A kind of hazardous waste-based high-strength lightweight aggregate and preparation method thereof

By combining hazardous waste and solid waste materials and drying, grinding, aging and high-temperature firing, high-strength lightweight aggregates are prepared, which solves the problems of low cylinder pressure strength and low resource utilization in the existing technology. Efficient solid waste resource utilization and low toxic leaching concentration are achieved.

CN116813369BActive Publication Date: 2024-10-18LIYANG SINOMA ENVIRONMENTAL PROTECTION CO LTD +1
View PDF 13 Cites 0 Cited by

Patent Information

Application Number
CN202310756337.4
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-06-26
Publication Date
2024-10-18
Estimated Expiration
2043-06-26

AI Technical Summary

Technical Problem

The existing hazardous waste-based lightweight aggregates have low cylinder compressive strength and low resource utilization, so they cannot achieve complete resource utilization of solid waste, and additional auxiliary materials such as fluxes and binders need to be added.

Method used

A combination of hazardous waste materials and solid waste materials is used, including aluminum ash, garbage incineration fly ash, electroplating sludge, oily sludge, etc. as hazardous waste materials, and construction spoil, contaminated soil, river sludge, domestic municipal sludge, etc. as solid waste materials. Waste materials are used to prepare high-strength lightweight aggregates through steps such as drying, grinding, screening, aging, granulation and high-temperature firing to reduce the use of auxiliary materials.

Benefits of technology

It achieves a cylinder pressure strength higher than 15MPa and a low toxic leaching concentration, realizes the harmlessness, reduction, and resource treatment of hazardous and solid waste, and avoids the need for additional auxiliary materials.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The present invention discloses a hazardous waste-based high-strength lightweight aggregate, which is composed of the following mass percentages: 10-40% hazardous waste materials and 60-90% solid waste materials; wherein the hazardous waste materials are a combination of at least three of aluminum ash, fly ash from garbage incineration, electroplating sludge or oily sludge, and the solid waste materials are a combination of at least three of construction waste, contaminated soil, river silt or municipal sludge. The present invention also discloses a method for preparing the above-mentioned hazardous waste-based high-strength lightweight aggregate. The raw materials used in the preparation of the lightweight aggregate of the present invention are all hazardous waste and solid waste, and there is no need to add additional auxiliary materials such as flux, binder, pore-forming agent, etc., which can achieve the harmless, reduced and resource-based treatment of a large amount of hazardous waste and solid waste. The lightweight aggregate prepared by the present invention can still maintain high cylinder pressure strength (23.16MPa) and low toxicity leaching concentration when the amount of hazardous waste added reaches 40%.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a hazardous waste-based high-strength lightweight aggregate and also relates to a preparation method of the hazardous waste-based high-strength lightweight aggregate. Background Art

[0002] Artificial lightweight aggregate is a common environmentally friendly building material on the market. It mainly includes clay ceramsite, shale ceramsite, expanded perlite, expanded vermiculite, expanded slag beads, zeolite lightweight aggregate, porous sintered material, coal slag and broken bricks, among which ceramsite is widely used due to its excellent performance.

[0003] The main raw materials for the production of traditional expanded clay and shale are non-renewable resources. Therefore, the use of solid waste with similar chemical composition to produce lightweight aggregates has become the mainstream research direction.

[0004] CN111517752B discloses a method for preparing sulfur-fixing ash ceramsite, which mainly uses sulfur-fixing ash, sludge, magma soil, tailings powder, aluminum ash powder, limestone powder, glass powder, and phosphate adhesive as raw materials, and realizes high-temperature sintering to obtain lightweight ceramsite with a cylinder pressure strength not exceeding 6.6MPa while using less high-temperature foaming agent and flux. Although this method eliminates a large amount of sulfur-fixing ash, sludge, and magma soil, the amount of hazardous waste bases in the raw materials is extremely small, the types are single, and the strength of the ceramsite produced is also low.

