A precursor of iron manganese oxalate, its preparation method, and lithium or sodium-ion battery cathode materials prepared therefrom.
By designing a gradient distribution structure for the iron-manganese oxalate precursor, the problem of manganese leaching in lithium-ion and sodium-ion battery cathode materials was solved, thereby improving the stability and cycle performance of the material.
Patent Information
- Application Number
- CN202310581537.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-05-23
- Publication Date
- 2026-11-10
- Estimated Expiration
- 2043-05-23
AI Technical Summary
The dissolution of manganese in the cathode materials of lithium-ion and sodium-ion batteries leads to a decrease in material stability and cycle performance. In particular, it causes lattice distortion and manganese ion dissolution during charge and discharge, affecting the cycle performance and rate performance of the battery.
A special structural design is adopted for the iron-manganese oxalate precursor, with MnC2O4 as the core, FeaMnbC2O4 as the first transition layer, FecMndC2O4 as the second transition layer, and FeC2O4 as the shell. By controlling the atomic ratio gradient distribution of Fe and Mn, the dissolution of manganese is suppressed and the stability of the material is improved.
It effectively suppresses the reaction between electrode materials and electrolyte, reduces capacity decay, and improves the stability and cycle performance of cathode materials for lithium or sodium-ion batteries.
Smart Images

Figure CN116730309B_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of new energy technology, specifically to an iron-manganese oxalate precursor with a gradient distribution of iron and manganese element concentration, its preparation method, and the cathode material for lithium or sodium-ion batteries obtained by using it. Background Technology
[0002] With social development and continuous progress, the depletion of non-renewable fossil fuels and energy shortages have become a serious problem facing humanity. Lithium-ion batteries, as one of the most advanced energy conversion and storage technologies, have attracted widespread attention due to their high energy density and relatively simple reaction mechanism. Currently, commercially produced lithium-ion battery cathode materials mainly include layered LiCoO2, spinel-structured LiMn2O4, and olivine-structured LiFePO4 cathode materials. However, certain issues remain regarding cycle performance and safety when used in large-scale, high-energy systems such as hybrid electric vehicles or electric vehicles. Furthermore, sodium-ion batteries have received considerable attention in recent years due to the abundance of sodium sources on Earth. However, the larger radius of sodium ions compared to lithium ions results in slower diffusion kinetics and more unstable insertion / extraction / deintercalation. Therefore, further research on lithium-ion and sodium-ion battery materials is essential.
[0003] Among them, lithium iron phosphate (LFP) cathode materials with olivine structures for lithium-ion batteries have become a research hotspot in the field of electrode materials. Lithium manganese iron phosphate (LFP) is based on LFP, doped with a certain amount of manganese and its atomic ratio to iron (manganese-iron ratio) to improve the voltage plateau of the material. Under comparable conditions, its theoretical energy density is 15%-20% higher than that of LFP, and it is considered an upgraded version of LFP. However, due to the existence of the Jan Taylor effect, Mn... 3+ Enriched on the surface of cathode particles, MnO6 octahedrons are distorted, leading to lattice distortion and reduced structural stability, thus affecting stability and cycle performance. Similar situations exist in sodium iron manganese pyrophosphate and sodium iron manganese oxide in sodium-ion batteries. 3+ During the charging and discharging process of the battery, the Jan Taylor effect occurs, which leads to lattice distortion and structural damage. This is accompanied by the dissolution of manganese ions into the electrolyte, which seriously affects the battery's cycle performance and rate performance, causing the specific capacity to decay rapidly. Summary of the Invention
[0004] To address the problem of deteriorated stability and cycle life of cathode materials due to manganese leaching, this invention aims to provide a manganese iron oxalate precursor, its preparation method, and lithium or sodium-ion battery cathode materials prepared using the precursor. These materials effectively suppress the reaction between the electrode material and the electrolyte, inhibit manganese leaching, reduce capacity decay, and improve material stability.
[0005] To achieve the above-mentioned technical objectives, the present invention adopts the following technical solution:
[0006] A manganese iron oxalate precursor, with MnC2O4 as the core and Fe... a Mn b C2O4 forms the first transition layer, Fe c Mn d C2O4 is the second transition layer, and FeC2O4 is the shell. In this shell, a, b, c, and d cannot all be 0, a+b=1, c+d=1, a / b is a fixed value, and c / d increases from the inside to the outside.
