Strontium titanate ceramics and preparation method and application thereof

By introducing +5-valent Nb and optimizing the preparation process, the prepared strontium titanate ceramic achieves an excellent balance in dielectric constant and loss, solving the problem in the existing technology that it is difficult to simultaneously increase the dielectric constant and reduce dielectric loss. The preparation of high-quality ceramics is achieved.

CN116813331BActive Publication Date: 2024-10-18TSINGHUA UNIVERSITY
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202310840763.6
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-07-10
Publication Date
2024-10-18
Estimated Expiration
2043-07-10

AI Technical Summary

Technical Problem

It is difficult for existing strontium titanate ceramics to simultaneously increase the dielectric constant and reduce dielectric loss, making it difficult to meet the demand for high-quality dielectric materials.

Method used

By introducing +5-valent Nb, defects are induced in the ST (SrTiO3) matrix to form defect dipoles and defect dipole clusters. Control 0 < The process of shaping and sintering in a reducing atmosphere prepares ceramics with high dielectric constant and low dielectric loss.

Benefits of technology

The high dielectric constant and low dielectric loss of strontium titanate ceramics are achieved. Specifically, the dielectric constant is 3.5×104-6×104 at room temperature and 1kHz, and the dielectric loss is less than 1%. At the same time, the process is simple, low-cost and repeatable. Good performance and stable performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116813331B_ABST
    Figure CN116813331B_ABST
Patent Text Reader

Abstract

The invention discloses a strontium titanate ceramic and a preparation method and application thereof. The chemical formula of the strontium titanate ceramic includes SrTiNb x O3, wherein 0<x≤0.012. The strontium titanate ceramic has a high dielectric constant and maintains an extremely low dielectric loss, which can meet the use needs to a greater extent. Specifically, at room temperature and 1kHz, the dielectric constant of the strontium titanate ceramic can be 3.5×10 4 ‑6×10 4 , dielectric loss is less than 1%.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of multifunctional electronic ceramic materials, and specifically relates to a strontium titanate ceramic and a preparation method and application thereof. Background Art

[0002] With the rapid development of the electronics field, many fields have put forward more stringent requirements for electronic components, and the development of high-quality dielectric materials is of great significance. Strontium titanate with a typical perovskite structure has excellent properties such as low dielectric loss, and is believed to be expected to develop into a multifunctional dielectric material after modification.

[0003] At present, there are two main methods for modifying strontium titanate ceramics. The first is ion doping, and common doping elements include La, Ta, Ce, Dy, Er, Nb, etc. The other is to adjust the preparation process, change the sintering atmosphere, etc. Both modification methods increase the dielectric constant of strontium titanate ceramics by adjusting the defect concentration, but it is often difficult to maintain low dielectric loss. Therefore, preparing a ceramic with both giant dielectric constant and low dielectric loss has very important application value. Summary of the invention

[0004] The present invention aims to solve one of the technical problems in the related art to at least a certain extent. To this end, one object of the present invention is to provide a strontium titanate ceramic and a preparation method and application thereof. The strontium titanate ceramic has a high dielectric constant and maintains a low dielectric loss, which can meet the use requirements to a greater extent. Specifically, at room temperature and 1KHz, the dielectric constant of the strontium titanate ceramic can be 3.5×10 4 -6×10 4 , dielectric loss is less than 1%.

[0005] In one aspect of the present invention, the present invention provides a strontium titanate ceramic. According to an embodiment of the present invention, the strontium titanate ceramic chemical formula includes SrTiNb x O3, where 0<x≤0.012.

[0006] According to the strontium titanate ceramic of the above embodiment of the present invention, the chemical formula includes SrTiNb x O3, by introducing +5-valent Nb, defects are induced in the ST (SrTiO3) matrix, especially by controlling 0<x≤0.012, and further forming defect dipoles and defect dipole clusters, thereby increasing the dielectric constant and producing a localized effect on free electrons, maintaining low dielectric loss. As a result, the strontium titanate ceramic has a high dielectric constant and maintains low dielectric loss, which can meet the needs of use to a greater extent. Specifically, at room temperature and 1kHz, the dielectric constant of the strontium titanate ceramic can be 3.5×10 4 -6×10 4, dielectric loss is less than 1%.

