A method for quickly identifying self-discharge abnormalities
By preparing a pouch cell by dividing the battery into cores and structural components and monitoring changes in OCV, the problem of difficulty in identifying battery self-discharge anomalies in existing technologies is solved, enabling rapid and accurate anomaly identification and clear directions for improvement.
Patent Information
- Application Number
- CN202310943448.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-07-28
- Publication Date
- 2026-11-10
- Estimated Expiration
- 2043-07-28
AI Technical Summary
Existing technologies struggle to accurately identify the causes of abnormal battery self-discharge, especially physical self-discharge abnormalities caused by variations in the properties of structural components and subtle defects. Conventional diagnostic methods are time-consuming, labor-intensive, and cannot completely eliminate the influence of structural components.
The battery is divided into two parts: the core and the remaining structural components. It is then fabricated into a soft-pack battery to monitor changes in OCV. By continuously monitoring OCV under pressure and low temperature conditions, and combining this with multimeter measurements, it is determined whether the abnormality originates from the core or the structural components.
This provides a fast and convenient method to accurately identify the source of abnormal battery self-discharge, avoid misattributing it to the winding core, clarify the direction for improvement, and improve diagnostic efficiency and accuracy.
Smart Images

Figure CN116774073B_ABST
Abstract
Description
Technical Field
[0001] This invention belongs to the field of battery performance abnormality diagnosis technology, and in particular relates to a method for rapidly identifying self-discharge abnormalities. Background Technology
[0002] The statements in this section are merely background information related to the present invention and do not necessarily constitute prior art.
[0003] Self-discharge performance is one of the key evaluation indicators of a battery. The concept of battery self-discharge refers to the spontaneous decrease in the open-circuit voltage (OCV) of a battery under a certain state of charge. OCV is the open-circuit voltage, and the magnitude of the battery's self-discharge capacity is generally characterized by the K value, referred to as the self-discharge rate, with units of mV / h. The magnitude of the battery's self-discharge rate significantly restricts the actual usable capacity of the cell and its cycle life. Severe self-discharge can also lead to safety risks such as thermal runaway. As users have increasingly higher requirements for the cycle life and safety of power batteries, it means that the self-discharge rate of power batteries should be as low as possible.
[0004] Battery self-discharge is mainly divided into two categories: chemical self-discharge and physical self-discharge. Chemical self-discharge is mainly caused by the electrochemical activity of the material system, such as internal side reactions like film formation, gas generation, and shuttle reactions. Physical self-discharge is caused by localized short circuits or leakage within the battery cell: some are caused by micro-short circuits due to particles, burrs, and poor bridging between the positive and negative electrodes inside the core; others are caused by slow leakage due to structural abnormalities, such as insulation failure between the terminals and the top cover, hidden overlap between the core and the aluminum shell or top cover, and tip discharge of metal parts due to processing defects.
[0005] For some battery self-discharges caused by impurities within the materials or foreign matter introduced during the battery manufacturing process, the failure location and clear evidence can be easily found through existing battery disassembly observation and related characterization analysis methods. However, the second type of abnormal battery self-discharge caused by variations in the properties of structural components and inherent defects is often difficult to detect: for example, the resistance variation between the terminals and the top cover due to fluctuations in incoming materials or corrosion and aging cannot be measured with a simple multimeter (its resistance range is far beyond the multimeter's range); as battery mass margin designs become increasingly aggressive, poor contact between the core and the casing can sometimes lead to leakage; and tiny, hard-to-detect burrs or metal wires left behind in the processing of metal structural components can also cause micro-conductivity between the positive and negative electrodes.
[0006] For the second type of abnormal battery physical self-discharge described above, it is difficult to draw a definite conclusion by directly characterizing the structural components.