[0007] Furthermore, in the iron manganese oxalate precursor, the total atomic ratio of Fe to Mn is 1:1.
[0008] Further, a / b = 0.5-2; even further, a / b = 1.
[0009] Furthermore, the iron manganese oxalate precursor is granular with a particle size of 5-10 micrometers.
[0010] The present invention also provides a method for preparing the above-mentioned iron manganese oxalate precursor, comprising the following steps:
[0011] (1) Soluble oxalate, soluble manganese salt and soluble ferrous salt are dissolved in water to obtain soluble oxalate solution A, soluble manganese salt solution B and soluble ferrous salt solution C, wherein an antioxidant is added to soluble ferrous salt solution C.
[0012] (2) Using soluble oxalate solution A as the base liquid, add part of soluble manganese salt solution B, and react to obtain a first solution containing MnC2O4 nuclei;
[0013] (3) Mix a portion of the soluble ferrous salt solution C and the remaining portion of the soluble manganese salt solution B to obtain an iron-manganese mixed solution D. Add a portion of the iron-manganese mixed solution D to the first solution to obtain Fe containing a fixed Fe / Mn ratio. a Mn b The second solution of the C2O4 transition layer;
[0014] (4) The remaining iron-manganese mixed solution D is continuously passed into the second solution, along with the remaining soluble ferrous salt solution C. The reaction yields Fe with a gradient increasing Fe / Mn ratio. c Mn d Iron manganese oxalate precursor with C2O4 transition layer and FeC2O4 shell.
[0015] Further, in step (1), the molar ratio of oxalate, manganese salt and ferrous salt in the soluble oxalate solution A, the soluble manganese salt solution B and the soluble ferrous salt solution C is 2.1-2.8:1:1; more preferably 2.2-2.4:1:1.
[0016] Further, in step (1), the soluble oxalate is one or more of oxalic acid, ammonium oxalate, and sodium oxalate; the soluble manganese salt is one or more of manganese sulfate, manganese nitrate, manganese chloride, and manganese citrate; the soluble ferrous salt is one or more of ferrous sulfate, ferrous chloride, and ferrous citrate; and the antioxidant is one or more of ascorbic acid, citric acid, and malic acid.
[0017] Furthermore, in step (2), a portion of the soluble manganese salt solution B accounts for 1 / 3 to 2 / 3 of the total amount of soluble manganese salt solution B.
[0018] Furthermore, in step (3), the soluble ferrous salt solution C accounts for 1 / 3 to 2 / 3 of the total soluble ferrous salt solution C; the ferrous manganese mixed solution D accounts for 1 / 2 of the total ferrous manganese mixed solution D.
[0019] In this invention, firstly, a portion of manganese salt solution is added to an oxalate solution to form a MnC₂O₄ core. Then, a mixed iron-manganese solution with a fixed Fe / Mn ratio is added to form Fe around the MnC₂O₄ core. a Mn b A C2O4 transition layer is then added, followed by the addition of the remaining ferrous salt solution while simultaneously adding the iron-manganese mixed solution, initially forming a Fe / Mn ratio with an increasing gradient. c Mn d A C2O4 transition layer is formed, and the flow rate is controlled so that the ferrous salt solution is dropped later than the iron-manganese mixed solution, ultimately resulting in a FeC2O4 shell, thus forming the MnC2O4 core and Fe... a Mn b C2O4 forms the first transition layer, Fe c Mn d C2O4 is the second transition layer, and FeC2O4 is a special structured iron manganese oxalate precursor.
[0020] This invention also provides a positive electrode material for lithium or sodium-ion batteries, obtained from the above-mentioned iron-manganese oxalate precursor, specifically as follows:
[0021] Option 1
[0022] The iron manganese oxalate precursor was mixed evenly with a phosphorus source and a lithium source, and then calcined to obtain lithium iron manganese phosphate, a lithium-ion cathode material.
[0023] Option 2
[0024] The iron manganese oxalate precursor was mixed evenly with a phosphorus source and a sodium source, and then calcined to obtain sodium iron manganese pyrophosphate, a sodium ion cathode material.