[0005] CN104402403B discloses a method for preparing high-strength ceramsite solidified with heavy metals from garbage incineration ash, which uses a large amount of garbage ash (60% to 80%), saline soil, glass powder, calcium carbonate, sodium carbonate, and water as raw materials, and is calcined and formed at a temperature below 1150°C. The leaching toxicity of the obtained ceramsite is much lower than the "Hazardous Waste Identification Standard and Hazardous Waste Landfill Standard", and the cylinder pressure strength can reach up to 10.52MPa. Although this method consumes a large amount of fly ash, the type of hazardous waste is single, and resources such as calcium carbonate, sodium carbonate, and water are used as auxiliary materials, which still has shortcomings in the efficient utilization of resources.

[0006] CN103241970B discloses a sintered expanded lightweight ceramsite produced from oily sludge and a manufacturing method thereof. The expanded lightweight ceramsite product is sintered using oily sludge, construction waste soil, waste residue from discarded energy-saving lamps, boiler waste residue, and wood processing waste residue as main raw materials, and calcium oxide, carboxymethyl cellulose, polycarboxylate high-efficiency water reducer, ferrous sulfate, magnesium sulfate, and water as auxiliary materials. The expanded lightweight ceramsite product is obtained by sintering, and the cylinder pressure strength is 3.85 MPa. The cylinder pressure strength is low, and the resource utilization rate is also low.

[0007] In summary, the current hazardous waste-based lightweight aggregate is prepared by only mixing single hazardous waste, with low cylinder pressure strength. At the same time, it also requires the consumption of auxiliary materials such as flux, binder, pore-forming agent, etc., and cannot achieve complete resource utilization of solid waste. Summary of the invention

[0008] Purpose of the invention: The purpose of the present invention is to provide a hazardous waste-based high-strength lightweight aggregate, the raw materials for the preparation of the lightweight aggregate are all hazardous waste materials and solid waste materials, which, on the one hand, realizes the complete resource utilization of solid waste, and on the other hand, the obtained lightweight aggregate has a cylinder compressive strength of not less than 15Mpa. Another purpose of the present invention is to provide a method for preparing the above-mentioned hazardous waste-based high-strength lightweight aggregate.

[0009] Technical solution: The hazardous waste-based high-strength lightweight aggregate described in the present invention is composed of the following components in percentage by mass: 10-40% hazardous waste materials and 60-90% solid waste materials; wherein the hazardous waste materials are a combination of at least three of aluminum ash, waste incineration fly ash, electroplating sludge or oily sludge, and the solid waste materials are a combination of at least three of construction waste, contaminated soil, river sludge or domestic municipal sludge.

[0010] The water content of the river sludge is 60%-80%. The water content of the river sludge can control the water-to-material ratio to 0.25-0.5, ensuring that the materials are completely mixed to form wet materials while not causing excessive moisture to cause granulation failure.

[0011] Among them, the hazardous waste-based high-strength lightweight aggregate is composed of the following components in mass percentage: 40% hazardous waste materials and 60% solid waste materials; wherein the hazardous waste materials are composed of the following components in mass percentage: 20% aluminum ash, 5% waste incineration fly ash, 6% electroplating sludge and 9% oil-containing sludge; the solid waste materials are composed of the following components in mass percentage: 4.8% construction waste soil, 8.4% contaminated soil, 42% river silt and 4.8% domestic municipal sludge.

[0012] The method for preparing the hazardous waste-based high-strength lightweight aggregate specifically comprises the following steps:

[0013] (1) Except for river sludge and domestic municipal sludge, all hazardous waste and solid waste materials are dried, ground and sieved; this method can ensure the mixing uniformity of the mixing process;

[0014] (2) Mixing the hazardous waste materials and solid waste materials in a prescribed amount, stirring them evenly to obtain a mixed wet material; the moisture in the wet material comes from river sludge and domestic municipal sludge;

[0015] (3) The mixed wet materials are aged at room temperature (the aging process is a homogenization process, which can achieve microscopic refinement and mixing of the raw materials, achieve full penetration, and make the composition of the mixed materials before roasting uniform and stable), and after aging, they are transported to a granulator to obtain spherical green embryos;

[0016] (4) conveying the spherical green embryo to a dryer and drying it for 1 to 3 hours using the residual heat from the rotary kiln, at a drying temperature of 105 to 350° C., so that the moisture content of the spherical green embryo is ≤ 3%. The staged heating effectively avoids cracking of the sphere during the firing process and improves the strength of the finished product.

