic finishing liquid;
[0061] The linen yarn and the nylon yarn are twisted and plied at a root ratio of 3:16 with a twist of 120 twists / 10cm to obtain a composite yarn. The composite yarn is used as warp yarn and weft yarn respectively to manufacture a composite fabric base cloth. The density of the composite fabric base cloth is 172 warp yarns and 143 weft yarns per square inch. The composite fabric base cloth is immersed in an antibacterial and antistatic finishing liquid with a bath ratio of 1:15, an immersion temperature of 55°C, an immersion time of 25min, two immersions and two rollings, and dried at 60°C for 3h to obtain an antibacterial and wear-resistant antistatic composite fabric.
[0062] Example 6
[0063] A method for preparing an antibacterial, wear-resistant and antistatic composite fabric comprises the following steps:
[0064] Step 1, adding nano titanium dioxide and γ-glycidyloxypropyltrimethoxysilane to a 90wt% ethanol aqueous solution, the mass ratio of nano titanium dioxide, γ-glycidyloxypropyltrimethoxysilane, and 90wt% ethanol aqueous solution is 80:266:1900, reacting at 75°C for 4.5h, filtering after the reaction, and drying at 60°C for 12h to obtain epoxy-modified nano titanium dioxide;
[0065] Step 2: adding lauramide and epoxy-modified nano titanium dioxide to ethanol, wherein the mass ratio of lauramide, epoxy-modified nano titanium dioxide and ethanol is 200:656:4600, adding triethylamine at a pH value of 10, reacting at 80°C for 4 hours, filtering after the reaction, washing with ethanol, and drying at 55°C for 15 hours to obtain nano titanium dioxide grafted with lauroyl diethanolamide;
[0066] Step 3: adding nano titanium dioxide grafted lauroyl diethanolamine and dimethyl sulfate to isopropanol, wherein the mass ratio of nano titanium dioxide grafted lauroyl diethanolamine, dimethyl sulfate and isopropanol is 850:146:1400, reacting at 80° C. for 2.5 hours, and after the reaction, rotary evaporating at 75° C. to obtain an antibacterial and antistatic finishing agent;
[0067] Step 4: adding the antibacterial and antistatic finishing agent to deionized water at a mass ratio of 3:97, and dispersing by ultrasonic at 30KHz for 15 minutes to obtain an antibacterial and antistatic finishing liquid;
[0068] The linen yarn and the nylon yarn are twisted and plied at a root ratio of 3:18 and a twist of 120 twists / 10cm to obtain a composite yarn. The composite yarn is used as warp yarn and weft yarn respectively to manufacture a composite fabric base cloth. The density of the composite fabric base cloth is 172 warp yarns and 143 weft yarns per square inch. The composite fabric base cloth is immersed in an antibacterial and antistatic finishing liquid with a bath ratio of 1:15, an immersion temperature of 55°C, an immersion time of 25min, two immersions and two rollings, and dried at 60°C for 3h to obtain an antibacterial and wear-resistant antistatic composite fabric.
[0069] Comparative Example 1
[0070] A method for preparing an antibacterial, wear-resistant and antistatic composite fabric comprises the following steps:
[0071] Step 1, adding nano titanium dioxide and γ-glycidyloxypropyltrimethoxysilane to a 95wt% ethanol aqueous solution, the mass ratio of nano titanium dioxide, γ-glycidyloxypropyltrimethoxysilane, and 95wt% ethanol aqueous solution is 80:270:2000, reacting at 80°C for 4h, filtering after the reaction, and drying at 65°C for 10h to obtain epoxy-modified nano titanium dioxide;
[0072] Step 2: adding lauramide and epoxy-modified nano titanium dioxide to ethanol, wherein the mass ratio of lauramide, epoxy-modified nano titanium dioxide and ethanol is 200:660:5000, adding triethylamine at a pH value of 10.5, reacting at 85° C. for 3 h, filtering after the reaction, washing with ethanol, and drying at 65° C. for 10 h to obtain nano titanium dioxide grafted with lauroyl diethanolamide;
[0073] Step 3: adding nano titanium dioxide grafted lauryl diethanolamine to deionized water, wherein the mass ratio of nano titanium dioxide grafted lauryl diethanolamine to deionized water is 1:99, and performing ultrasonic dispersion at 20KHz for 20 minutes to obtain an antibacterial and antistatic finishing liquid;
[0074] The linen yarn and the nylon yarn are twisted and plied at a root ratio of 4:20 with a twist of 120 twists / 10cm to obtain a composite yarn, and the composite yarn is used as warp yarn and weft yarn respectively to manufacture a composite fabric base cloth. The density of the composite fabric base cloth is 140 warp yarns and 110 weft yarns per square inch. The composite fabric base cloth is immersed in an antibacterial and antistatic finishing liquid with a bath ratio of 1:20, an immersion temperature of 60°C, an immersion time of 20min, two immersions and two rollings, and dried at 70°C for 2h to obtain an antibacterial and wear-resistant antistatic composite fabric.