[0025] Option 3
[0026] The iron manganese oxalate precursor was mixed evenly with a sodium source and calcined to obtain sodium iron manganese oxide, a sodium ion cathode material.
[0027] Furthermore, the phosphorus source is one or more of phosphoric acid, diammonium hydrogen phosphate, and ammonium dihydrogen phosphate; the lithium source is one or more of lithium carbonate, lithium hydroxide, and lithium acetate; and the sodium source is one or more of sodium carbonate, sodium bicarbonate, and sodium acetate.
[0028] Furthermore, the calcination temperature of Scheme 1, Scheme 2 and Scheme 3 is 550-900℃ and the calcination time is 6-18 hours. The calcination atmosphere of Scheme 1 and Scheme 2 is a mixture of nitrogen, argon and helium with hydrogen, and the calcination atmosphere of Scheme 3 is air or oxygen.
[0029] A lithium-ion or sodium-ion battery comprising the aforementioned lithium-ion or sodium-ion battery cathode material.
[0030] The beneficial effects of this invention are as follows:
[0031] Using MnC2O4 as the core, Fe a Mn b C2O4 forms the first transition layer, Fe c Mn d The cathode material prepared from a special structured iron-manganese oxalate precursor with C2O4 as the second transition layer and FeC2O4 as the shell can effectively suppress the reaction between the electrode material and the electrolyte, inhibit the dissolution of manganese, reduce capacity decay, and improve the stability of the material. Attached Figure Description
[0032] Figure 1 The graphs show the charge-discharge curves of the lithium iron manganese phosphate cathode materials prepared in Example 1 and Comparative Examples 1-4.
[0033] Figure 2 The image shows the charge-discharge curves of the sodium iron manganese pyrophosphate cathode material prepared in Example 3.
[0034] Figure 3 The image shows the charge-discharge curves of the sodium iron manganese oxide cathode material prepared in Example 4. Detailed Implementation
[0035] The present invention will be further described below with reference to the embodiments, but these specific embodiments do not limit the scope of protection of the present invention in any way.
[0036] Example 1
[0037] 3.4106 g of ammonium oxalate was dissolved in 120 mL of distilled water to prepare solution A containing soluble oxalate ions. 1.6902 g of manganese sulfate monohydrate was dissolved in 50 mL of distilled water to prepare solution B containing soluble manganese salts. 0.5 g of ascorbic acid and 2.7801 g of ferrous sulfate heptahydrate were dissolved in 50 mL of distilled water to prepare solution C containing soluble iron salts. Using solution A as the base solution, solution B was first added to solution A, half the total volume of solution B, and stirred until homogeneous to allow the core particles to grow (MnC₂O₄). Then, solution C was added to the remaining solution B to obtain mixed solution D, half the total volume of solution C. Mixed solution D was then added to solution A, and stirred until homogeneous to allow the first transition layer to grow (Fe). 0.5 Mn 0.5 When the amount of C2O4 added is half the total amount of solution D, the mixture of solution D is continuously added dropwise, while the remaining solution C is added to solution A at a lower rate than that of solution D. The iron-manganese ratio continuously increases, and the mixture is stirred until homogeneous, allowing the second transition layer to grow (Fe2O4). c Mn d C2O4 (c / d increases from the inside to the outside); finally, mixed solution D is added dropwise first, followed by solution C, and stirred until homogeneous to allow the outermost shell to grow (FeC2O4). After aging, the final product obtained is MnC2O4 as the core and Fe... 0.5 Mn 0.5 C2O4 forms the first transition layer, Fe c Mn d C2O4 forms the second transition layer, and FeC2O4 is a specially structured iron-manganese oxalate precursor with a shell structure. The reaction temperature is controlled at 60℃ throughout the process, the reaction pH is 5, and the stirring speed is 500 rpm.