[0007] The above analysis shows that the common practice for diagnosing abnormal battery self-discharge is to perform self-discharge testing at the battery level. If the battery's OCV (Output Voltage Value) deviates significantly from the normal range over time at low temperatures, the abnormality is considered to originate from physical self-discharge at the battery level. Non-destructive analysis methods generally involve visual inspection and X-ray penetration, such as using X-ray or CT scans to observe internal overlaps or foreign objects in the casing. However, these tests are expensive and time-consuming. Destructive analysis involves disassembling the battery, briefly inspecting internal structural components for abnormalities such as poor overlaps, and then gradually unfolding the core to search for suspicious short circuit points or other defects that could cause micro-short circuits on the electrode and separator surfaces.
[0008] Battery-level self-discharge anomalies originate from two sources: the internal structure of the battery core, which is significantly affected by cell manufacturing processes, and structural abnormalities in the casing and other components. The diagnostic methods mentioned above cannot completely eliminate the influence of structural components on self-discharge. For example, voltage anomalies caused by variations in the resistance of the insulating rubber between the casing and a particular terminal are difficult to identify through simple non-destructive scanning and disassembly. Furthermore, in many cases of searching for internal short circuits, a significant number fail to find clear evidence of a short circuit point. In practical diagnostic work, attributing severe battery self-discharge solely to manufacturing problems lacks scientific rigor. Summary of the Invention
[0009] To overcome the shortcomings of the prior art, the present invention provides a method for rapidly identifying self-discharge anomalies, which can accurately identify the causes of structural components, so as to avoid misattributing the cause to the core or the core manufacturing process.
[0010] To achieve the above objectives, one or more embodiments of the present invention provide the following technical solutions:
[0011] Firstly, a method for rapidly identifying self-discharge anomalies is disclosed, including:
[0012] The battery with abnormal self-discharge is divided into two parts and the two parts are separated. The first part is the core, and the second part is the remaining structural components of the battery except for the core.
[0013] The core was vacuum-sealed into an aluminum-plastic film to prepare a pouch cell. The change of OCV of the pouch cell over time was continuously monitored under pressure.
[0014] If the OCV of the soft-pack battery deviates from the set range over time, it is determined that the battery's abnormal self-discharge originates from inside the core.
[0015] If the change in OCV of the pouch battery over time is within the set range, it is a normal trend. This excludes the possibility that the battery's self-discharge abnormality originates from inside the core. The improvement of the battery's self-discharge abnormality should focus on the second part, namely the structural components.
[0016] As a further technical solution, a step for identifying batteries with abnormal self-discharge is also included:
[0017] A number of batteries with abnormal self-discharge rates, qualified batteries, or batteries with poor voltage drop due to customer complaints were returned.
[0018] After placing abnormal and qualified batteries at low temperature for a first set time, the battery OCV is collected at fixed intervals, and then continuously collected for a second set time.
[0019] If the OCV change of an abnormal battery at low temperature deviates from the OCV change of a qualified battery by more than the set range, then the abnormal battery is judged to be a physical self-discharge abnormality at the battery level.
[0020] As a further technical solution, the core is vacuum-sealed into an aluminum-plastic film to prepare a soft-pack battery. The specific process is as follows:
[0021] Remove the casing from the abnormal battery and the qualified battery, separate the top cover from the core at the electrode tab welding point, and leave a portion of the electrode tab in the core part.
[0022] Design the volume or size of the aluminum-plastic film bag according to the core size, and prepare the external lead tabs with heat-sealing adhesive;
[0023] Quickly place the separated core into an aluminum-plastic film bag with the tab side facing outwards. Overlap the external lead tab onto the tab reserved on the core to fix the overlap. At this time, the heat-sealing adhesive part is stuck to the edge of the aluminum-plastic film.
[0024] Inside the glove box, a heat sealer with a vacuum extraction function is used to seal the aluminum-plastic film bag at the heat sealant to prepare a soft-pack battery.
[0025] As a further technical solution, after the soft-pack battery is prepared, the soft-pack battery containing qualified and abnormal cores is taken out of the glove box and left to stand at room temperature for a certain period of time.
