A garnet-type solid electrolyte with glass grain boundaries and a preparation method thereof

By adding the second glass phase lithium chloride at the grain boundary of Ga-LLZO solid electrolyte to form composite metal oxide particles, the problems of lithium dendrite growth and high electronic conductivity in lithium-ion batteries are solved, and efficient lithium Ionic conductivity and low electronic conductivity simplify the process and improve battery safety and energy density.

CN116683020BActive Publication Date: 2024-10-18CHINA HUBEI LONGZHONG LABORATORY +1
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202310815030.7
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-07-05
Publication Date
2024-10-18
Estimated Expiration
2043-07-05

AI Technical Summary

Technical Problem

The grains of the Ga-LLZO solid electrolyte in lithium-ion batteries grow abnormally during the high-temperature sintering process, resulting in the growth of lithium dendrites. The electronic conductivity is high and difficult to effectively suppress. The existing methods have limited effects and complicated processes.

Method used

Using a garnet-type solid electrolyte with glass grain boundaries, a second glass phase lithium chloride with nanometer or submicron thickness is added to the grain boundaries of LLZO grains to form composite metal oxide particles, blocking electron migration and inhibiting lithium Dendrite growth increases lithium ion conductivity.

Benefits of technology

A solid electrolyte with low electronic conductivity and high lithium ion conductivity at room temperature has been realized. The uniform grain size is less than 10 μm, which effectively suppresses lithium dendrites, simplifies the preparation process, and improves the safety and energy density of the electrolyte.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116683020B_ABST
    Figure CN116683020B_ABST
Patent Text Reader

Abstract

The invention discloses a garnet-type solid electrolyte with glass grain boundaries and a preparation method thereof. The solid electrolyte comprises a test block composed of composite metal oxide particles and a coating layer coated on the surface of the test block composed of composite metal oxide particles, wherein the coating layer is a first glass phase lithium chloride, the test block composed of composite metal oxide particles comprises a second glass phase lithium chloride and garnet-type LLZO grains co-doped with Ga and Cl, the second glass phase lithium chloride exists at the grain boundaries of the garnet-type LLZO grains with a thickness of nanometer or submicron level, the garnet-type LLZO comprises Li, La, Zr, O, Ga and Cl, the doped Ga replaces a Li site, the doped Cl replaces an O site, and the doped Cl replaces an O site, the room temperature electronic conductivity is low and the lithium ion conductivity is high.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of solid electrolytes, and in particular to a garnet-type solid electrolyte with glass grain boundaries and a preparation method thereof. Background Art

[0002] Lithium-ion batteries are widely used due to their high energy density, low self-discharge, and long cycle life. However, due to the flammability of the liquid electrolytes they use, limited pressure window, and poor compatibility with high-capacity electrode materials, lithium-ion batteries are difficult to meet the needs of the development of new lithium batteries with high safety and higher energy density.

[0003] In contrast, all-solid-state lithium batteries use solid electrolytes instead of organic electrolytes, which is expected to fundamentally solve the safety risks of lithium-ion batteries, further improve energy density, and simplify battery assembly. Among the many solid lithium-ion electrolytes, gallium-doped Li with a garnet structure is the most popular. 7-3x Ga x La3Zr2O 12 (Ga-LLZO) has a high room temperature ionic conductivity (>10 -3 S / cm), a wide electrochemical window (≥5 V / Li), and stable contact with metallic lithium make Ga-LLZO one of the most promising solid electrolytes. However, Ga-LLZO has a high grain size (grain size >100 μm) and high electronic conductivity (10 -8 ~10 -7 S / cm) leading to the growth of lithium dendrites.