[0038] Weigh 0.957g of ammonium dihydrogen phosphate and mix with 2.536mL of oleic acid by ball milling for 1 hour. Then add 1.436g of iron manganese oxalate precursor and mix by ball milling for 30 minutes. Then add 0.3074g of lithium carbonate and mix by ball milling for 1 hour. Remove the mixture and dry it in an oven at 80℃. Heat the mixture to 650℃ at a rate of 3℃ / min and calcine it under argon / hydrogen (95 / 5) gas protection for 6 hours. The resulting powder is the lithium iron manganese phosphate cathode material.
[0039] Example 2
[0040] 3.0257 g of oxalic acid was dissolved in 240 mL of distilled water to prepare solution A containing soluble oxalate ions. 1.6902 g of manganese sulfate monohydrate was dissolved in 100 mL of distilled water to prepare solution B containing soluble manganese salts. 0.5 g of ascorbic acid and 2.7801 g of ferrous sulfate heptahydrate were dissolved in 100 mL of distilled water to prepare solution C containing soluble iron salts. Using solution A as the base solution, solution B was first added to solution A, one-third of the total volume of solution B, and stirred until homogeneous to allow the core particles to grow (MnC₂O₄). Then, solution C was added to the remaining solution B to obtain mixed solution D, one-third of the total volume of solution C. Mixed solution D was then added to solution A, and stirred until homogeneous to allow the first transition layer to grow (Fe). 1 / 3 Mn 2 / 3 When the amount of C2O4 added is half the total amount of solution D, the mixture of solution D is continuously added dropwise, while the remaining solution C is added to solution A at a lower rate than that of solution D. The iron-manganese ratio continuously increases, and the mixture is stirred until homogeneous, allowing the second transition layer to grow (Fe2O4). c Mn d C2O4 (c / d increases from the inside to the outside); finally, mixed solution D is added dropwise first, followed by solution C, and stirred until homogeneous to allow the outermost shell to grow (FeC2O4). After aging, the final product obtained is MnC2O4 as the core and Fe... 1 / 3 Mn 2 / 3 C2O4 forms the first transition layer, Fe c Mn d C2O4 forms the second transition layer, and FeC2O4 is a specially structured iron-manganese oxalate precursor with a shell structure. The reaction temperature is controlled at 80℃ throughout the process, the reaction pH is 3, and the stirring speed is 600 rpm.
[0041] Weigh 0.957g of ammonium dihydrogen phosphate and mix with 2.536mL of oleic acid by ball milling for 1 hour. Then add 1.436g of iron manganese oxalate precursor and mix by ball milling for 30 minutes. Then add 0.3074g of lithium carbonate and mix by ball milling for 1 hour. Remove the mixture and dry it in an oven at 100℃. Heat the mixture to 750℃ at a rate of 2℃ / min and calcine it under argon / hydrogen (95 / 5) gas protection for 8 hours. The resulting powder is the lithium iron manganese phosphate cathode material.
[0042] Example 3
[0043] 3.4106 g of ammonium oxalate was dissolved in 120 mL of distilled water to prepare solution A containing soluble oxalate ions. 1.6902 g of manganese sulfate monohydrate was dissolved in 100 mL of distilled water to prepare solution B containing soluble manganese salts. 0.5 g of ascorbic acid and 2.7801 g of ferrous sulfate heptahydrate were dissolved in 100 mL of distilled water to prepare solution C containing soluble iron salts. Using solution A as the base solution, solution B was first added to solution A, with the amount added being two-thirds of the total volume of solution B. The mixture was stirred until homogeneous to allow the core particles to grow (MnC₂O₄). Then, solution C was added to the remaining solution B to obtain mixed solution D, with the amount added being two-thirds of the total volume of solution C. Mixed solution D was then added to solution A, and the mixture was stirred until homogeneous to allow the first transition layer to grow (Fe). 2 / 3 Mn 1 / 3 When the amount of C2O4 added is half the total amount of solution D, the mixture of solution D is continuously added dropwise, while the remaining solution C is added to solution A at a lower rate than that of solution D. The iron-manganese ratio continuously increases, and the mixture is stirred until homogeneous, allowing the second transition layer to grow (Fe2O4). c Mn d C2O4 (c / d increases from the inside to the outside); finally, mixed solution D is added dropwise first, followed by solution C, and stirred until homogeneous to allow the outermost shell to grow (FeC2O4). After aging, the final product obtained is MnC2O4 as the core and Fe... 2 / 3 Mn 1 / 3 C2O4 forms the first transition layer, Fe c Mn d C2O4 forms the second transition layer, and FeC2O4 is a specially structured iron-manganese oxalate precursor with a shell structure. The reaction temperature is controlled at 40℃ throughout the process, the reaction pH is 5, and the stirring speed is 500 rpm.