[0017] (5) The dried spherical green embryo is sent to the end of the rotary kiln and fired at a temperature of 1050-1200°C for 10-25 minutes to obtain the required aggregate. If the firing temperature is too high, the sphere will be burned solid; if the firing temperature is not enough, the strength of the obtained ceramsite will be insufficient.

[0018] Wherein, in step (1), the dried material is sieved through a 200-mesh sieve.

[0019] Wherein, in step (3), the aging time is 1 to 2 days.

[0020] In step (3), the diameter of the spherical embryo is 5 to 15 mm, which can meet the needs of subsequent applications.

[0021] Wherein, in step (4), the drying temperature is 220°C.

[0022] In step (5), the fired aggregate balls enter a cooler, are cooled to below 80° C., and are graded, screened, and stored according to the size of the aggregate balls.

[0023] On the one hand, the hazardous waste used in the raw materials of the present invention can solidify the heavy metals in the hazardous waste into the ceramsite minerals through high-temperature sintering. On the other hand, the decomposition of organic matter in the hazardous waste can also help the ceramsite to form a porous expanded structure, thereby reducing the use of pore formers and expanders.

[0024] Beneficial effects: Compared with the prior art, the present invention has the following significant advantages: (1) The raw materials used in the preparation of lightweight aggregates by the present invention are all hazardous waste and solid waste, and there is no need to add additional auxiliary materials such as flux, binder, pore-forming agent, etc., which can achieve the harmless, reduced and resource-based treatment of a large amount of hazardous waste and solid waste; (2) The water content of river sludge and domestic municipal sludge is utilized, and there is no need to add additional water for preparation; (3) The lightweight aggregate prepared by the present invention can still maintain high cylinder pressure strength (23.16MPa) and low toxicity leaching concentration when the amount of hazardous waste added reaches 40%. DETAILED DESCRIPTION

[0025] Aluminum ash is secondary aluminum ash. In the embodiment, the aluminum ash comes from hazardous waste materials formed in the production process of Jiangsu Huilian Aluminum Co., Ltd.; waste incineration fly ash includes incineration fly ash of waste incineration power plants and bypass vent ash generated by the coordinated disposal of domestic waste in cement kilns. In the embodiment, the waste incineration fly ash comes from hazardous waste materials formed in the production process of Hubei Everbright Waste Incineration Power Generation Co., Ltd. and Jiangsu Tianshan Cement Group Co., Ltd.; electroplating sludge is electroplating tank slag, tank liquid and water treatment sludge in the electroplating industry. In the embodiment, the electroplating sludge comes from hazardous waste materials formed in the production process of Jiangsu Guoqiang Galvanizing Industrial Co., Ltd.; oily sludge is oily sludge generated by refinery wastewater treatment. In the embodiment, the oily sludge comes from hazardous waste materials formed in the production process of Jiangsu Yongbao Environmental Protection Technology Co., Ltd.; contaminated soil is contaminated soil formed by chemical agents, coking, and petroleum organic pollution. In the embodiment, the contaminated soil is soil polluted by the water discharged by Black Peony (Group) Co., Ltd.; construction waste is waste soil that does not contain bricks, tiles, and stones and has loose soil. In the embodiment, the construction waste comes from the construction waste soil generated by Nanjing Lugang Environmental Technology Co., Ltd. during the construction process.

[0026] Example 1

[0027] The hazardous waste-based high-strength lightweight aggregate of the present invention is composed of the following components in percentage by mass: 10% hazardous waste materials and 90% solid waste materials; wherein the hazardous waste materials are composed of the following components in percentage by mass: 7% aluminum ash, 2% fly ash from garbage incineration and 1% oily sludge; the solid waste materials are composed of the following components in percentage by mass: 19.8% contaminated soil, 63% river sludge and 7.2% domestic municipal sludge.

