Self-lubricating polyamide-imide wire enamel and preparation method thereof
By using low-density polyethylene wax as a lubricant in polyamide-imide enameled wire paint and controlling the ratio of it to polyamide-imide resin, the problem of lubricant precipitation in the enameled wire is solved and the self-lubricating performance of the enameled wire is improved. and wear resistance, extending the use time and reducing production costs and environmental pollution.
Patent Information
- Application Number
- CN202310918659.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-07-25
- Publication Date
- 2024-10-08
- Estimated Expiration
- 2043-07-25
AI Technical Summary
The lubricant in the existing polyamide-imide enameled wire paint is easy to precipitate after being left for a long time, resulting in a rough surface and poor lubricity of the enameled wire, and is easily damaged during the high-speed winding process, affecting the stability and service life of the motor and electrical appliances.
Low-density polyethylene wax is used as the lubricant, and by controlling the ratio of polyamide-imide resin and low-density polyethylene wax, the compatibility of the lubricant is improved to ensure that it is fully dispersed and combined in the paint film, thereby reducing precipitation. , improve the self-lubricating performance and wear resistance of enameled wire.
It effectively extends the service time of enameled wire, maintains smooth surface and low static friction coefficient, reduces production costs, avoids the use of external lubricating oil, and reduces environmental pollution and process complexity.
Smart Images

Figure BDA0004358031340000061
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of wire enamels, in particular to a self-lubricating polyamide-imide wire enamel and a preparation method thereof. Background Art
[0002] As people's requirements for the convenience and stability of electrical products gradually increase, high-quality enameled wire is an inevitable requirement for the miniaturization and lightweight trend of motors and electrical appliances. On the one hand, high-quality enameled wire requires good temperature resistance, and on the other hand, good self-lubrication and flexibility.
[0003] Among the existing enameled wire varieties, polyamideimide enameled wire has a very important position. Polyamideimide enameled wire has the advantages of high heat resistance and good lubrication performance. However, with the application of high-speed winding machines, the enameled wire passes through the wire at high speed. When winding, the enameled wire will be subjected to friction and impact, and the insulation layer of the enameled wire is susceptible to mechanical loss, resulting in a decrease in insulation performance. In addition, in the case of high-speed winding, due to poor lubrication, the enameled wire will be pulled thinner and the cross-sectional area of the enameled wire will be reduced, resulting in the scrapping of the coil or the enameled wire being broken. In order to reduce the surface friction coefficient of the enameled wire during winding, lubricants are added to the polyamideimide enameled wire paint. However, the polyamideimide enameled wire paint purchased on the market will have sedimentation of the lubricant after being placed for two days, resulting in a rough appearance and poor surface slip of the polyamideimide enameled wire. Summary of the invention
[0004] In order to solve the problem that the lubricant in the existing polyamide-imide wire enamel precipitates and settles after being left for a long time, the present invention provides a self-lubricating polyamide-imide wire enamel and a preparation method thereof.
[0005] The first aspect of the present invention provides a self-lubricating polyamide-imide wire enamel, which adopts the following technical scheme: a self-lubricating polyamide-imide wire enamel, wherein the raw materials of the wire enamel include 60-70% of polyamide-imide resin, 15-25% of a first solvent, 5-10% of a second solvent, and 1-5% of a low-density polyethylene wax by weight percentage, and the low-density polyethylene wax model is Mitsui Hi-Wax NL-200 low crystallinity, low-density polyethylene wax.
[0006] By adopting the above technical scheme, when low-density polyethylene wax is used as a lubricant for polyamide-imide wire enamel in the present application, the compatibility of the lubricant with the polyamide-imide solution can be greatly improved, thereby effectively reducing the precipitation of the lubricant from the polyamide-imide wire enamel and improving the convenience of using the polyamide-imide wire enamel.
[0007] In addition, when the content of the polyamide-imide resin is controlled within the range of 60-70% in the present application, not only can the adhesion between the wire enamel and the copper wire be improved, but also the polyamide-imide wire enamel can be ensured to have good wear resistance and heat resistance. However, when the content of the polyamide-imide resin exceeds 70%, the flexibility of the polyamide-imide wire enamel film will be reduced, and the production cost of the polyamide-imide wire enamel will also increase accordingly. Therefore, when the content of the polyamide-imide resin and the low-density polyethylene wax is controlled within the range of the present application, the self-lubricating properties, flexibility and adhesion of the polyamide-imide wire enamel can be effectively guaranteed, so that the enameled wire can adapt to the bending and stretching during the coil winding process.