[0007] In addition, the strontium titanate ceramic according to the above embodiment of the present invention may also have the following technical features:

[0008] According to an embodiment of the present invention, 0.003≤x≤0.006. Thus, the strontium titanate ceramic has a high dielectric constant and a low dielectric loss.

[0009] In another aspect of the present invention, the present invention provides a method for preparing the above-mentioned strontium titanate ceramic. According to an embodiment of the present invention, the method comprises:

[0010] (1) mixing strontium titanate raw material and Nb2O5, grinding and drying to obtain a mixed material powder;

[0011] (2) calcining the mixed material powder, grinding and drying it to obtain Nb-doped strontium titanate powder;

[0012] (3) mixing the Nb-doped strontium titanate powder and the binder, grinding and sieving, and then dry-pressing and debinding to obtain a ceramic green body;

[0013] (4) Sintering the ceramic green body in a reducing atmosphere to obtain strontium titanate ceramics.

[0014] According to the molecular formula of strontium titanate ceramics, weigh strontium titanate raw materials and Nb2O5, mix, grind and dry to obtain a mixed powder. The mixed powder is calcined, and the ions in the strontium titanate raw materials and Nb2O5 diffuse through the solid phase chemical reaction under the action of heat, thereby obtaining a solid solution with a fixed composition and forming a main crystal phase; at the same time, in this process, volatile impurities such as moisture in the raw materials are removed, the purity of the ceramic material is improved, the second phase is avoided, the raw material particles are densified, and have a certain reactivity, which is conducive to obtaining a dense microstructure after sintering, and then the ceramic material obtained after calcination is ground and dried to obtain Nb-doped strontium titanate powder. The Nb-doped strontium titanate powder and the binder are mixed, ground and sieved, and then dry-pressed and debonded to obtain a ceramic green body. Finally, the ceramic green body is sintered in a reducing atmosphere, and the Nb-doped strontium titanate powder is formed and begins to shrink after being heated to a certain temperature. At a temperature below the melting point, the particles interact with each other and generate strength through material migration, and the sintering process can eliminate pores, and the grains grow evenly, thereby obtaining a dense ceramic block with a certain strength, achieving ceramic densification, and then preparing strontium titanate ceramics with high dielectric constant and low dielectric loss. Therefore, the method can be used to prepare strontium titanate ceramics with high dielectric constant and low dielectric loss, and the method is simple in process, low in cost, good in repeatability, and stable in performance.

[0015] In addition, the method for preparing strontium titanate ceramics according to the above embodiment of the present invention may also have the following technical features:

[0016] According to an embodiment of the present invention, in step (1), the strontium titanate raw material includes SrTiO3 and / or a mixture of SrCO3 and TiO2. Thus, a strontium titanate ceramic with a high dielectric constant and low dielectric loss can be obtained.

[0017] According to an embodiment of the present invention, in step (1), the grinding speed is 260r / min-300r / min, and the grinding time is 12h-24h.

[0018] According to an embodiment of the present invention, in step (2), the calcination temperature is 1100° C.-1200° C. and the calcination time is 2 h-3 h. Thus, the fineness and activity of the Nb-doped strontium titanate powder can be improved.

[0019] According to an embodiment of the present invention, in step (2), the grinding speed is 260r / min-300r / min, and the grinding time is 12h-24h.

[0020] According to an embodiment of the present invention, in step (3), the mesh size of the sieving is 130-170 meshes.

[0021] According to an embodiment of the present invention, in step (3), the binder includes at least one of a 5wt%-8wt% polyvinyl alcohol aqueous solution and a 5wt%-8wt% polyvinyl butyral ethanol solution.