[0004] In related technologies, researchers have made many attempts to improve the ability of Ga-LLZO to suppress lithium dendrites. For example, LiPON is deposited on the surface of LLZO to reduce the electron transmission capacity; the sintering process is adjusted to solve the abnormal growth of Ga-LLZO grains; however, the above methods have limited inhibitory effects on lithium dendrites, and the sintering process is relatively complicated. At the same time, after electrons pass through the modified interface, they may still combine with lithium ions inside LLZO to form lithium dendrites. The electronic conductivity of the modified solid electrolyte is still relatively high. Summary of the invention

[0005] In view of this, the present application provides a garnet-type solid electrolyte with glass grain boundaries and a preparation method thereof, which has low room temperature electronic conductivity and high lithium ion conductivity.

[0006] In order to achieve the above technical objectives, this application adopts the following technical solutions:

[0007] In a first aspect, the present application provides a garnet-type solid electrolyte with glass grain boundaries, comprising a test block composed of composite metal oxide particles and a coating layer coated on the surface of the test block composed of the composite metal oxide particles, wherein the coating layer is a first glass phase lithium chloride, and the test block composed of the composite metal oxide particles comprises a second glass phase lithium chloride and Ga and Cl co-doped garnet-type LLZO grains, wherein the second glass phase lithium chloride exists at the grain boundaries of the garnet-type LLZO grains with a thickness of nanometers or submicrometers, and the garnet-type LLZO comprises Li, La, Zr, O, Ga and Cl, and the doped Ga replaces the Li site, and the doped Cl replaces the O site.

[0008] Preferably, the chemical formula of LLZO is Li 7-3x-y Ga x La3Zr2O 12-y Cl y , wherein the chemical formula of the LLZO is Li 7-3x-y Ga x La3Zr2O 12-y Cl y , where 0.1≤x≤0.5, 0<y<the amount of Cl added.

[0009] Preferably, the amount of lithium chloride in the second glass phase is greater than the amount of lithium chloride in the first glass phase.

[0010] Preferably, the particle size of the garnet-type solid electrolyte having glass grain boundaries is 1-10 μm.

[0011] In a second aspect, the present application provides a method for preparing a garnet-type solid electrolyte having a glass grain boundary, comprising the following steps:

[0012] S1. A lithium source, a lanthanum source, a zirconium source, a gallium source and a chlorine source are used as raw materials, ball milled and dried to obtain a mixed material;

[0013] S2. The mixture was pre-fired to obtain an initial phase, the initial phase was ball-milled and dried to obtain a pre-fired powder;

[0014] S3. The pre-calcined powder was pressed into a sheet to obtain a sample;

[0015] S4. The sample is sintered to obtain a garnet-type solid electrolyte with glass grain boundaries.

[0016] Preferably, the chlorine source is lithium chloride.

[0017] Preferably, the mass of lithium chloride is 0.5-3% of the sum of the mass of the lithium source, the lanthanum source, the zirconium source and the gallium source.

[0018] Preferably, the lithium source is one or more of lithium oxide, carbonate, nitrate, and hydroxide; the lanthanum source is one or more of lanthanum oxide, carbonate, nitrate, and hydroxide; the zirconium source is one or more of zirconium oxide, carbonate, nitrate, and hydroxide; and the gallium source is one or more of gallium oxide, carbonate, nitrate, and hydroxide.

[0019] Preferably, the pre-firing temperature is 700-1100° C., and the pre-firing time is 1-12 hours.

[0020] Preferably, the sintering temperature is 1100-1200° C., and the sintering time is 8-20 h.

[0021] Preferably, the pressure for tableting is 50-500 MPa, and the tableting method is one or more of uniaxial pressing and cold isostatic pressing.