[0044] Weigh 1.346g of iron manganese oxalate precursor, 1.1503g of ammonium dihydrogen phosphate and 0.5299g of anhydrous sodium carbonate, ball mill them together with 5mL of anhydrous ethanol for 3 hours, dry them in an 80℃ oven, heat them to 350℃ at a rate of 5℃ / min, calcine them for 3 hours under argon gas protection, grind them, heat them to 600℃ at a rate of 5℃ / min, and calcine them for 6 hours under argon gas protection. The resulting powder is the sodium iron manganese pyrophosphate cathode material.
[0045] Example 4
[0046] 3.4106 g of ammonium oxalate was dissolved in 120 mL of distilled water to prepare solution A containing soluble oxalate ions. 1.6902 g of manganese sulfate monohydrate was dissolved in 50 mL of distilled water to prepare solution B containing soluble manganese salts. 0.5 g of ascorbic acid and 2.7801 g of ferrous sulfate heptahydrate were dissolved in 50 mL of distilled water to prepare solution C containing soluble iron salts. Using solution A as the base solution, solution B was first added to solution A, half the total volume of solution B, and stirred until homogeneous to allow the core particles to grow (MnC₂O₄). Then, solution C was added to the remaining solution B to obtain mixed solution D, half the total volume of solution C. Mixed solution D was then added to solution A, and stirred until homogeneous to allow the first transition layer to grow (Fe). 0.5 Mn 0.5 When the amount of C2O4 added is half the total amount of solution D, the mixture of solution D is continuously added dropwise, while the remaining solution C is added to solution A at a lower rate than that of solution D. The iron-manganese ratio continuously increases, and the mixture is stirred until homogeneous, allowing the second transition layer to grow (Fe2O4). c Mn d C2O4 (c / d increases from the inside to the outside); finally, mixed solution D is added dropwise first, followed by solution C, and stirred until homogeneous to allow the outermost shell to grow (FeC2O4). After aging, the final product obtained is MnC2O4 as the core and Fe... a Mn b C2O4 forms the first transition layer, Fe c Mn d C2O4 forms the second transition layer, and FeC2O4 is a specially structured iron-manganese oxalate precursor with a shell structure. The reaction temperature is controlled at 60℃ throughout the process, the reaction pH is 5, and the stirring speed is 500 rpm.
[0047] Weigh 1.436g of iron manganese oxalate precursor and 0.2983g of anhydrous sodium carbonate, ball mill them together with 5mL of anhydrous ethanol for 5 hours, take them out and dry them in an 80℃ oven, heat them to 500℃ at a rate of 5℃ / min, calcine them in air for 6 hours, cool them to room temperature, take them out and grind them, then heat them to 900℃ at a rate of 5℃ / min and calcine them in air for 12 hours. The resulting powder is the sodium iron manganese oxide cathode material.
[0048] Comparative Example 1
[0049] 3.4106 g of ammonium oxalate was dissolved in 120 mL of distilled water to prepare solution A containing soluble oxalate ions. 0.5 g of ascorbic acid, 2.7801 g of ferrous sulfate heptahydrate, and 1.6902 g of manganese sulfate monohydrate were dissolved in 100 mL of distilled water to prepare solution B containing soluble iron and manganese salts. Using solution A as the base solution, solution B was added to solution A and stirred. The reaction temperature was controlled at 60℃, the reaction pH at 5, and the stirring speed at 500 rpm. After aging, Fe was obtained. 0.5 Mn0.5 C2O4·2H2O precursor.
[0050] Weigh 0.957g of ammonium dihydrogen phosphate and mix with 2.536mL of oleic acid by ball milling for 1 hour. Then add 1.436g of iron manganese oxalate precursor and mix by ball milling for 30 minutes. Then add 0.3074g of lithium carbonate and mix by ball milling for 1 hour. Remove the mixture and dry it in an oven at 80℃. Heat the mixture to 650℃ at a rate of 3℃ / min and calcine it under argon / hydrogen (95 / 5) gas protection for 6 hours. The resulting powder is the lithium iron manganese phosphate cathode material.