[0022] According to an embodiment of the present invention, in step (3), the debinding temperature is 600° C.-650° C. and the time is 2 h-3 h, thereby removing the binder in the ceramic green body.

[0023] According to an embodiment of the present invention, in step (4), the sintering temperature is 1400° C.-1450° C., and the sintering time is 2 h-3 h; thereby, the purity and density of the strontium titanate ceramic are improved.

[0024] According to an embodiment of the present invention, in step (4), the reducing atmosphere includes at least one of N2, H2 / N2 mixed gas and H2 / Ar mixed gas, the volume proportion of H2 in the H2 / N2 mixed gas is 1%-10%, and the volume proportion of H2 in the H2 / Ar mixed gas is 1%-10%.

[0025] In a third aspect of the present invention, the present invention proposes the use of the above strontium titanate ceramic or the strontium titanate ceramic prepared by the above method in the fields of communication, radar or electronics.

[0026] Additional aspects and advantages of the present invention will be given in part in the following description and in part will be obvious from the following description, or will be learned through practice of the present invention. BRIEF DESCRIPTION OF THE DRAWINGS

[0027] The above and / or additional aspects and advantages of the present invention will become apparent and easily understood from the description of the embodiments in conjunction with the following drawings, in which:

[0028] Figure 1 is the XRD diagram of the strontium titanate ceramics of Examples 1-4 of the present invention and Comparative Example 2;

[0029] Figure 2 is a SEM image of the strontium titanate ceramics of Examples 1-4 of the present invention;

[0030] Figure 3 1 is a dielectric spectrum analysis diagram of strontium titanate ceramics of Examples 1 to 4 of the present invention and Comparative Example 2;

[0031] Figure 4 This is a dielectric temperature spectrum analysis diagram of the strontium titanate ceramic sample of Example 1 of the present invention;

[0032] Figure 5 This is a dielectric temperature spectrum analysis diagram of the strontium titanate ceramic sample of Example 2 of the present invention;

[0033] Figure 6 This is a dielectric temperature spectrum analysis diagram of the strontium titanate ceramic sample of Example 3 of the present invention;

[0034] Figure 7 This is a dielectric temperature spectrum analysis diagram of the strontium titanate ceramic sample of Example 4 of the present invention. DETAILED DESCRIPTION

[0035] The embodiments of the present invention are described in detail below, which are intended to explain the present invention but should not be construed as limiting the present invention.

[0036] In one aspect of the present invention, the present invention provides a strontium titanate ceramic. According to an embodiment of the present invention, the strontium titanate ceramic chemical formula includes SrTiNb x O3, where 0<x≤0.012.

[0037] According to the strontium titanate ceramic of the above embodiment of the present invention, the chemical formula includes SrTiNb x O3, the inventors found that by introducing +5-valent Nb, defects are induced in the ST (SrTiO3) matrix, especially by controlling 0<x≤0.012, defect dipoles and defect dipole clusters can be further formed, thereby increasing the dielectric constant and producing a localized effect on free electrons, maintaining low dielectric loss. As a result, the strontium titanate ceramic has a high dielectric constant and maintains extremely low dielectric loss, which can meet the needs of use to a greater extent. Specifically, the dielectric constant of the strontium titanate ceramic can be 3.5×10 4 -6×10 4, the dielectric loss is less than 1%. Further, preferably, 0.003≤x≤0.006.