[0028] The method for preparing the hazardous waste-based high-strength lightweight aggregate specifically comprises the following steps:

[0029] (1) Put the formulated amount of aluminum ash, waste incineration fly ash, oily sludge and contaminated soil into a dryer, dry them using the residual heat from the rotary kiln, grind them and sieve them with a 200-mesh sieve to ensure uniform particle size;

[0030] (2) After screening, the dry material, river sludge, and domestic municipal sludge are placed in a vertical mixer and stirred to obtain a mixed wet material;

[0031] (3) The mixed wet materials are aged at room temperature for 1 day and conveyed by belt to a disc granulator to obtain spherical green embryos of 5 to 15 mm;

[0032] (4) The aggregate balls are conveyed by belt to a fluidized bed dryer, where the temperature is controlled to be 350°C and dried for 1 hour. The aggregate balls are then conveyed to the end of a rotary kiln, where the firing temperature is controlled to be 1200°C and fired for 10 minutes. The fired aggregate balls are discharged from the head of the kiln, enter a cooler and are rapidly cooled to below 80°C. The aggregate balls are then graded and screened according to their size and stored.

[0033] The bulk density of the obtained lightweight aggregate is 1000kg / m 3 , cylinder pressure strength is 25.24MPa, 1h water absorption rate is 4.9%, which meets the standard requirements of "Light Aggregate and Its Test Methods: Light Aggregate" (GB / T 17431.1-2010).

[0034] According to the "Determination of Leachable Heavy Metals in Cement Mortar" (GB / T 30810-2014), the leaching toxicity test of lightweight aggregate was carried out, and the heavy metal leaching concentrations were measured to be 0.003 mg / L for arsenic (As), 0.01 mg / L for lead (Pb), 0.004 mg / L for cadmium (Cd), 0.016 mg / L for chromium (Cr), 0.167 mg / L for copper (Cu), 0.049 mg / L for nickel (Ni), 0.201 mg / L for zinc (Zn), and 0.528 mg / L for manganese (Mn), which are lower than the leaching heavy metal content limits of "Technical Specifications for Co-treatment of Solid Waste in Cement Kilns" (GB 30760-2014).

[0035] Example 2

[0036] The hazardous waste-based high-strength lightweight aggregate of the present invention is composed of the following components in percentage by mass: 25% hazardous waste materials and 75% solid waste materials; wherein the hazardous waste materials are composed of the following components in percentage by mass: 15% aluminum ash, 2% fly ash from garbage incineration and 8% oily sludge; and the solid waste materials are composed of the following components in percentage by mass: 6% construction waste soil, 16.5% contaminated soil and 52.5% river sludge.

[0037] The method for preparing the hazardous waste-based high-strength lightweight aggregate specifically comprises the following steps:

[0038] (1) Put the formulated amount of aluminum ash, waste incineration fly ash, oily sludge, construction waste soil and contaminated soil into a dryer, dry them using the residual heat from the rotary kiln, grind them and sieve them with a 200-mesh sieve to ensure uniform particle size;

[0039] (2) After screening, the dry material, river sludge, and domestic municipal sludge are placed in a vertical mixer and stirred to obtain a mixed wet material;

[0040] (3) The mixed wet materials are aged at room temperature for 1 day and conveyed by belt to a disc granulator to obtain spherical green embryos of 5 to 15 mm;

[0041] (4) The aggregate balls are conveyed by belt to a fluidized bed dryer, where the temperature is controlled to be 350°C and dried for 1 hour. The aggregate balls are then conveyed to the end of a rotary kiln, where the firing temperature is controlled to be 1200°C and fired for 10 minutes. The fired aggregate balls are discharged from the head of the kiln, enter a cooler and are rapidly cooled to below 80°C. The aggregate balls are then graded and screened according to their size and stored.

[0042] The bulk density of the obtained lightweight aggregate is 1030kg / m 3 , cylinder pressure strength is 21.79MPa, 1h water absorption rate is 4.5%, which meets the standard requirements of "Light Aggregate and Its Test Methods: Light Aggregate" (GB / T 17431.1-2010).