[0026] As a further technical solution, the settling time is 2 hours.
[0027] As a further technical solution, after the settling period, a clamp is applied to the pouch battery and an appropriate clamping force is set. The battery is then set to stand again at a low temperature, and a clamping force is applied to the pouch battery. If there are soft conductive points inside, they are fully exposed.
[0028] As a further technical solution, under clamping force and in a low-temperature environment, the battery OCV of the soft-pack battery is monitored continuously using a multimeter at fixed intervals in voltage mode.
[0029] As a further technical solution, before continuing to monitor the OCV change of the pouch cell over time under pressure, a curve is plotted based on the measured data to compare the trends of OCV change over time for qualified and abnormal cells.
[0030] As a further technical solution, if the OCV of qualified and abnormal batteries changes in a basically consistent trend over time or the OCV change rate is within the qualified range, then it is necessary to focus on investigating issues such as abnormal overlap between the core and structural components, as well as insulation resistance failure of structural components.
[0031] As a further technical solution, if the OCV change trend of the abnormal soft-pack battery deviates significantly from that of the qualified soft-pack battery, it indicates that the abnormal self-discharge originates from the core part of the original square-shell battery, and the micro-short circuit inside the core needs to be investigated.
[0032] The above one or more technical solutions have the following beneficial effects:
[0033] This invention isolates the internal winding core and other structural components of the battery, retaining only a portion of the winding core's tabs. The winding core is vacuum-sealed within an aluminum-plastic film to create a pouch battery. Under pressure, the battery's open-circuit volume (OCV) is continuously monitored over time. If the OCV of the newly manufactured pouch battery still significantly deviates from the normal range, the anomaly is determined to originate from within the winding core. If the OCV change follows a normal trend, the anomaly is likely due to a structural component, thus improvements to the battery's self-discharge anomaly should focus on the structural components. This method avoids the erroneous conclusion that the battery's self-discharge anomaly actually originates from the structural components, but the underlying cause is mistakenly attributed to the internal winding core. It provides a simple, convenient, practical, and effective method for determining the cause, offering clear guidance for anomaly improvement.
[0034] Advantages of additional aspects of the invention will be set forth in part in the description which follows, and in part will be obvious from the description, or may be learned by practice of the invention. Attached Figure Description
[0035] The accompanying drawings, which form part of this invention, are used to provide a further understanding of the invention. The illustrative embodiments of the invention and their descriptions are used to explain the invention and do not constitute an improper limitation of the invention.
[0036] Figure 1 This is an example diagram of an internal short circuit in the core of the present invention.
[0037] Figure 2 This is an example diagram of battery self-discharge caused by structural component abnormality in an embodiment of the present invention;
[0038] Figures 3(a)-3(b) This is a schematic diagram of a square-shell battery product according to an embodiment of the present invention; front view of the square-shell battery;
[0039] Figures 4(a)-4(b) This is an example diagram of the disassembled square battery casing and top cover portion according to an embodiment of the present invention;
[0040] Figure 5 This is an example diagram of the disassembled core according to an embodiment of the present invention;
[0041] Figures 6(a)-6(b) The images show the front and top views of a soft-pack battery made from disassembled core coils, as described in an embodiment of the present invention. Detailed Implementation
[0042] It should be noted that the following detailed descriptions are exemplary and intended to provide further illustration of the invention. Unless otherwise specified, all technical and scientific terms used herein have the same meaning as commonly understood by one of ordinary skill in the art to which this invention pertains.
[0043] It should be noted that the terminology used herein is for the purpose of describing particular implementations only and is not intended to limit the exemplary implementations of the present invention.
[0044] Where there is no conflict, the embodiments and features in the embodiments of the present invention can be combined with each other.