[0038] In another aspect of the present invention, the present invention provides a method for preparing the above-mentioned strontium titanate ceramic. According to an embodiment of the present invention, the method comprises:

[0039] S100: Mix strontium titanate raw materials and Nb2O5, grind and dry them

[0040] In this step, according to the specific chemical formula of strontium titanate ceramics, strontium titanate raw materials and Nb2O5 are accurately weighed and mixed, and then the above-mentioned mixture is ground and dried. Specifically, the grinding speed is 260r / min-300r / min, and the time is 12h-24h, so as to obtain a mixed material powder. Further, the strontium titanate raw material includes SrTiO3 and / or a mixture containing SrCO3 and TiO2. It should be noted that grinding and drying are conventional operations in this field, and those skilled in the art can select specific grinding types and drying process parameters according to actual conditions. For example, grinding adopts ball milling, that is, after the raw materials are prepared according to a certain ratio, the mixed material powder is obtained after wet ball milling mixing and drying. Specifically, the dispersant used in ball milling includes anhydrous ethanol or high-purity water, and the ball milling medium includes zirconia balls, steel balls, agate balls, etc., and the ball milling speed is 260r / min-300r / min.

[0041] S200: Calcine the mixed powder, grind and dry it

[0042] In this step, the mixed material powder is calcined, and the solid phase chemical reaction between the strontium titanate raw material and the ions in Nb2O5 is completed by diffusion under the action of heat, thereby obtaining a solid solution with a fixed composition and forming a main crystalline phase; at the same time, in this process, impurities such as volatile moisture in the raw material are removed, the purity of the porcelain material is improved, the second phase is avoided, the raw material particles are densified, and have a certain reactivity, which is conducive to obtaining a dense microstructure after sintering, and then the porcelain material obtained after calcination is ground and dried to obtain Nb-doped strontium titanate powder. It should be noted that grinding and drying are conventional operating methods in this field, and those skilled in the art can choose according to actual conditions, which will not be repeated here.

[0043] According to an embodiment of the present invention, the calcination temperature is 1100°C-1200°C, and the time is 2h-3h. The inventors found that the calcination temperature and time directly affect the fineness and activity of the ceramic powder, and the influence of the calcination temperature is more significant. Too high or too low temperature will cause the deterioration of the dielectric properties of the ceramic material. Therefore, the present application adopts a calcination process with a temperature of 1100°C-1200°C and a time of 2h-3h, which can improve the fineness and activity of Nb-doped strontium titanate powder. Furthermore, the grinding speed is 260r / min-300r / min, and the time is 12h-24h.

[0044] S300: Mix Nb-doped strontium titanate powder and binder, grind and sieve, dry press and then remove the binder

[0045] In this step, a proper amount of binder is added to the Nb-doped strontium titanate powder, which is fully ground and passed through a 130-170 mesh sieve, and then dry-pressed and debinded at a heating temperature of 600° C. to 650° C. for a holding time of 2 h to 3 h, thereby obtaining a ceramic green body. Specifically, the binder includes at least one of a 5wt% to 8wt% polyvinyl alcohol aqueous solution and a 5wt% to 8wt% polyvinyl butyral ester ethanol solution.

[0046] S400: Sintering the ceramic green body in a reducing atmosphere

[0047] In this step, the above-mentioned ceramic green body is sintered in a reducing atmosphere, and the Nb-doped strontium titanate powder is formed and begins to shrink after being heated to a certain temperature. At a temperature below the melting point, the particles interact and generate strength through material migration, and the sintering process can eliminate pores, and the grains grow evenly, thereby obtaining a dense ceramic block with a certain strength, achieving ceramic densification, and then preparing strontium titanate ceramics with high dielectric constant and low dielectric loss. Further, the reducing atmosphere includes at least one of N2, H2 / N2 mixed gas and H2 / Ar mixed gas, and the volume proportion of H2 in the H2 / N2 mixed gas is 1%-10%, and the volume proportion of H2 in the H2 / Ar mixed gas is 1%-10%.