[0043] According to the "Determination of Leachable Heavy Metals in Cement Mortar" (GB / T 30810-2014), the leaching toxicity test of lightweight aggregate was carried out, and the heavy metal leaching concentrations were measured to be 0.002 mg / L for arsenic (As), 0.02 mg / L for lead (Pb), 0.008 mg / L for cadmium (Cd), 0.021 mg / L for chromium (Cr), 0.118 mg / L for copper (Cu), 0.073 mg / L for nickel (Ni), 0.167 mg / L for zinc (Zn), and 0.69 mg / L for manganese (Mn), which are lower than the leaching heavy metal content limits of "Technical Specifications for Co-treatment of Solid Waste in Cement Kilns" (GB 30760-2014).

[0044] Example 3

[0045] The hazardous waste-based high-strength lightweight aggregate of the present invention is composed of the following components in percentage by mass: 40% of hazardous waste materials and 60% of solid waste materials; wherein the hazardous waste materials are composed of the following components in percentage by mass: 20% of aluminum ash, 5% of fly ash from garbage incineration, 6% of electroplating sludge and 9% of oily sludge; and the solid waste materials are composed of the following components in percentage by mass: 4.8% of construction waste soil, 8.4% of contaminated soil, 42% of river sludge and 4.8% of domestic municipal sludge.

[0046] The method for preparing the hazardous waste-based high-strength lightweight aggregate specifically comprises the following steps:

[0047] (1) Put the formulated amount of aluminum ash, waste incineration fly ash, electroplating sludge, oily sludge, construction waste soil and contaminated soil into a dryer, dry them using the residual heat from the rotary kiln, grind them and sieve them with a 200-mesh sieve to ensure uniform particle size;

[0048] (2) After screening, the dry material, river sludge, and domestic municipal sludge are placed in a vertical mixer and stirred to obtain a mixed wet material;

[0049] (3) The mixed wet materials are aged at room temperature for 2 days and conveyed by belt to a disc granulator to obtain spherical green embryos of 5 to 15 mm;

[0050] (4) The aggregate balls are conveyed by belt to a fluidized bed dryer, where the temperature is controlled at 105°C for 2 hours, and then conveyed to the end of a rotary kiln, where the firing temperature is controlled at 1050°C and fired for 25 minutes. The fired aggregate balls are discharged from the head of the kiln, enter a cooler and rapidly cooled to below 80°C, and are graded, screened and stored according to their size.

[0051] The bulk density of the obtained lightweight aggregate is 987kg / m 3 , cylinder pressure strength is 18.66MPa, 1h water absorption rate is 5.6%, which meets the standard requirements of "Light Aggregate and Its Test Methods: Light Aggregate" (GB / T 17431.1-2010).

[0052] According to the "Determination of Leachable Heavy Metals in Cement Mortar" (GB / T 30810-2014), the leaching toxicity test of lightweight aggregate was carried out, and the heavy metal leaching concentrations were measured to be 0.007 mg / L for arsenic (As), 0.054 mg / L for lead (Pb), 0.025 mg / L for cadmium (Cd), 0.047 mg / L for chromium (Cr), 0.137 mg / L for copper (Cu), 0.032 mg / L for nickel (Ni), 0.195 mg / L for zinc (Zn), and 0.687 mg / L for manganese (Mn), which are lower than the leaching heavy metal content limits of "Technical Specifications for Co-treatment of Solid Waste in Cement Kilns" (GB 30760-2014).

[0053] Example 4

[0054] The hazardous waste-based high-strength lightweight aggregate of the present invention is composed of the following components in percentage by mass: 40% of hazardous waste materials and 60% of solid waste materials; wherein the hazardous waste materials are composed of the following components in percentage by mass: 20% of aluminum ash, 5% of fly ash from garbage incineration, 6% of electroplating sludge and 9% of oily sludge; and the solid waste materials are composed of the following components in percentage by mass: 4.8% of construction waste soil, 8.4% of contaminated soil, 42% of river sludge and 4.8% of domestic municipal sludge.