[0008] Preferably, the raw materials of the wire enamel include 65-70% polyamide-imide resin, 20-25% first solvent, 5-10% second solvent, and 2-5% low-density polyethylene wax by weight.
[0009] Preferably, the molecular weight of the low-density polyethylene wax is 2800.
[0010] By adopting the above technical solution, when the molecular weight of the low-density polyethylene wax is 2800, the low-density polyethylene wax can be well dissolved in the second solvent and does not need to be operated under high temperature conditions, thus saving costs, while also ensuring the self-lubricating properties of the polyamide-imide wire enamel.
[0011] Preferably, the first solvent comprises N-methyl-2-pyrrolidone and a co-solvent in a weight ratio of (10-15):(5-10).
[0012] Preferably, the co-solvent is solvent oil.
[0013] Preferably, the second solvent is xylene.
[0014] The second aspect of the present invention provides a method for preparing a self-lubricating polyamide-imide wire enamel, which comprises the following steps:
[0015] (1) stirring and mixing a weighed amount of polyamide-imide resin and a first solvent to form a polyamide-imide solution;
[0016] (2) heating the weighed second solvent in a water bath to 80-100° C., and then adding the weighed low-density polyethylene wax to the xylene solution for heating and dissolving until the low-density polyethylene wax is completely dissolved;
[0017] (3) Pour the solution obtained in step (2) into step (1) and stir for 1-2 hours to obtain a self-lubricating polyamide-imide insulating varnish.
[0018] By adopting the above technical scheme, the present invention has the following beneficial effects: the polyamide-imide resin has excellent wear resistance, low friction coefficient and electrical insulation performance, but the friction coefficient of the polyamide-imide resin will be affected by the contact between the materials, the sliding speed, the temperature, the load and the lubrication conditions, which will make the friction coefficient of the polyamide-imide resin in different application scenarios different. In the present application, the polyamide-imide resin and the first solvent are first mixed to form a polyamide-imide solution, and then the xylene solution in which the low-density polyethylene wax is dissolved is stirred and mixed with the polyamide-imide solution, so that the low-density polyethylene wax can be fully dispersed in the polyamide-imide solution and fully miscible with the polyamide-imide solution, so that the self-lubricating polyamide-imide enameled wire obtained in the present application will not have the situation of low-density polyethylene wax precipitation after being stored for 2 days, and the low-density polyethylene wax can be completely combined with the paint film, so that the slipperiness of the enameled wire will not be damaged due to wear, so that the surface of the enameled wire is smooth, and the static friction coefficient of the surface of the enameled wire is reduced by 30%.
[0019] In addition, the preparation method of the present application is simple, and the low-density polyethylene wax will not precipitate when the self-lubricating polyamide-imide enameled wire obtained by the present application is stored for a short period of time. Therefore, users can prepare and use it by themselves, which is convenient for operation. At the same time, due to the good compatibility between low-density polyethylene wax and polyamide-imide solution, the process of coating the surface of the enameled wire with external wire oil (the process of lubricating the surface of the enameled wire) can be omitted in the production process of the enameled wire, which not only saves the process, but also avoids environmental pollution and physical harm to operators caused by the volatilization of solvents in the external wire oil. DETAILED DESCRIPTION
[0020] The present invention is further described in detail below with reference to the embodiments.
[0021] The raw materials used in the examples and comparative examples of the present application are all commercially available.
[0022] The low-density polyethylene wax model is Mitsui Hi-Wax NL-200, with a molecular weight of 2800 and a density of 920kg / m 3 , crystallinity is 54%;
[0023] The polyamide-imide resin used was Torlon 4301 from Solvay.