[0022] The beneficial effects of this application are as follows:

[0023] The garnet-type solid electrolyte with glass grain boundaries of the present application has both high room temperature ionic conductivity and low electronic conductivity;

[0024] The garnet-type solid electrolyte with glass grain boundaries of the present application has a uniform grain size of less than 10 μm, and the excess lithium chloride can exist in the glass phase at the grain boundaries to form a second glass phase lithium chloride to refine the LLZO grains and block electron migration, inhibit abnormal grain growth and electron transport, and improve the lithium dendrite inhibition ability;

[0025] The second glass phase lithium chloride grain boundary thickness of the garnet-type solid electrolyte with glass grain boundaries of the present application is small (nanometer or submicron level, less than 1 μm) and evenly distributed. The reason for the even distribution is that, compared with other grain boundary modification materials, lithium chloride has a low melting point and can exist in an amorphous form at the grain boundary of the garnet-type LLZO grains, so that the second glass phase lithium chloride covers each garnet-type LLZO grain to form composite metal oxide particles, rather than local aggregation, so that the finally obtained solid electrolyte can evenly transmit ions and block electrons, thereby achieving a better inhibition effect on lithium dendrites;

[0026] The preparation method of the present application is simple. Compared with the direct mixing of LLZO material and LiCl, the Cl in the present application is added in the form of doping to form a first glass phase lithium chloride and a second glass phase lithium chloride, which inhibits electron transport without affecting ion transport. BRIEF DESCRIPTION OF THE DRAWINGS

[0027] Figure 1 X-ray diffraction patterns of garnet-type solid electrolytes with glass grain boundaries prepared in Examples 1 and 4 of the present invention;

[0028] Figure 2 This is a SEM image of a garnet-type solid electrolyte having a glass grain boundary prepared in Example 1 of the present invention ( Figure 2 (a)) and its comparison with the unmodified sample SEM ( Figure 2 (c));

[0029] Figure 3 This is an EDS spectrum of the garnet-type solid electrolyte with glass grain boundaries prepared in Example 1 of the present invention;

[0030] Figure 4 The AC impedance curve of the garnet-type solid electrolyte with glass grain boundaries prepared in Example 1 of the present invention at room temperature ( Figure 2 (a) 、Activation energy ( Figure 2 (b)) and electronic conductivity ( Figure 2 (c));

[0031] Figure 5 The X-ray photoelectron spectrum of the garnet-type solid electrolyte with glass grain boundaries prepared in Example 1 of the present invention; wherein Figure 5 (a) is the Li 1s spectrum, Figure 5 (b) C 1s spectrum, Figure 5 (c) Zr 3d spectrum, Figure 5 (d) Cl 2p spectrum. DETAILED DESCRIPTION

[0032] In order to make the purpose, technical solution and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with the embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not used to limit the present invention.

[0033] The present application provides a garnet-type solid electrolyte with glass grain boundaries, comprising a test block composed of composite metal oxide particles and a coating layer coated on the surface of the test block composed of the composite metal oxide particles, wherein the coating layer is a first glass phase lithium chloride, and the test block composed of the composite metal oxide particles comprises a second glass phase lithium chloride and Ga and Cl co-doped garnet-type LLZO grains, wherein the second glass phase lithium chloride exists at the grain boundaries of the garnet-type LLZO grains with a thickness of nanometers or submicrometers, and the garnet-type LLZO comprises Li, La, Zr, O, Ga and Cl, and the doped Ga replaces the Li site, and the doped Cl replaces the O site.

[0034] On the one hand, Cl doping into LLZO oxygen sites can improve the lithium ion conductivity of LLZO. On the other hand, slightly excess lithium chloride can form a second glass phase. Lithium chloride exists at the grain boundaries to refine LLZO grains and block electron migration, which plays a better role in inhibiting lithium dendrites. The chemical formula of LLZO can be expressed as Li 7-3x-y Gax La3Zr2O 12-y Cl y , 0.1≤x≤0.5, 0<y<the amount of Cl added. Here, for every Cl added, there is one less negative valence and one less positive valence Li, that is, Ga replaces a part of the Li site and Cl replaces a part of the O site. The specific values ​​of x and y depend on the changes in the raw materials.

[0035] In this embodiment, the amount of lithium chloride in the second glass phase is greater than the amount of lithium chloride in the first glass phase.