[0075] Comparative Example 2
[0076] A method for preparing an antibacterial, wear-resistant and antistatic composite fabric comprises the following steps:
[0077] Step 1: adding lauroyl diethanolamine and nano titanium dioxide into deionized water, wherein the mass ratio of lauroyl diethanolamine, nano titanium dioxide and deionized water is 0.64:0.36:99, and performing ultrasonic dispersion at 20KHz for 20 minutes to obtain an antibacterial and antistatic finishing liquid;
[0078] The linen yarn and the nylon yarn are twisted and plied at a root ratio of 4:20 with a twist of 120 twists / 10cm to obtain a composite yarn, and the composite yarn is used as warp yarn and weft yarn respectively to manufacture a composite fabric base cloth. The density of the composite fabric base cloth is 140 warp yarns and 110 weft yarns per square inch. The composite fabric base cloth is immersed in an antibacterial and antistatic finishing liquid with a bath ratio of 1:20, an immersion temperature of 60°C, an immersion time of 20min, two immersions and two rollings, and dried at 70°C for 2h to obtain an antibacterial and wear-resistant antistatic composite fabric.
[0079] In the above embodiments and comparative examples: nano titanium dioxide was purchased from Darcin Nano Technology (Changzhou) Co., Ltd., crystal form: anatase, average particle size: 30-50nm; the yarn count of the linen yarn was 36Nm (metric yarn count), spun from linen fiber, the linen fiber was purchased from Haiyan Jinyi Silk Spinning Co., Ltd., item number: L100, and the fiber length was 130mm; the nylon yarn was nylon yarn 66, purchased from Shenzhen Teli Chemical Fiber Co., Ltd., item number: LLJL, and the fineness was: 50D.
[0080] Test example
[0081] The performance tests were conducted on the antibacterial and wear-resistant antistatic composite fabrics prepared in the above-mentioned embodiments and comparative examples:
[0082] (1) Wear resistance test: The antibacterial and wear-resistant antistatic composite fabrics prepared in Examples 1-6 and Comparative Examples 1-2 were taken, with a diameter of 150 cm, and subjected to friction test using a fabric flat grinder with a weight of 400 g. The weight loss rate after 300 revolutions of friction was measured. The test results are shown in Table 1:
[0083] Table 1
[0084]
[0085] As shown in Table 1, the composite fabric prepared by the present invention has good wear resistance, and the weight loss rate in the wear test is low, all lower than 4%. Compared with Example 2, in Comparative Examples 1 and 2, the base material of the composite fabric has not changed, and is still linen yarn and nylon yarn, so the wear resistance has no obvious change.
[0086] (2) Antibacterial performance test: The test method refers to the standard GB / T20944.3-2008 "Evaluation of antibacterial properties of textiles Part 3: Oscillation method", and the antibacterial properties of the antibacterial and wear-resistant antistatic composite fabrics prepared in Examples 1-6 and Comparative Examples 1-2 after washing 40 times are compared. The test results are shown in Table 2:
[0087] Table 2
[0088]
[0089] As shown in Table 2, the composite fabric prepared by the present invention has good antibacterial properties. After washing 40 times, the antibacterial rates of Escherichia coli and Candida albicans can still reach 95%, and the antibacterial rate of Staphylococcus aureus can reach more than 90%. Lauramide reacts with epoxy-modified nano-titanium dioxide to form nano-titanium dioxide grafted lauroyl diethanolamine. The hydroxyl groups obtained by ring-opening the epoxy groups can form hydrogen bonds with the amide groups on the polyamide fiber molecules, thereby improving the bonding strength between nano-titanium dioxide and polyamide fibers, and thus improving the durability of the antibacterial properties of the composite fabric; quaternary ammonium salts are obtained by quaternizing nano-titanium dioxide grafted lauroyl diethanolamine, further improving the antibacterial properties of the antibacterial and antistatic finishing agent. Compared with Example 2, in Comparative Example 1, the nano-titanium dioxide grafted lauryl diethanolamine was not quaternized, and the antibacterial performance only depended on the nano-titanium dioxide. The antibacterial effect of the quaternary ammonium salt was lacking, and the antibacterial performance was greatly reduced; in Comparative Example 2, the nano-titanium dioxide did not react, the bonding strength between the nano-titanium dioxide and the polyamide fiber was reduced, and the antibacterial durability of the composite fabric was significantly reduced.