[0048] According to an embodiment of the present invention, the sintering temperature is 1400°C-1450°C, and the time is 2h-3h. The inventors found that the control of sintering temperature and time has an important influence on the density of the particles, the size of the grains and the strength, thereby affecting the dielectric properties of the prepared strontium titanate ceramics. Specifically, if the sintering temperature is too high and the time is too long, local oversized grains may be formed, resulting in uneven grain size, and the ceramic sample may react with the support plate, which has an adverse effect on the final performance; if the sintering temperature is too low and the time is too short, the densification degree of the ceramic is not enough and the ceramic strength is insufficient. Therefore, the present application adopts a sintering condition of a temperature of 1400°C-1450°C and a time of 2h-3h, which can improve the height and density of strontium titanate ceramics, and then obtain strontium titanate ceramics with high dielectric constant and low dielectric loss.

[0049] Thus, the method can be used to prepare strontium titanate ceramics with high dielectric constant and low dielectric loss, and the method is simple in process, low in cost, good in repeatability and stable in performance. It should be noted that the characteristics and advantages described above for strontium titanate ceramics are also applicable to this method and will not be repeated here.

[0050] In a third aspect of the present invention, the present invention proposes the use of the above strontium titanate ceramic or the strontium titanate ceramic prepared by the above method in the fields of communication, radar or electronics.

[0051] The present invention is described below with reference to specific embodiments. It should be noted that these embodiments are merely illustrative and do not limit the present invention in any way.

[0052] Example 1

[0053] Preparation of SrTiNb 0.003 O3, the specific steps are as follows:

[0054] (1) According to SrTiNb 0.003 Weigh about 10g of raw materials SrTiO3 and Nb2O5 in a total of about 10g and add them to the ball mill, and the mass ratio of raw material powder: anhydrous ethanol: zirconium oxide ball is 1:4:15. After ball milling at a speed of 260r / min for 24 hours, separate the grinding balls and place the slurry on a heating table for drying. After drying, place the powder in a muffle furnace and calcine it at 1100℃ for 3 hours. After cooling, crush and grind it, and perform secondary ball milling to obtain Nb-doped strontium titanate powder. The secondary ball milling process is consistent with the primary ball milling process.

[0055] (2) Add an appropriate amount of 5% by mass PVA solution as a binder to the above-mentioned Nb-doped strontium titanate powder, with the addition ratio being about 1g of powder: 2 drops of binder, and grind it thoroughly for granulation. After grinding until the powder is fine and loose, pass it through a 150-mesh sieve, and put it into a mold for dry pressing to obtain Size of SrTiNb 0.003 O3 ceramic green disc.

[0056] (3) The ceramic green disc is placed in a muffle furnace and heated to 600°C at a heating rate of 2°C / min for 3 hours to fully debind, and then placed in a tube furnace and sintered at 1450°C for 3 hours in a 5% H2 / Ar atmosphere. During the sintering process, the atmosphere is always circulated in the tube furnace to obtain SrTiNb 0.003 O3 ceramics. After grinding and polishing the ceramic sample, silver electrode slurry was coated on both sides, and sintered at 600°C for 15 minutes to obtain a ceramic sample with uniform silver electrodes.

[0057] Example 2

[0058] The chemical formula of the strontium titanate ceramic prepared in Example 2 is SrTiNb 0.006 O3, weigh the raw materials SrTiO3 and Nb2O5 according to the chemical formula of strontium titanate ceramics, and the other preparation process conditions are the same as those in Example 1.

[0059] Example 3

[0060] The chemical formula of the strontium titanate ceramic prepared in Example 3 is SrTiNb 0.009 O3, weigh the raw materials SrTiO3 and Nb2O5 according to the chemical formula of strontium titanate ceramics, and the other preparation process conditions are the same as those in Example 1.

[0061] Example 4

[0062] The chemical formula of the strontium titanate ceramic prepared in Example 4 is SrTiNb 0.012 O3, weigh the raw materials SrTiO3 and Nb2O5 according to the chemical formula of strontium titanate ceramics, and the other preparation process conditions are the same as those in Example 1.