[0024] Example 1
[0025] A method for preparing a self-lubricating polyamide-imide wire enamel comprises the following preparation steps:
[0026] (1) pouring 7 kg of polyamide-imide resin and 2.4 kg of a first solvent into a stirring barrel, turning on a stirrer to stir and mix to form a polyamide-imide solution, wherein the first solvent includes 1.5 kg of N-methyl-2-pyrrolidone and 0.9 kg of solvent oil;
[0027] (2) Pour 0.5 kg of xylene into a heating barrel, turn on the heater and heat it in a water bath to 80° C., then add 0.1 kg of low-density polyethylene wax with a molecular weight of 2800 into the xylene solution and heat and dissolve it until the low-density polyethylene wax is completely dissolved in the toluene without any particles;
[0028] (3) Pour the solution obtained in step (2) into the polyamide-imide solution obtained in step (1) and stir for 1-2 hours to obtain a self-lubricating polyamide-imide insulating varnish.
[0029] Example 2
[0030] A method for preparing a self-lubricating polyamide-imide wire enamel comprises the following preparation steps:
[0031] (1) pouring 6.5 kg of polyamide-imide resin and 2.5 kg of a first solvent into a stirring barrel, turning on a stirrer to stir and mix to form a polyamide-imide solution, wherein the first solvent includes 1.5 kg of N-methyl-2-pyrrolidone and 1 kg of solvent oil;
[0032] (2) Pour 0.8 kg of xylene into a heating barrel, turn on the heater and heat in a water bath to 80° C., then add 0.2 kg of low-density polyethylene wax with a molecular weight of 2800 into the xylene solution and heat and dissolve until the low-density polyethylene wax is completely dissolved in the toluene without any particles;
[0033] (3) Pour the solution obtained in step (2) into the polyamide-imide solution obtained in step (1) and stir for 1 hour to obtain a self-lubricating polyamide-imide insulating varnish.
[0034] Example 3
[0035] A method for preparing a self-lubricating polyamide-imide wire enamel comprises the following preparation steps:
[0036] (1) pouring 6 kg of polyamide-imide resin and 2.5 kg of a first solvent into a stirring barrel, turning on a stirrer to stir and mix to form a polyamide-imide solution, wherein the first solvent includes 1.5 kg of N-methyl-2-pyrrolidone and 1 kg of solvent oil;
[0037] (2) Pour 1 kg of xylene into a heating barrel, turn on the heater and heat in a water bath to 80° C., then add 0.5 kg of low-density polyethylene wax with a molecular weight of 2800 into the xylene solution and heat and dissolve until the low-density polyethylene wax is completely dissolved in the toluene without any particles;
[0038] (3) Pour the solution obtained in step (2) into the polyamide-imide solution obtained in step (1) and stir for 2 hours to obtain a self-lubricating polyamide-imide insulating varnish.
[0039] Example 4
[0040] A method for preparing a self-lubricating polyamide-imide wire enamel comprises the following preparation steps:
[0041] (1) pouring 7 kg of polyamide-imide resin and 1.5 kg of a first solvent into a stirring barrel, turning on a stirrer to stir and mix to form a polyamide-imide solution, wherein the first solvent includes 1 kg of N-methyl-2-pyrrolidone and 0.5 kg of solvent oil;
[0042] (2) Pour 1 kg of xylene into a heating barrel, turn on the heater and heat in a water bath to 80° C., then add 0.5 kg of low-density polyethylene wax with a molecular weight of 2800 into the xylene solution and heat and dissolve until the low-density polyethylene wax is completely dissolved in the toluene without any particles;
[0043] (3) Pour the solution obtained in step (2) into the polyamide-imide solution obtained in step (1) and stir for 2 hours to obtain a self-lubricating polyamide-imide insulating varnish.
[0044] Example 5
[0045] A method for preparing a self-lubricating polyamide-imide wire enamel comprises the following preparation steps:
[0046] (1) pouring 6.9 kg of polyamide-imide resin and 2 kg of a first solvent into a stirring barrel, turning on a stirrer to stir and mix to form a polyamide-imide solution, wherein the first solvent includes 1.2 kg of N-methyl-2-pyrrolidone and 0.8 kg of solvent oil;
[0047] (2) Pour 0.8 kg of xylene into a heating barrel, turn on the heater and heat to 80° C. in a water bath, then add 0.3 kg of low-density polyethylene wax with a molecular weight of 2800 into the xylene solution and heat to dissolve until the low-density polyethylene wax is completely dissolved in the toluene without any particles;
[0048] (3) Pour the solution obtained in step (2) into the polyamide-imide solution obtained in step (1) and stir for 1.5 hours to obtain a self-lubricating polyamide-imide insulating varnish.