[0045] Example 1
[0046] This embodiment discloses a method for rapidly identifying self-discharge anomalies, including:
[0047] The internal winding core and other structural components of the battery are isolated, while a portion of the winding core's tabs are retained. The winding core is then vacuum-sealed within an aluminum-plastic film to prepare a pouch battery. Under pressure, its open-circuit volume (OCV) is continuously monitored over time. If the OCV of the newly prepared pouch battery still significantly deviates from the normal range, the anomaly is determined to originate from within the winding core. If the OCV change follows a normal trend, the anomaly is likely due to the battery's structural components, and improvements to address self-discharge anomalies should focus on these structural components.
[0048] The detailed identification steps for this embodiment are as follows:
[0049] Step 1: Take a number of batteries from the production line that have abnormal or qualified K values, or batteries that have poor voltage drop due to customer complaints, or good batteries.
[0050] Step 2: After placing the abnormal and qualified batteries (≥2) at low temperature for 2 hours, use a multimeter in voltage mode to collect the battery OCV at fixed intervals for 2-3 consecutive days.
[0051] Step 3: If the abnormal battery OCV change at low temperature deviates significantly from the qualified battery OCV change, it can be determined that the abnormality is a physical self-discharge abnormality at the battery level.
[0052] The abnormal battery OCV changes significantly at low temperatures, i.e., K 异常电池 >K 合格电池 +3σ 合格电池 σ is the standard deviation of the distribution of K values for a certain batch of qualified batteries.
[0053] Step 4: Remove the outer casing of the defective battery and the qualified battery under the glove box atmosphere. Use a knife or needle-nose pliers to separate the top cover from the core at the electrode tab welding point. The operation method is the same for defective and qualified batteries. Leave a part of the electrode tab in the core part. The length of the reserved electrode tab is L≥0.2mm.
[0054] The aforementioned glove box can isolate air and prevent the battery from reacting with the air inside.
[0055] Step 5: Based on the core size, design the volume or size of the aluminum-plastic film bag in advance. The volume of the aluminum-plastic film bag and the core volume should meet the following condition: T 厚-铝塑膜袋 *W 宽-铝塑膜袋 *H 高-铝塑膜袋 >1.05*T 厚-卷芯 *1.15W 宽-卷芯 *1.15H 高-卷芯 Prepare external square electrode tabs with heat-sealing adhesive in advance. The external electrode tabs enable the soft-pack inner core to conduct to the outside.
[0056] Step 6: Quickly place the separated core into the aluminum-plastic film bag with the tab side facing outwards. Overlap the external lead tab onto the tab reserved on the core and fix the overlap by welding or other methods. At this time, the heat-sealing adhesive part is just stuck on the edge of the aluminum-plastic film.
[0057] The purpose of this step is to obtain a well-encapsulated pouch battery, which facilitates the monitoring of the battery's open-circuit voltage later. The advantage is that the internal structure and interface of the core will not be damaged under the inert atmosphere of the glove box, and the original prismatic battery's charge can be maintained.
[0058] Step 7: In the glove box atmosphere, use a heat sealer with vacuum pumping function to seal the aluminum-plastic film bag at the heat seal adhesive to prepare a soft-pack battery. The aluminum shell of the square battery is prone to poor overlap with the core, while the packaging of the soft-pack battery is a non-conductive aluminum-plastic film, which can eliminate the influence of the aluminum shell on the self-discharge of the original battery.
[0059] Step 8: Remove the soft-pack batteries containing qualified and defective cores from the glove box and let them stand at room temperature for 2 hours.
[0060] Step 9: After the settling period, apply a clamp to the soft-pack battery and set an appropriate clamping force. Let it stand at a low temperature for 2 hours. Applying clamping force to the soft-pack battery here will allow it to be fully exposed if there are soft conductive points inside. Full exposure can help determine the source of self-discharge and actually find the cause of the abnormality.
[0061] Applying clamping force is to make the internal cores more tightly contacted. If there are foreign particles inside, pressure can be applied to puncture the diaphragm, exposing the defects inside the core.
[0062] Step 10: Under clamping force and in a low-temperature environment, use a multimeter (voltage setting) to monitor the battery OCV at fixed intervals for 2-3 days.