[0051] Comparative Example 2
[0052] 3.4106 g of ammonium oxalate was dissolved in 120 mL of distilled water to prepare solution A containing soluble oxalate ions. 1.6902 g of manganese sulfate monohydrate was dissolved in 50 mL of distilled water to prepare solution B containing soluble manganese salts. 0.5 g of ascorbic acid and 2.7801 g of ferrous sulfate heptahydrate were dissolved in 50 mL of distilled water to prepare solution C containing soluble iron salts. Using solution A as the base solution, solution B was first added to solution A, half the total volume of solution B, and stirred until homogeneous to allow the core particles to grow (MnC₂O₄). Then, solution C was added to the remaining solution B to obtain mixed solution D, half the total volume of solution C. Finally, all of mixed solution D was added to solution A, and stirred until homogeneous to allow the transition layer to grow (Fe). 0.5 Mn 0.5 C2O4), then the remaining solution C is added to solution A, stirred evenly to allow the shell to grow (FeC2O4), and after aging, the final product of this invention is obtained with MnC2O4 as the core and Fe... 0.5 Mn 0.5 C2O4 serves as the transition layer, while FeC2O4 forms the shell, creating a special structure for the iron-manganese oxalate precursor. The entire reaction process is controlled at 60℃, pH 5, and a stirring speed of 500 rpm.
[0053] Weigh 0.957g of ammonium dihydrogen phosphate and mix with 2.536mL of oleic acid by ball milling for 1 hour. Then add 1.436g of iron manganese oxalate precursor and mix by ball milling for 30 minutes. Then add 0.3074g of lithium carbonate and mix by ball milling for 1 hour. Remove the mixture and dry it in an oven at 80℃. Heat the mixture to 650℃ at a rate of 3℃ / min and calcine it under argon / hydrogen (95 / 5) gas protection for 6 hours. The resulting powder is the lithium iron manganese phosphate cathode material.
[0054] Comparative Example 3
[0055] 3.4106 g of ammonium oxalate was dissolved in 120 mL of distilled water to prepare solution A containing soluble oxalate ions. 1.6902 g of manganese sulfate monohydrate was dissolved in 50 mL of distilled water to prepare solution B containing soluble manganese salt. 0.5 g of ascorbic acid and 2.7801 g of ferrous sulfate heptahydrate were dissolved in 50 mL of distilled water to prepare solution C containing soluble iron salt. Using solution A as the base solution, solution B was first added to solution A and stirred until homogeneous to allow the core particles to grow (MnC₂O₄). Then, solution C was added dropwise and stirred until homogeneous to allow the shell layer to grow (FeC₂O₄). After aging, the iron-manganese oxalate precursor with the special structure of MnC₂O₄ core and FeC₂O₄ shell of this invention was finally obtained. The reaction temperature was controlled at 60℃, the reaction pH was 5, and the stirring speed was 500 rpm.
[0056] Weigh 0.957g of ammonium dihydrogen phosphate and mix with 2.536mL of oleic acid by ball milling for 1 hour. Then add 1.436g of iron manganese oxalate precursor and mix by ball milling for 30 minutes. Then add 0.3074g of lithium carbonate and mix by ball milling for 1 hour. Remove the mixture and dry it in an oven at 80℃. Heat the mixture to 650℃ at a rate of 3℃ / min and calcine it under argon / hydrogen (95 / 5) gas protection for 6 hours. The resulting powder is the lithium iron manganese phosphate cathode material.