[0036] The particle size of the garnet-type solid electrolyte having glass grain boundaries is 1-10 μm.

[0037] The present application provides a method for preparing a garnet-type solid electrolyte having a glass grain boundary, comprising the following steps:

[0038] S1. A lithium source, a lanthanum source, a zirconium source, a gallium source and a chlorine source are used as raw materials, ball milled and dried to obtain a mixed material;

[0039] S2. The mixture was pre-fired to obtain an initial phase, the initial phase was ball-milled and dried to obtain a pre-fired powder;

[0040] S3. The pre-calcined powder was pressed into a sheet to obtain a sample;

[0041] S4. The sample is sintered to obtain a garnet-type solid electrolyte with glass grain boundaries.

[0042] This scheme uses excess LiCl as a raw material for preparing LLZO, so that Cl is doped into the oxygen sites of the LLZO lattice to increase the conductivity (1.2*10 -3 S / cm), and a slightly excessive amount of LiCl exists at the grain boundaries to form a second glass phase lithium chloride, which reduces the electronic conductivity of the solid electrolyte; during the sintering process, the first glass phase lithium chloride and the second glass phase lithium chloride are formed at the same time, shortening the process flow.

[0043] In this scheme, LiCl is used to replace part of other lithium sources to directly prepare LLZO in one step. The chemical ratio satisfies the corresponding chemical formula and Cl is doped into the oxygen position of LLZO at high temperature (doped during pre-sintering). At the same time, slightly excess LiCl exists at the grain boundary to form a second glass phase lithium chloride. Cl doped into the oxygen position of LLZO can improve lithium ion conduction, and the second glass phase lithium chloride exists at the LLZO grain boundary so as not to affect lithium ion conduction and reduce electronic conduction, so the performance is excellent. Through the sintering and pressing process, excess LiCl can form the first glass phase lithium chloride on the surface of the composite metal oxide particle composition test block, so that the composite metal oxide particles containing LLZO can be completely coated without the need for such cumbersome processes as ball milling and recombining with LiCl. On the other hand, although Ga doping improves the conductivity, it will cause abnormal grain growth and the electronic conductivity is also relatively high. Therefore, this scheme adds Cl on the basis of Ga-doped LLZO.

[0044] In this scheme, the chlorine source is lithium chloride. By adding excess lithium chloride to replace other lithium sources for sintering, Ga-Cl co-doped LLZO (composite metal oxide particles) with lithium chloride glass (second glass phase lithium chloride) grain boundaries can be directly obtained; on the one hand, Cl doped into LLZO oxygen sites can improve the lithium ion conductivity of LLZO, and on the other hand, the second glass phase lithium chloride exists at the grain boundaries to refine the LLZO grains and block electron migration, thereby playing a better inhibitory effect on lithium dendrites.

[0045] The lithium source is one or more of lithium oxide, carbonate, nitrate, and hydroxide; the lanthanum source is one or more of lanthanum oxide, carbonate, nitrate, and hydroxide; the zirconium source is one or more of zirconium oxide, carbonate, nitrate, and hydroxide; the gallium source is one or more of gallium oxide, carbonate, nitrate, and hydroxide.

[0046] The mass of lithium chloride is 0.5-3% of the sum of the masses of lithium source, lanthanum source, zirconium source and gallium source. Below this range, Cl may be completely incorporated into the crystal lattice, and no excess LiCl exists at the grain boundary, that is, the second glass phase lithium chloride cannot be formed. Above this range, too much LiCl exists at the grain boundary, which will affect the performance.

[0047] The pre-firing temperature is 700-1100°C and the pre-firing time is 1-12h.

[0048] The sintering temperature is 1100-1200℃, and the sintering time is 8-20h. It is difficult to densify below 1000℃ and the performance is poor. Above 1200℃, LLZO may melt.