[0063] Step 11: Plot the measured data and compare the trends of OCV changes over time for qualified and abnormal batteries;
[0064] Step 12: If the trends of the two are basically consistent or the OCV change rate is within the qualified range, it indicates that the self-discharge abnormality is likely to originate from the structural components of the square battery. In this case, it is necessary to focus on investigating aspects such as abnormal overlap between the core and the structural components, and failure of the insulation resistance of the structural components.
[0065] Step 13: If the OCV change trend of the abnormal soft-pack battery deviates significantly from that of a qualified soft-pack battery, it indicates that the abnormal self-discharge originates from the core part of the original square-shell battery. In this case, it is necessary to focus on investigating the micro-short circuit inside the core.
[0066] The image shows the effect of accurately identifying abnormalities in the internal core and structural components of a battery using the method of this invention. Figure 1 The method of this invention is used to determine that the abnormal self-discharge of the battery originates from inside the battery core and is unrelated to the battery structural components. Figure 2 It was determined that the internal winding of the battery was normal, and the low battery voltage was due to leakage caused by an abnormality in the structural components.
[0067] Specifically, Figure 1 This is an example diagram of an internal short circuit in a battery core. NG Cell represents a pouch cell prepared from a core taken from a prismatic battery with an abnormal K value; OK Cell represents a pouch cell prepared from a core taken from a battery with a normal K value. Due to the thermal entropy effect of the battery, the battery voltage will increase slightly at low temperatures, and since the battery has not undergone further charging and discharging, the voltage basically remains at the initial level. The magnitude of self-discharge is generally evaluated by the slope of the change in OCV.
[0068] Figure 2 This is an example diagram of battery self-discharge caused by structural abnormalities. NG Cell represents a pouch cell prepared by taking the core from a low-voltage square-shell battery returned by a customer complaint; OK Cell represents a pouch cell prepared by taking the core from a battery with normal voltage in the same module; the three batteries have not undergone further charging and discharging, and the voltage basically remains at the initial level. The magnitude of self-discharge is generally evaluated by the slope of the change in OCV.
[0069] Example 2
[0070] To better illustrate a method for rapidly identifying self-discharge anomalies, specific experimental examples are provided, including:
[0071] Step 1: Take one battery with an abnormal K value from the production line. a =0.0995mV / h, see Figures 3(a)-3(b) Two normal battery cells, K b =0.036mV / h, K c =0.034mV / h, the voltage values measured by the multimeter are 3.6955, 3.7654, and 3.7700V respectively;
[0072] Step 2: Place the three batteries in a -30℃ high and low temperature chamber and let them stand for 2 hours. Then, use a multimeter to test their voltage at 8-hour intervals and record the results. Continue testing for 2 days.
[0073] Step 3: Obtain the OCV variation graph of the three batteries over the test time. Calculate the K-temperature values of the three batteries from the curve slopes, as follows: K a1 =0.0982, K b1 =0.0225, K c1 =0.0232mV / h;
[0074] Step 4, obviously K a1 Significantly greater than K b1 K c1 The abnormal K value of the abnormal battery originates from a physical micro-short circuit inside the battery.
[0075] Step 5: Remove the battery casing under the protective atmosphere of the glove box, and cut off the top cover. See Figures 4(a)-4(b) To obtain the complete roll core, see Figure 5 In this step, some tabs should be retained on the core;
[0076] Step 6: Insert the core into the pre-prepared three-side sealed aluminum-plastic film bag, overlap one end of the external lead tab on the core lead tab, and fix it simply. The heat seal adhesive of the external lead tab should be aligned with the edge of the aluminum-plastic film bag.
[0077] Step 7: Use a heat sealer with vacuum function to seal the aluminum-plastic film at the heat sealant area to obtain a well-encapsulated soft-pack battery, as shown in Figure 6.