[0063] Comparative Example 1

[0064] The chemical formula of the strontium titanate ceramic prepared in Comparative Example 1 is SrTiNb 0.015 O3, weigh the raw materials SrTiO3 and Nb2O5 according to the chemical formula of strontium titanate ceramics, and the other preparation process conditions are the same as those in Example 1.

[0065] Comparative Example 2

[0066] Preparation of SrTiO3, the specific preparation method is as follows:

[0067] (a) Weigh about 10g of SrTiO3 raw material and add it into a ball mill, with the mass ratio of raw material powder: anhydrous ethanol: zirconium oxide ball being 1:4:15. After ball milling at a speed of 260r / min for 24 hours, separate the grinding balls and place the slurry on a heating table for drying. After drying, crush and grind to obtain undoped strontium titanate ceramic powder.

[0068] (b) Add an appropriate amount of 5% by mass PVA solution as a binder to the above strontium titanate ceramic powder, with the addition ratio being about 1g of powder: 2 drops of binder, and fully grind to granulate. After grinding until the powder is fine and loose, pass through a 150-mesh sieve, and put it into a mold for dry pressing to obtain SrTiO3 ceramic green disc of size.

[0069] (c) The ceramic green disc was placed in a muffle furnace and heated to 600°C at a heating rate of 2°C / min for 3 hours to fully debind, and then placed in a tube furnace and sintered at 1400°C for 3 hours in a 5% H2 / Ar atmosphere. During the sintering process, the atmosphere was always circulated in the tube furnace to obtain strontium titanate ceramics. After the ceramic sample was polished, silver electrode slurry was coated on both sides, and sintered at 600°C for 15 minutes to obtain a ceramic sample with uniform silver electrodes.

[0070] The properties of the strontium titanate ceramics of Examples 1-4 and Comparative Examples 1-2 were measured, as follows:

[0071] (1) XRD analysis was performed on the strontium titanate ceramics of Examples 1-4 and Comparative Example 2. The results are as follows: Figure 1 .from Figure 1 It can be seen that the strontium titanate ceramic samples of Examples 1-4 and Comparative Example 2 all have a single cubic perovskite structure without obvious impurity phases. Figure 1 (b) is a local enlarged view of the (110) diffraction peak. It can be seen that with the increase of Nb content, the (110) peak gradually shifts to the left, indicating that the lattice constant increases, proving that Nb with a larger ionic radius 5+ Entered the lattice and replaced Ti 4+ position, increasing the lattice constant.

[0072] (2) SEM analysis was performed on the strontium titanate ceramics of Examples 1-4. The results are as follows: Figure 2 .from Figure 2 It can be seen that the strontium titanate ceramic samples of Examples 1-4 all have a dense microstructure without obvious pores and second phases. Further analysis of the change in grain size shows that as the Nb content increases, the grain size gradually decreases, indicating that the introduction of Nb has a certain effect of inhibiting grain growth.

[0073] (3) The dielectric spectrum analysis was performed on the strontium titanate ceramic samples of Examples 1-4 and Comparative Example 2. The dielectric constants of the strontium titanate ceramics of Examples 1-4 and Comparative Example 2 varied with frequency as shown in FIG. Figure 3 As shown. Figure 3 It can be seen that the strontium titanate ceramic samples of Examples 1-4 and Comparative Example 2 all have excellent frequency stability, but Examples 1-4 have significantly increased dielectric constants compared to Comparative Example 2. The dielectric constant and dielectric loss data of Examples 1-4 and Comparative Example 1-2 tested at room temperature and 1 kHz are shown in Table 1.

[0074] Table 1

[0075]

[0076] It can be seen from Table 1 that the strontium titanate ceramic samples of Examples 1-4 not only have a higher dielectric constant, but also have extremely low dielectric loss. From the data of Comparative Example 2, it can be seen that with the increase in the amount of doped Nb element, the dielectric constant decreases and the dielectric loss increases.