[0049] The pressure for pressing into tablets is 50-500MPa, and the method for pressing into tablets is one or more of uniaxial pressing and cold isostatic pressing. Through the sintering process, the lithium chloride in the raw material forms the first glass phase lithium chloride and the second glass phase lithium chloride in one step.

[0050] The present solution is further described below through specific embodiments.

[0051] Example 1

[0052] A garnet-type solid electrolyte with glass grain boundaries, the preparation method of which is as follows:

[0053] According to Li 6.4 Ga 0.2 La3Zr2O 12 Weigh lithium carbonate Li2CO3, lanthanum oxide La2O3, zirconium oxide ZrO2 and gallium oxide Ga2O3 powders in stoichiometric ratio (add 10 wt.% of excess lithium source to make up for lithium loss during high-temperature sintering), and add 0.5 wt.% of lithium chloride, which accounts for the sum of the mass of lithium source, lanthanum source, zirconium source and gallium source, and mix them evenly to obtain a mixed powder. The total mass is about 10g. The mixed powder is placed in a ball mill, and 30g (300% by mass) of isopropanol and an appropriate amount of zirconium oxide balls are added for ball milling. The ball mill speed is 300 rpm and the ball milling time is 12 hours. After the ball milling is completed, the mixed material is placed in a drying oven and dried at 80°C for 8 hours. Then pre-sinter at 900℃ for 6 hours, then ball-mill dry, weigh 3.0g of the dried mixture and put it into a mortar, add 0.3g (10%) of 10% PVA aqueous solution, grind for 30 minutes, then put the mixture into a steel mold, and keep the pressure at 300MPa for 5 minutes to obtain a green body. The green body is heated to 1200℃ at a heating rate of 5℃ / min, kept at this temperature for 12 hours, and then cooled with the furnace to obtain a garnet-type solid electrolyte with lithium chloride grain boundaries.

[0054] The novel garnet-type solid electrolyte Li prepared in Example 1 6.4 Ga 0.2 La3Zr2O 12 The X-ray diffraction patterns of the -0.5wt.%LiCl samples are as follows Figure 1 As shown in the LGLZO-0.5wt.%LiCl identification curve. Figure 1 It can be seen that the X-ray diffraction peak of the new garnet-type solid electrolyte matches well with the PDF card (45-0109) of the cubic phase LLZO, indicating that the LiCl in this example will not affect the physical phase of LLZO, which is still cubic phase LLZO.

[0055] SEM images of garnet-type solid electrolyte samples are shown in Figure 2 Compared with the unmodified solid electrolyte grains ( Figure 2 c) abnormal growth, compared with the grain size of the new solid electrolyte ( Figure 2 (a) The grains are uniform in size, less than 5 μm, and have a dense microstructure. At the same time, the surface of the grains is covered with a layer of amorphous material.

[0056] SEM and EDS spectrum images of garnet solid electrolyte samples are shown in Figure 3 As shown. Figure 3 It can be seen that the fracture mode of the solid electrolyte obtained by sintering is intercrystalline fracture, and the LLZO grains are coated with a layer of nano- or submicron-level second glass phase lithium chloride. At the same time, Ga, Cl, La, Zr, and O elements are evenly distributed without local enrichment, indicating that no second phase is formed.

[0057] X-ray photoelectron spectroscopy images of garnet-type solid electrolyte samples are shown in Figure 2. Figure 5 The presence of LiCl can be seen from the peak separation results of the Li 1S spectrum, and the Zr-Cl bond appearing in Zr 3d indicates that a portion of Cl is doped into the oxygen position in the LLZO lattice.

[0058] Example 2

[0059] A garnet-type solid electrolyte with glass grain boundaries, the other contents of which are the same as those of Example 1, except that 1 wt.% of lithium chloride LiCl, which accounts for the total mass of a lithium source, a lanthanum source, a zirconium source and a gallium source, is added and mixed uniformly to obtain a mixed powder.