[0055] The method for preparing the hazardous waste-based high-strength lightweight aggregate specifically comprises the following steps:

[0056] (1) Put the formulated amount of aluminum ash, waste incineration fly ash, electroplating sludge, oily sludge, construction waste soil and contaminated soil into a dryer, dry them using the residual heat from the rotary kiln, grind them and sieve them with a 200-mesh sieve to ensure uniform particle size;

[0057] (2) After screening, the dry material, river sludge, and domestic municipal sludge are placed in a vertical mixer and stirred to obtain a mixed wet material;

[0058] (3) The mixed wet materials are aged at room temperature for 2 days and conveyed by belt to a disc granulator to obtain spherical green embryos of 5 to 15 mm;

[0059] (4) The aggregate balls are conveyed by belt to a fluidized bed dryer, where the temperature is controlled at 350°C for 1 hour, and then conveyed to the tail of a rotary kiln, where the firing temperature is controlled at 1200°C and fired for 15 minutes. The fired aggregate balls are discharged from the head of the kiln, enter a cooler and are rapidly cooled to below 80°C, and are graded, screened and stored according to their size.

[0060] The bulk density of the obtained lightweight aggregate is 1080kg / m 3 , cylinder pressure strength is 24.35MPa, 1h water absorption rate is 3.5%, which meets the standard requirements of "Light Aggregate and Its Test Methods: Light Aggregate" (GB / T 17431.1-2010).

[0061] According to the "Determination of Leachable Heavy Metals in Cement Mortar" (GB / T 30810-2014), the leaching toxicity test of lightweight aggregate was carried out, and the heavy metal leaching concentration was measured: the heavy metal leaching concentration measured was: arsenic (As) was not detected, lead (Pb) was 0.022 mg / L, cadmium (Cd) was 0.005 mg / L, chromium (Cr) was 0.012 mg / L, copper (Cu) was 0.013 mg / L, nickel (Ni) was 0.058 mg / L, zinc (Zn) was 0.192 mg / L, and manganese (Mn) was 0.177 mg / L, which were lower than the leaching heavy metal content limits of "Technical Specifications for Co-treatment of Solid Waste in Cement Kilns" (GB 30760-2014).

[0062] When the two-stage heating temperature increases, the cylinder compressive strength of the aggregate increases significantly, while the toxic leaching concentration decreases significantly.

[0063] Example 5

[0064] The hazardous waste-based high-strength lightweight aggregate of the present invention is composed of the following components in percentage by mass: 40% hazardous waste materials and 60% solid waste materials; wherein the hazardous waste materials are composed of the following components in percentage by mass: 20% aluminum ash, 5% waste incineration fly ash, 6% electroplating sludge and 9% oily sludge; the solid waste materials are composed of the following components in percentage by mass: 13.2% contaminated soil, 42% river sludge and 4.8% domestic municipal sludge.

[0065] The method for preparing the hazardous waste-based high-strength lightweight aggregate specifically comprises the following steps:

[0066] (1) Put the formulated amount of aluminum ash, waste incineration fly ash, electroplating sludge, oily sludge and contaminated soil into a dryer, dry them using the residual heat from the rotary kiln, grind them and sieve them with a 200-mesh sieve to ensure uniform particle size;

[0067] (2) After screening, the dry material, river sludge, and domestic municipal sludge are placed in a vertical mixer and stirred to obtain a mixed wet material;

[0068] (3) The mixed wet materials are aged at room temperature for 2 days and conveyed by belt to a disc granulator to obtain spherical green embryos of 5 to 15 mm;

[0069] (4) The aggregate balls are conveyed by belt to a fluidized bed dryer, where the temperature is controlled at 350°C for 1 hour, and then conveyed to the tail of a rotary kiln, where the firing temperature is controlled at 1200°C and fired for 15 minutes. The fired aggregate balls are discharged from the head of the kiln, enter a cooler and are rapidly cooled to below 80°C, and are graded, screened and stored according to their size.

[0070] The bulk density of the obtained lightweight aggregate is 1050kg / m 3 , cylinder pressure strength is 20.49MPa, 1h water absorption rate is 4.2%, which meets the standard requirements of "Light Aggregate and Its Test Methods: Light Aggregate" (GB / T 17431.1-2010).