[0078] Step 8: Repeat steps 5-7 to make the remaining batteries into pouch batteries using the same method.
[0079] Step 9: Remove the finished soft-pack battery from the glove box and let it stand at room temperature for 2 hours;
[0080] Step 10: After the settling period, place the soft-pack battery in a -30℃ high and low temperature chamber for 2 hours. Then, use a multimeter to test the OCV of the battery every 8 hours and record the results.
[0081] Step 11: Plot the OCV~t of the three pouch cells. It can be seen that the voltage drop rate of the abnormal pouch cell is significantly greater than that of the normal cell. Figure 1 If so, it can be determined that the abnormal self-discharge of the original square-shell battery originated from the core.
[0082] Step 12: Disassemble the core. Metal deposition points can be found at the diaphragm interface and the corresponding negative electrode.
[0083] Example 3
[0084] To better illustrate a method for rapidly identifying self-discharge anomalies, specific experimental examples are provided, including:
[0085] Step 1: Take one battery with abnormal (low voltage) terminal voltage from the customer's returned module and two normal batteries. The voltage values measured by the multimeter are 3.4965, 3.552, and 3.550V respectively. The voltage difference between individual cells in the same module is greater than the customer's standard ΔV > 36mV.
[0086] Step 2: Place the three batteries in a -30℃ high and low temperature chamber and let them stand for 2 hours. Then, use a multimeter to test their voltage at 8-hour intervals and record the results. Continue testing for 2 days.
[0087] Step 3: Obtain the OCV variation curves of the three cells over time. Calculate the K-temperature values of the three cells from the curve slopes, as follows: K a2 =0.0706mV / h, K b2 =0.042mV / h, K c2 =0.038mV / h;
[0088] Step 4, K a2 Significantly greater than K b2 K c2 The low voltage of the module-end battery originates from the physical self-discharge inside the battery.
[0089] Step 5: Remove the outer casing of the battery under the protective atmosphere of a glove box, and cut off the top cover to obtain a complete core. In this step, some tabs should be left on the core.
[0090] Step 6: Quickly insert the removed core into the pre-prepared three-sided sealed aluminum-plastic film bag. Overlap one end of the square external lead tab onto the core lead tab and fix it in place. The heat sealant of the external lead tab should be aligned with the edge of the aluminum-plastic film bag.
[0091] Step 7: Use a heat sealer with vacuum function to seal the aluminum-plastic film at the heat sealant to obtain a well-encapsulated soft-pack battery.
[0092] Step 8: Repeat steps 5-7 to make the remaining batteries into pouch batteries using the same method;
[0093] Step 9: Remove the finished soft-pack battery from the glove box and let it stand at room temperature for 2 hours;
[0094] Step 10: After the settling period, place the soft-pack battery in a -30℃ high and low temperature chamber for 2 hours. Then, use a multimeter in voltage mode to measure the OCV of the battery every 8 hours and record the results.
[0095] Step 11: Plot the OCV of the three pouch cells over time. By comparing the slopes of the three curves, the rate of change of OCV of the three pouch cells over time is basically the same. (See...) Figure 2 ;
[0096] Step 12: Based on the conclusion of step 11, it is considered that the internal structure of the core is normal, and the potential cause of the low voltage of the original square-shell battery is an abnormality in the structural components.
[0097] Step 13: A computed tomography scan of the battery top cover terminal position revealed that the insulating rubber between the negative terminal and the top cover was misaligned, resulting in micro-contact between the terminal and the casing, thus causing leakage.
[0098] While the specific embodiments of the present invention have been described above in conjunction with the accompanying drawings, this is not intended to limit the scope of protection of the present invention. Those skilled in the art should understand that various modifications or variations that can be made by those skilled in the art without creative effort based on the technical solutions of the present invention are still within the scope of protection of the present invention.