[0060] Example 3

[0061] A garnet-type solid electrolyte with glass grain boundaries, the other contents of which are the same as those of Example 1, except that 2 wt.% of lithium chloride LiCl, which accounts for the total mass of a lithium source, a lanthanum source, a zirconium source and a gallium source, is added and mixed evenly to obtain a mixed powder.

[0062] Example 4

[0063] A garnet-type solid electrolyte with glass grain boundaries, the other contents are the same as those of Example 1, except that 3 wt.% of lithium chloride LiCl, which accounts for the sum of the weight of the lithium source, the lanthanum source, the zirconium source and the gallium source, is added and mixed evenly to obtain a mixed powder.

[0064] Garnet-type solid electrolyte Li 6.4 Ga 0.2 La3Zr2O 12 The X-ray diffraction patterns of the -3wt.% LiCl samples are shown in Figure 1 As shown in the LGLZO-3 wt.%LiCl identification curve. Figure 1It can be seen that the X-ray diffraction peak of the new garnet-type solid electrolyte matches well with the PDF card (45-0109) of the cubic phase LLZO, indicating that the LiCl in this example will not affect the physical phase of LLZO, which is still cubic phase LLZO.

[0065] Example 5

[0066] A garnet-type solid electrolyte with glass grain boundaries, other contents are the same as those of Example 1, except that the sintering temperature is 1100°C.

[0067] Example 6

[0068] A garnet-type solid electrolyte with glass grain boundaries, the other contents of which are the same as those of Example 1, except that the electrolyte is kept at 1200° C. for 20 hours.

[0069] Comparative Example 1 (without Cl doping)

[0070] A garnet-type solid electrolyte, the other contents are the same as those of Example 1, except that LiCl is not included in the raw materials, so no glass phase exists at the grain boundaries and Cl is not doped into LLZO.

[0071] Comparative Example 2 (not doped with Ga)

[0072] A garnet-type solid electrolyte with glass grain boundaries, the other contents of which are the same as those of Example 1, except that Ga2O3 is not included in the raw materials.

[0073] Comparative Example 3 (no Cl doping, no Ga doping)

[0074] A garnet-type solid electrolyte, the other contents are the same as those of Example 1, except that the raw materials do not include LiCl and Ga2O3, so no glass phase exists at the grain boundaries.

[0075] Comparative Example 4 (small amount of Cl doping and no LiCl grain boundary)

[0076] A garnet-type solid electrolyte, the other contents are the same as those of Example 1, except that 0.2 wt.% of lithium chloride LiCl is added based on the total mass of the lithium source, the lanthanum source, the zirconium source and the gallium source, and there is no second glass phase lithium chloride.

[0077] Comparative Example 5 (High Amount of Cl)

[0078] A garnet-type solid electrolyte with glass grain boundaries, the other contents of which are the same as those of Example 1, except that 5 wt.% of lithium chloride LiCl is added, which accounts for the total mass of the lithium source, the lanthanum source, the zirconium source and the gallium source.

[0079] Evaluation Test

[0080] The novel garnet-type solid electrolyte prepared in Example 1 was subjected to AC impedance tests at different temperatures and DC polarization tests at room temperature using an electrochemical workstation. The test results are as follows: Figure 4 According to the test results, the ionic conductivity of the new garnet solid electrolyte sample prepared in Example 1 can reach 1.25×10 -3 S / cm, the activation energy is 0.20 eV, and the electronic conductivity is only 1.90×10 -9 S / cm. Compared with the Ga-doped LLZO garnet-type solid electrolyte comparative example 1 without LiCl modification (1×10 -3 S / cm), the ionic conductivity has been improved, reflecting that the incorporation of Cl into the LLZO lattice can promote the lithium ion conductivity, and the amount of LiCl existing in the grain boundary is very small, which will not affect the overall lithium ion transport (LiCl ion conductivity: 1×10 -9 S / cm). Compared with Comparative Example 4 without the second glassy phase lithium chloride, the room temperature ionic conductivity of the novel garnet-type solid electrolyte prepared in Example 1 is comparable, but the electronic conductivity is significantly reduced (only 19.5%), reflecting that the second glassy phase lithium chloride present at the grain boundary has a blocking effect on electron migration.