[0090] (3) Antistatic performance: The test method refers to the standard GB / T12703.2-2009 "Evaluation of electrostatic properties of textiles Part 2: Charge surface density". The test results are shown in Table 3:
[0091] Table 3
[0092]
[0093] As shown in Table 3, the composite fabric prepared by the present invention has good antistatic performance, and the charge surface density is as low as 1.2 μC / m 2. Nylon material easily generates negative charge due to friction. Lauramide reacts with epoxy-modified nano titanium dioxide to obtain non-ionic antistatic agent nano titanium dioxide grafted with lauryl diethanolamine. After the nano titanium dioxide grafted with lauryl diethanolamine undergoes quaternization reaction, the non-ionic antistatic agent is converted into a cationic antistatic agent with a positive charge, which can neutralize the negative charge on the surface of the nylon material fabric, thereby increasing the antistatic effect. Compared with Example 2, in Comparative Example 1, the non-ionic antistatic agent nano titanium dioxide grafted with lauryl diethanolamine is not converted into a cationic antistatic agent through quaternization reaction, and the antistatic effect is reduced. In Comparative Example 2, the antistatic agent is a non-ionic antistatic agent lauryl diethanolamine, and the antistatic performance is also reduced.
[0094] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.
Claims
1. A method for preparing an antibacterial, wear-resistant and antistatic composite fabric, characterized in that: The following steps are involved: Step 1, adding nano titanium dioxide and γ-glycidyloxypropyltrimethoxysilane to an ethanol aqueous solution, reacting, filtering, and drying after the reaction to obtain epoxy-modified nano titanium dioxide; Step 2, adding lauramide and epoxy-modified nano titanium dioxide into ethanol, adding triethylamine at a pH value of 9.5-10.5, reacting, filtering, washing, and drying after the reaction to obtain nano titanium dioxide grafted with lauroyl diethanolamide; The mass ratio of lauramide, epoxy-modified nano-titanium dioxide and ethanol is 200:(630-660):(3000-5000), and the reaction conditions are 75-85°C for 3-5h; Step 3, adding nano titanium dioxide grafted with lauroyl diethanolamine and dimethyl sulfate to isopropanol for reaction, and then rotary evaporating to obtain an antibacterial and antistatic finishing agent; The mass ratio of nano-titanium dioxide grafted with lauroyl diethanolamine, dimethyl sulfate and isopropanol is 850:(130-150):(1000-1500), and the reaction conditions are 80-90°C for 2.5-3.5h; Step 4, adding the antibacterial and antistatic finishing agent into deionized water, and ultrasonically dispersing the mixture to obtain an antibacterial and antistatic finishing liquid; The linen yarn and the nylon yarn are twisted and plied to obtain a composite yarn, and the composite yarn is used as a warp yarn and a weft yarn respectively to manufacture a composite fabric base cloth, and the composite fabric base cloth is immersed in an antibacterial and antistatic finishing liquid, double immersed and double rolled, and dried to obtain an antibacterial and wear-resistant antistatic composite fabric.
2. The method for preparing an antibacterial, wear-resistant and antistatic composite fabric according to claim 1, characterized in that: In the step 1, the mass ratio of nano-titanium dioxide, γ-glycidyloxypropyltrimethoxysilane and ethanol aqueous solution is 80:(250-270):(1500-2000), and the reaction conditions are 70-80° C. for 4-5 hours.
3. The method for preparing an antibacterial, wear-resistant and antistatic composite fabric according to claim 2, characterized in that: The ethanol aqueous solution includes 90wt%-95wt% ethanol aqueous solution.
4. The method for preparing an antibacterial, wear-resistant and antistatic composite fabric according to claim 1, characterized in that: In the step 4: the mass ratio of the antibacterial and antistatic finishing agent to deionized water is (1-10):(90-99).
5. The method for preparing an antibacterial, wear-resistant and antistatic composite fabric according to claim 1, characterized in that: In the step 4, the frequency of ultrasonic dispersion is 20-40 KHz, and the time of ultrasonic dispersion is 10-20 min.
6. The method for preparing an antibacterial, wear-resistant and antistatic composite fabric according to claim 1, characterized in that: In the step 4, the ratio of the number of linen yarns to the number of nylon yarns is (2-4):(10-20), and the density of the composite fabric base cloth is that the total number of warp yarns and weft yarns per square inch of the fabric is not less than 200.
7. The method for preparing an antibacterial, wear-resistant and antistatic composite fabric according to claim 1, characterized in that: In the step 4, the bath ratio of the immersion treatment is 1:(20-30), the immersion temperature is 50-60° C., and the immersion time is 20-30 min.
8. An antibacterial, wear-resistant and antistatic composite fabric prepared by the method for preparing an antibacterial, wear-resistant and antistatic composite fabric as claimed in any one of claims 1 to 7.