[0049] Comparative Example 1
[0050] A method for preparing a self-lubricating polyamide-imide wire enamel, which is different from that of Example 1 in that the low-density polyethylene wax used in step (2) is a low-density polyethylene wax of Mitsui Hi-Wax NL-100, having a molecular weight of 2400 and a density of 920 kg / m 3 , the crystallinity is 54%.
[0051] Comparative Example 2
[0052] A method for preparing a self-lubricating polyamide-imide wire enamel, which is different from Example 1 in that the low-density polyethylene wax used in step (2) is a low-density polyethylene wax of Mitsui Hi-Wax NL-500, with a molecular weight of 4200 and a density of 920 kg / m 3 , the crystallinity is 54%.
[0053] Comparative Example 1
[0054] The solution of Example 2 in the method for preparing a self-lubricating polyamide-imide wire enamel in Chinese patent CN106752894A is adopted.
[0055] Comparative Example 2
[0056] A method for preparing a self-lubricating polyamide-imide wire enamel is different from that of Example 1 in that an equal amount of polytetrafluoroethylene is used instead of low-density polyethylene wax, and other components and contents are the same as those of Example 1.
[0057] Comparative Example 3
[0058] A method for preparing a self-lubricating polyamide-imide wire enamel, which is different from Example 1 in that an equal amount of graphite is used to replace low-density polyethylene wax, and other components and contents are the same as those in Example 1.
[0059] Comparative Example 4
[0060] A method for preparing a self-lubricating polyamide-imide wire enamel, which is different from Example 1 in that the components of the raw materials are different, specifically 7 kg of polyamide-imide resin, 1.9 kg of a first solvent, 0.5 kg of xylene, and 0.6 kg of a low-density polyethylene wax with a molecular weight of 200, wherein the first solvent includes 1.4 kg of N-methyl-2-pyrrolidone and 0.5 kg of solvent oil, and the rest are the same as Example 1.
[0061] Comparative Example 5
[0062] A method for preparing a self-lubricating polyamide-imide wire enamel, which is different from Example 1 in that the components of the raw materials are different, specifically 7 kg of polyamide-imide resin, 2.4 kg of a first solvent, 0.55 kg of xylene, and 0.05 kg of a low-density polyethylene wax with a molecular weight of 200, wherein the first solvent includes 1.4 kg of N-methyl-2-pyrrolidone and 1 kg of solvent oil, and the rest are the same as Example 1.
[0063] Comparison Example
[0064] The commercially available self-lubricating polyamide-imide wire enamel has the following specific components in percentage by weight: 60% polyamide-imide resin, 34.5% solvent, 5% n-butanol, and 0.5% lubricant.
[0065] Performance Testing
[0066] The self-lubricating polyamide-imide wire enamel obtained in the above-mentioned embodiment and comparative example was uniformly coated on a drawn copper wire with a diameter of 0.5 mm, and then the copper wire coated with the self-lubricating polyamide-imide wire enamel was placed in a baking oven for baking. The self-lubricating polyamide-imide wire enamel was cured on the copper wire to form a paint film, so that the thickness of the paint film was 0.02 mm, and then the wire was cooled and wound to test the static friction coefficient of the enameled wire surface, the flexibility and adhesion of the paint film. The surface of the enameled wire obtained in the control example was coated with a wire discharge oil and then the static friction coefficient of the enameled wire surface was tested again. The test results are shown in Table 1;
[0067] The tests of static friction coefficient, flexibility and adhesion of the paint film are carried out according to the test method of static friction coefficient in GB / T4074.3-2008 "Test methods for winding wires Part 3: Mechanical properties", and the test results are shown in Table 1.
[0068] The self-lubricating polyamide-imide wire enamel obtained in the above-mentioned embodiments and comparative examples was placed in an open state at room temperature of about 25±2°C and stored. On the 2nd, 5th and 15th days, the lubricant was checked for precipitation. After being sealed and stored at room temperature for half a year, the precipitation was checked. The test results are shown in Table 1.