[0057] Comparative Example 4
[0058] 3.4106 g of ammonium oxalate was dissolved in 120 mL of distilled water to prepare solution A containing soluble oxalate ions. 1.6902 g of manganese sulfate monohydrate was dissolved in 50 mL of distilled water to prepare solution B containing soluble manganese salt. 0.5 g of ascorbic acid and 2.7801 g of ferrous sulfate heptahydrate were dissolved in 50 mL of distilled water to prepare solution C containing soluble iron salt. Using solution A as the base solution, solutions B and C were simultaneously added to solution A. Solution B was added dropwise from fast to slow, and solution C was added dropwise from slow to fast, ensuring that solutions B and C were added simultaneously. The iron-manganese ratio increased with each layer. After stirring until homogeneous and aging, the iron-manganese gradient distribution of the iron-manganese oxalate precursor of this invention was finally obtained. The reaction temperature was controlled at 60℃, the reaction pH was 5, and the stirring speed was 500 rpm.
[0059] Weigh 0.957g of ammonium dihydrogen phosphate and mix with 2.536mL of oleic acid by ball milling for 1 hour. Then add 1.436g of iron manganese oxalate precursor and mix by ball milling for 30 minutes. Then add 0.3074g of lithium carbonate and mix by ball milling for 1 hour. Remove the mixture and dry it in an oven at 80℃. Heat the mixture to 650℃ at a rate of 3℃ / min and calcine it under argon / hydrogen (95 / 5) gas protection for 6 hours. The resulting powder is the lithium iron manganese phosphate cathode material.
[0060] Performance testing:
[0061] Weigh the active material (positive electrode), binder (PVDF), and conductive agent (SP) in a mass ratio of 7:2:1, grind and disperse them, and mix them evenly to maintain good fluidity of the slurry. Apply the slurry to a flat aluminum foil and dry it. Place the dried electrode in an 80℃ vacuum drying oven and let it stand. Finally, use a manual cutting machine to cut it into circular electrode sheets with a diameter of 10mm.
[0062] The button cell simulated batteries were assembled in a well-ventilated glove box. The lithium battery consisted of the following components: a C2025 model battery case, working electrode, negative electrode lithium metal, separator, and a suitably sized nickel mesh (for support). The electrolyte was 1M LiPF6 (EC / DMC / EMC = 1 / 1 / 1 by volume). The assembly sequence was: positive electrode case - positive electrode plate - two drops of electrolyte - separator - one drop of electrolyte - lithium metal - nickel mesh - negative electrode case. The sodium battery consisted of the following components: a C2025 model battery case, working electrode, negative electrode sodium metal, separator, and a suitably sized nickel mesh (for support). The electrolyte was 1M NaClO4 (PC / FEC = 95 / 5 by volume). The assembly sequence was: positive electrode case - positive electrode plate - two drops of electrolyte - separator - one drop of electrolyte - sodium metal - nickel mesh - negative electrode case. After assembly, the batteries were sealed using a sealing machine under 50 MPa pressure and then allowed to stand at room temperature. All electrochemical performance tests were conducted at room temperature using the LAND battery testing system manufactured by Wuhan Landian Electronics Co., Ltd. The battery performance test results are shown in Table 1.
[0063] Table 1. Performance test results of Example 1 and Comparative Examples 1-4
[0064] project 0.1C discharge specific capacity 1C500-cycle capacity retention Example 1 156mAh / g 85.5% Comparative Example 1 150mAh / g 63.9% Comparative Example 2 151mAh / g 74.2% Comparative Example 3 141mAh / g 66.5% Comparative Example 4 153mAh / g 70.3%
[0065] As shown in Table 1, the different structures of the iron manganese oxalate precursors result in differences in electron and ion transport in the composite material, thus affecting its electrochemical performance. Compared to Comparative Examples 1-4, Example 1 of the present invention exhibits higher 0.1C discharge specific capacity and 1C cycle capacity retention, reflecting that the lithium iron manganese phosphate obtained in Example 1 has the best performance. Furthermore, compared to Comparative Example 1, the capacity retention of other examples and comparative examples shows some improvement. In particular, the structural regulation method of the present invention can more effectively suppress the reaction between the electrode material and the electrolyte, thereby inhibiting manganese dissolution, reducing capacity decay, and improving the stability of the material.