[0077] The dielectric thermogram analysis of the strontium titanate ceramic samples of Examples 1-4 is shown in Figure 4-7 .from Figure 4-7 It can be seen that the strontium titanate ceramic samples of Examples 1-4 have good temperature stability in the low temperature range, and the dielectric constant and dielectric loss increase rapidly after exceeding a certain temperature range. Among them, the strontium titanate ceramic sample of Example 1 has the best temperature stability, with a dielectric constant change rate of less than 8% and a loss of less than 3% in the temperature range of -55°C-125°C.

[0078] In the description of this specification, the description with reference to the terms "one embodiment", "some embodiments", "example", "specific example", or "some examples" etc. means that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic representations of the above terms do not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described may be combined in any one or more embodiments or examples in a suitable manner. In addition, those skilled in the art may combine and combine the different embodiments or examples described in this specification and the features of the different embodiments or examples, without contradiction.

[0079] Although the embodiments of the present invention have been shown and described above, it is to be understood that the above embodiments are exemplary and are not to be construed as limitations of the present invention. A person skilled in the art may change, modify, replace and vary the above embodiments within the scope of the present invention.

Claims

1. A strontium titanate ceramic, characterized in that: The chemical formula includes SrTiNb x O3, wherein 0<x≤0.012; at room temperature and 1kHz, the dielectric constant of the strontium titanate ceramic is 3.5×10 4 -6×10 4 , dielectric loss is less than 1%; The preparation method of the strontium titanate ceramic comprises: (1) Mixing strontium titanate raw material and Nb2O5, grinding and drying to obtain a mixed material powder; (2) calcining the mixed material powder, grinding and drying it to obtain Nb-doped strontium titanate powder; (3) mixing the Nb-doped strontium titanate powder and the binder, grinding and sieving, dry pressing and then removing the binder to obtain a ceramic green body; (4) sintering the ceramic green body in a reducing atmosphere to obtain strontium titanate ceramics; In step (4), the sintering temperature is 1400°C-1450°C, and the sintering time is 2h-3h.

2. The strontium titanate ceramic according to claim 1, characterized in that: 0.003≤x≤0.006。 3. The strontium titanate ceramic according to claim 1, characterized in that: In step (1), the strontium titanate raw material includes SrTiO3 and / or a mixture of SrCO3 and TiO2; Optionally, the grinding speed is 260 r / min-300 r / min, and the grinding time is 12h-24h.

4. The strontium titanate ceramic according to claim 1, characterized in that: In step (2), the calcination temperature is 1100°C-1200°C and the time is 2h-3h; Optionally, the grinding speed is 260 r / min-300 r / min, and the grinding time is 12h-24h.

5. The strontium titanate ceramic according to claim 1, characterized in that: In step (3), the mesh size of the sieving is 130-170 mesh; Optionally, the binder comprises at least one of a 5wt%-8wt% polyvinyl alcohol aqueous solution and a 5wt%-8wt% polyvinyl butyral ethanol solution.

6. The strontium titanate ceramic according to claim 1, characterized in that: In step (3), the debinding temperature is 600°C-650°C, and the time is 2h-3h.

7. The strontium titanate ceramic according to claim 1, characterized in that: The reducing atmosphere includes at least one of a H2 / N2 mixed gas and a H2 / Ar mixed gas, wherein the volume proportion of H2 in the H2 / N2 mixed gas is 1%-10%, and the volume proportion of H2 in the H2 / Ar mixed gas is 1%-10%.

8. Use of the strontium titanate ceramic according to any one of claims 1 to 7 in the fields of communication, radar or electronics.

Citation Information

Patent Citations

  • Producing semiconductor strontium titanate particles

    CH669951A5

  • Ti-position high-valence substituted SrTiO3 giant dielectric ceramic and preparation method thereof

    CN105130421A

  • Ti-bit donor-acceptor co-doping SrTiO3 base high-dielectric ceramic and preparation method thereof

    CN105777112A

  • Sintered ceramic dielectric body

    US4058404A