[0069] Table 1 Performance test results of wire enamel and wire enamel film
[0070]
[0071]
[0072] It can be seen from Table 1 that the self-lubricating polyamide-imide wire enamel obtained in the embodiment of the present application has good stability compared with comparative example 1. The low-density polyethylene wax of the self-lubricating polyamide-imide wire enamel obtained in the embodiment of the present application has not precipitated after 15 days of opening. It can be seen that the low-density polyethylene wax in the self-lubricating polyamide-imide wire enamel obtained in the present application does not precipitate and settle after long-term storage, indicating that its self-lubricating performance has not decreased, so that the service life of the self-lubricating polyamide-imide wire enamel can be extended. In addition, the static friction coefficient of the enameled wire obtained in the embodiment of the present application is much lower than that in the control example and the comparative example, indicating that the ratio of the present application can effectively ensure the self-lubricating performance of the enameled wire, and the paint film and the copper wire also have good adhesion, and no cracking will occur during the winding process.
[0073] Compared with Example 1, when the low-density polyethylene wax is replaced with an equal amount of polytetrafluoroethylene and graphite, the self-lubricating polyamide-imide wire enamels obtained in Comparative Examples 2 and 3 have precipitation and sedimentation of polytetrafluoroethylene and graphite on the second day of static placement. The main reason may be that compared with the low-density polyethylene wax, polytetrafluoroethylene and graphite are fully dispersed in the polyamide-imide solution under the action of stirring, and are not dissolved in the solvent in the polyamide-imide solution. Therefore, when lubricants such as polytetrafluoroethylene and graphite are used, lubricant precipitation and sedimentation will occur. It can be seen from Table 2 that the static friction coefficients of the paint films of Comparative Examples 2 and 3 are increased. The reason may be that lubricants such as polytetrafluoroethylene and graphite cannot be effectively dissolved in the polyamide-imide resin solution, resulting in a rough surface of the enameled wire and a high static friction coefficient. At the same time, the adhesion between the paint film and the copper wire is also poor.
[0074] Compared with Example 1, the self-lubricating properties of the self-lubricating polyamide-imide wire enamels obtained in Comparative Examples 4 and 5 are worse than those of the self-lubricating polyamide-imide wire enamels obtained in Example 1, and the static friction coefficient is increased compared with that in Example 1, indicating that when the content of the low-density polyethylene wax is higher or lower than the limit of the present application, the self-lubricating properties of the self-lubricating polyamide-imide wire enamels will decrease to a certain extent.
[0075] The embodiments of this specific implementation method are all preferred embodiments of the present invention, and are not intended to limit the protection scope of the present invention. Therefore, any equivalent changes made based on the structure, shape, and principle of the present invention should be included in the protection scope of the present invention.
Claims
1. A self-lubricating polyamide-imide wire enamel, characterized in that: The raw materials of the wire enamel include 60-70% polyamide-imide resin, 15-25% first solvent, 5-10% second solvent, and 1-5% low-density polyethylene wax by weight percentage; The first solvent includes N-methyl-2-pyrrolidone and a co-solvent in a weight ratio of (10-15):(5-10); the co-solvent is solvent oil, and the molecular weight of the low-density polyethylene wax is 2800.
2. The self-lubricating polyamide-imide wire enamel according to claim 1, characterized in that: The raw materials of the wire enamel include 65-70% of polyamide-imide resin, 20-25% of a first solvent, 5-10% of a second solvent, and 2-5% of a low-density polyethylene wax by weight.
3. A self-lubricating polyamide-imide wire enamel according to claim 1 or 2, characterized in that: The second solvent is xylene.
4. A method for preparing the self-lubricating polyamide-imide wire enamel according to any one of claims 1 to 3, characterized in that: The steps include: Step (1) mixing the weighed polyamide-imide resin and the first solvent by stirring to form a polyamide-imide solution; Step (2) heating the weighed second solvent in a water bath to 80-100° C., then adding the weighed low-density polyethylene wax into the second solvent and heating and dissolving the wax until the low-density polyethylene wax is completely dissolved; The solution obtained in step (2) is poured into step (1) and stirred for 1-2 hours to obtain a self-lubricating polyamide-imide wire enamel.