Claims
1. A method for preparing a precursor of iron manganese oxalate, characterized in that: Includes the following steps, (1) Soluble oxalate, soluble manganese salt and soluble ferrous salt are dissolved in water to obtain soluble oxalate solution A, soluble manganese salt solution B and soluble ferrous salt solution C, wherein an antioxidant is added to soluble ferrous salt solution C. (2) Using soluble oxalate solution A as the base liquid, add part of soluble manganese salt solution B, and react to obtain a first solution containing MnC2O4 nuclei; (3) Mix a portion of the soluble ferrous salt solution C and the remaining portion of the soluble manganese salt solution B to obtain an iron-manganese mixed solution D. Add a portion of the iron-manganese mixed solution D to the first solution to obtain Fe containing a fixed Fe / Mn ratio. a Mn b The second solution of the C2O4 transition layer; (4) The remaining iron-manganese mixed solution D is continuously passed into the second solution, along with the remaining soluble ferrous salt solution C. The reaction yields Fe with a gradient increasing Fe / Mn ratio. c Mn d Iron manganese oxalate precursor with C2O4 transition layer and FeC2O4 shell; The iron manganese oxalate precursor has a MnC2O4 core and Fe... a Mn b C2O4 forms the first transition layer, Fe c Mn d C2O4 is the second transition layer, and FeC2O4 is the shell, where a, b, c, and d cannot all be 0, a+b=1, c+d=1, a / b=0.5-2, and c / d increases from the inside to the outside.
2. The preparation method according to claim 1, characterized in that: In the iron manganese oxalate precursor, the total atomic ratio of Fe to Mn is 1:
1.
3. The preparation method according to claim 1, characterized in that: In step (1), the molar ratio of oxalate, manganese salt and ferrous salt in the soluble oxalate solution A, soluble manganese salt solution B and soluble ferrous salt solution C is 2.1-2.8:1:1; The soluble oxalate is one or more of oxalic acid, ammonium oxalate, and sodium oxalate; the soluble manganese salt is one or more of manganese sulfate, manganese nitrate, manganese chloride, and manganese citrate; the soluble ferrous salt is one or more of ferrous sulfate, ferrous chloride, and ferrous citrate; and the antioxidant is one or more of ascorbic acid, citric acid, and malic acid.
4. The preparation method according to claim 1, characterized in that: In step (2), a portion of the soluble manganese salt solution B accounts for 1 / 3 to 2 / 3 of the total soluble manganese salt solution B; In step (3), the soluble ferrous salt solution C accounts for 1 / 3 to 2 / 3 of the total soluble ferrous salt solution C; the ferrous manganese mixed solution D accounts for 1 / 2 of the total ferrous manganese mixed solution D.
5. A positive electrode material for lithium or sodium-ion batteries, characterized in that: The iron manganese oxalate precursor prepared by the preparation method according to any one of claims 1-4 is obtained, specifically any one of Scheme 1, Scheme 2 and Scheme 3: Option 1 The iron manganese oxalate precursor was mixed evenly with a phosphorus source and a lithium source, and then calcined to obtain lithium iron manganese phosphate, a lithium-ion cathode material. Option 2 The iron manganese oxalate precursor was mixed evenly with a phosphorus source and a sodium source, and then calcined to obtain sodium iron manganese pyrophosphate, a sodium ion cathode material. Option 3 The iron manganese oxalate precursor was mixed evenly with a sodium source and calcined to obtain sodium iron manganese oxide, a sodium ion cathode material.
6. The lithium or sodium-ion battery cathode material according to claim 5, characterized in that: The phosphorus source is one or more of phosphoric acid, diammonium hydrogen phosphate, and ammonium dihydrogen phosphate; the lithium source is one or more of lithium carbonate, lithium hydroxide, and lithium acetate; and the sodium source is one or more of sodium carbonate, sodium bicarbonate, and sodium acetate.
7. The lithium or sodium-ion battery cathode material according to claim 5, characterized in that: The calcination temperature of Scheme 1, Scheme 2 and Scheme 3 is 550-900℃ and the calcination time is 6-18 hours. The calcination atmosphere of Scheme 1 and Scheme 2 is a mixture of nitrogen, argon and helium with hydrogen, and the calcination atmosphere of Scheme 3 is air or oxygen.
8. A lithium-ion or sodium-ion battery, characterized in that: It includes the lithium or sodium-ion battery cathode material as described in any one of claims 5-7.
Citation Information
Patent Citations
Precursor and LMFP and preparation method and application thereof
CN105514422A