[0081] Table 1 Test results

[0082]

[0083] From the above, it can be seen that the garnet-type solid electrolyte with glass grain boundaries of the present application has both high room temperature ionic conductivity and low electronic conductivity.

[0084] The above are only preferred specific implementations of the present invention, but the protection scope of the present invention is not limited thereto. Any changes or substitutions that can be easily conceived by any technician familiar with the technical field within the technical scope disclosed by the present invention should be covered within the protection scope of the present invention.

Claims

1. A garnet-type solid electrolyte having glass grain boundaries, characterized in that: The invention comprises a test block composed of composite metal oxide particles and a coating layer coated on the surface of the test block composed of composite metal oxide particles, wherein the coating layer is a first glass phase lithium chloride, and the test block composed of composite metal oxide particles comprises a second glass phase lithium chloride and garnet-type LLZO grains co-doped with Ga and Cl, wherein the second glass phase lithium chloride exists at the grain boundaries of the garnet-type LLZO grains with a thickness of nanometer or submicron level, and the garnet-type LLZO comprises Li, La, Zr, O, Ga and Cl, and the doped Ga replaces the Li site, and the doped Cl replaces the O site.

2. The garnet-type solid electrolyte having glass grain boundaries according to claim 1, characterized in that: The amount of the second glassy phase lithium chloride is greater than the amount of the first glassy phase lithium chloride.

3. The garnet-type solid electrolyte having glass grain boundaries according to claim 1, characterized in that: The particle size of the garnet-type solid electrolyte with glass grain boundaries is 1-10 μm.

4. A method for preparing a garnet-type solid electrolyte having a glass grain boundary as claimed in any one of claims 1 to 3, characterized in that: The following steps are involved: S1. A lithium source, a lanthanum source, a zirconium source, a gallium source and a chlorine source are used as raw materials, ball milled and dried to obtain a mixed material; S2. The mixture was pre-calcined to obtain an initial phase, the initial phase was ball-milled and dried to obtain a pre-calcined powder; S3. The pre-burned powder was pressed into a sheet to obtain a sample; S4. The sample is sintered to obtain the garnet-type solid electrolyte with glass grain boundaries; the chlorine source is lithium chloride; the mass of the lithium chloride is 0.5-3% of the sum of the masses of the lithium source, lanthanum source, zirconium source and gallium source; the sintering temperature is 1100-1200°C, and the sintering time is 8-20h; the mass of the lithium source is at least 10% of the sum of the masses of the lithium source, lanthanum source, zirconium source and gallium source.

5. The method for preparing a garnet-type solid electrolyte having a glass grain boundary according to claim 4, characterized in that: The lithium source is one or more of lithium oxide, carbonate, nitrate, and hydroxide; the lanthanum source is one or more of lanthanum oxide, carbonate, nitrate, and hydroxide; the zirconium source is one or more of zirconium oxide, carbonate, nitrate, and hydroxide; the gallium source is one or more of gallium oxide, carbonate, nitrate, and hydroxide.

6. The method for preparing a garnet-type solid electrolyte having a glass grain boundary according to claim 4, characterized in that: The pre-firing temperature is 700-1100° C., and the pre-firing time is 1-12 hours.

7. The method for preparing a garnet-type solid electrolyte having a glass grain boundary according to claim 4, characterized in that: The pressure for pressing into tablets is 50-500 MPa, and the method for pressing into tablets is one or more of uniaxial pressing and cold isostatic pressing.

Citation Information

Patent Citations

  • Preparation method of LLZO powder

    CN108417889A

  • Nb and Ta co-doped garnet-type LLZO solid electrolyte and preparation method thereof

    CN109935901A