Claims
1. A method for rapidly identifying self-discharge anomalies, characterized in that, include: The battery with abnormal self-discharge is divided into two parts and the two parts are separated. The first part is the core, and the second part is the remaining structural components of the battery except for the core. The core was vacuum-sealed into an aluminum-plastic film to prepare a pouch cell. The change of OCV of the pouch cell over time was continuously monitored under pressure. The core is vacuum-sealed into an aluminum-plastic film to prepare a pouch battery. The specific process is as follows: Remove the outer casing from the abnormal battery and the qualified battery, and separate the top cover from the core at the electrode tab welding point, leaving a portion of the electrode tab in the core part. Design the size of the aluminum-plastic film bag according to the core size, and prepare the external lead tabs with heat-sealing adhesive; Quickly place the separated core into an aluminum-plastic film bag with the tab side facing outwards. Overlap the external lead tab onto the tab reserved on the core to fix the overlap. At this time, the heat-sealing adhesive part is stuck to the edge of the aluminum-plastic film. Inside the glove box, a heat sealer with a vacuum pumping function is used to seal the aluminum-plastic film bag at the heat sealant to prepare a soft-pack battery. If the OCV of the soft-pack battery deviates from the set range over time, it is determined that the battery's abnormal self-discharge originates from inside the core. If the change in OCV of the pouch battery over time is within the set range, it is a normal trend. This excludes the possibility that the battery's self-discharge abnormality originates from inside the core. The improvement of the battery's self-discharge abnormality should focus on the second part, namely the structural components.
2. The method for rapidly identifying self-discharge anomalies as described in claim 1, characterized in that, It also includes steps for identifying batteries with abnormal self-discharge: Take a number of batteries with abnormal discharge rate, qualified discharge rate, or returned due to customer complaints with poor voltage drop, or good batteries. After placing abnormal and qualified batteries at low temperature for a first set time, the battery OCV is collected at fixed intervals, and then continuously collected for a second set time. If the OCV change of an abnormal battery at low temperature deviates from the OCV change of a qualified battery by more than the set range, then the abnormal battery is judged to be a physical self-discharge abnormality at the battery level.
3. The method for rapidly identifying self-discharge anomalies as described in claim 1, characterized in that, After the soft-pack batteries are prepared, the soft-pack batteries containing qualified and abnormal cores are taken out of the glove box and left to stand at room temperature for a certain period of time.
4. The method for rapidly identifying self-discharge anomalies as described in claim 3, characterized in that, After the settling period, apply a clamp to the pouch battery and set an appropriate clamping force. Set it to stand again at a low temperature and apply clamping force to the pouch battery. If there are soft conductive points inside, expose them fully.
5. The method for rapidly identifying self-discharge anomalies as described in claim 4, characterized in that, Under clamping force and in a low-temperature environment, the OCV of the soft-pack battery is monitored continuously using a multimeter at fixed intervals in voltage mode.
6. The method for rapidly identifying self-discharge anomalies as described in claim 1, characterized in that, Before continuing to monitor the OCV of the pouch cell over time under pressure, a curve is plotted based on the measured data to compare the trends of OCV changes over time for qualified and abnormal cells.
7. The method for rapidly identifying self-discharge anomalies as described in claim 1, characterized in that, If the OCV of qualified and abnormal batteries changes in a basically consistent trend over time, or if the OCV change rate is within the qualified range, then it is necessary to focus on investigating abnormal overlap between the core and structural components, as well as the failure of insulation resistance of structural components.
8. The method for rapidly identifying self-discharge anomalies as described in claim 1, characterized in that, If the OCV change trend of an abnormal pouch battery deviates significantly from that of a qualified pouch battery, it indicates that the abnormal self-discharge originates from the core of the original square-shell battery, and the micro-short circuit inside the core needs to be investigated.
9. The method for rapidly identifying self-discharge anomalies as described in claim 1, characterized in that, The method is used for diagnosing abnormal performance of lithium-ion batteries.
Citation Information
Patent Citations
Method for detecting internal defects of battery cell
CN111141755A
Battery testing tool
CN208847825U