[0071] According to the "Determination of Leachable Heavy Metals in Cement Mortar" (GB / T 30810-2014), the leaching toxicity test of lightweight aggregate was carried out, and the heavy metal leaching concentrations were measured to be 0.005 mg / L for arsenic (As), 0.025 mg / L for lead (Pb), 0.018 mg / L for cadmium (Cd), 0.021 mg / L for chromium (Cr), 0.213 mg / L for copper (Cu), 0.058 mg / L for nickel (Ni), 0.152 mg / L for zinc (Zn), and 0.434 mg / L for manganese (Mn), which are lower than the leaching heavy metal content limits of "Technical Specifications for Co-treatment of Solid Waste in Cement Kilns" (GB 30760-2014).

[0072] In Example 5, the content of contaminated soil increased and the content of construction waste soil decreased. Since the contaminated soil contains more organic matter, there are more pores during the sintering process and the strength will decrease; and the contaminated soil has more heavy metals, which also affects leaching.

[0073] Example 6

[0074] The hazardous waste-based high-strength lightweight aggregate of the present invention is composed of the following components in percentage by mass: 40% hazardous waste materials and 60% solid waste materials; wherein the hazardous waste materials are composed of the following components in percentage by mass: 20% aluminum ash, 5% fly ash from garbage incineration, and 15% oily sludge; the solid waste materials are composed of the following components in percentage by mass: 4.8% construction waste soil, 8.4% contaminated soil, 42% river sludge, and 4.8% domestic municipal sludge.

[0075] The method for preparing the hazardous waste-based high-strength lightweight aggregate specifically comprises the following steps:

[0076] (1) Put the formulated amount of aluminum ash, waste incineration fly ash, electroplating sludge, oily sludge and contaminated soil into a dryer, dry them using the residual heat from the rotary kiln, grind them and sieve them with a 200-mesh sieve to ensure uniform particle size;

[0077] (2) After screening, the dry material, river sludge, and domestic municipal sludge are placed in a vertical mixer and stirred to obtain a mixed wet material;

[0078] (3) The mixed wet materials are aged at room temperature for 2 days and conveyed by belt to a disc granulator to obtain spherical green embryos of 5 to 15 mm;

[0079] (4) The aggregate balls are conveyed by belt to a fluidized bed dryer, where the temperature is controlled at 350°C for 1 hour, and then conveyed to the tail of a rotary kiln, where the firing temperature is controlled at 1200°C and fired for 15 minutes. The fired aggregate balls are discharged from the head of the kiln, enter a cooler and are rapidly cooled to below 80°C, and are graded, screened and stored according to their size.

[0080] The bulk density of the obtained lightweight aggregate is 1060kg / m 3 , cylinder pressure strength is 23.16MPa, 1h water absorption rate is 3.8%, which meets the standard requirements of "Light Aggregate and Its Test Methods: Light Aggregate" (GB / T 17431.1-2010).

[0081] According to the "Determination of Leachable Heavy Metals in Cement Mortar" (GB / T 30810-2014), the leaching toxicity test of lightweight aggregate was carried out, and the heavy metal leaching concentrations were measured as arsenic (As) was not detected, lead (Pb) was not detected, cadmium (Cd) was 0.001 mg / L, chromium (Cr) was 0.026 mg / L, copper (Cu) was 0.007 mg / L, nickel (Ni) was 0.035 mg / L, zinc (Zn) was 0.104 mg / L, and manganese (Mn) was 0.124 mg / L, which are lower than the leaching heavy metal content limits of the "Technical Specifications for Co-treatment of Solid Waste in Cement Kilns" (GB 30760-2014).

[0082] In Example 6, the oily sludge has more organic matter, reduced strength and increased porosity; the oily sludge has less heavy metal content than the electroplating sludge and has less impact on leaching toxicity.

Claims

1. A hazardous waste-based high-strength lightweight aggregate, It is characterized in that The hazardous waste-based high-strength lightweight aggregate is composed of the following components in mass percentage: 40% hazardous waste materials and 60% solid waste materials; wherein the hazardous waste materials are composed of the following components in mass percentage: 20% aluminum ash, 5% waste incineration fly ash, 6% electroplating sludge and 9% oily sludge; the solid waste materials are composed of the following components in mass percentage: 4.8% construction waste soil, 8.4% contaminated soil, 42% river sludge and 4.8% domestic municipal sludge; the water content of the river sludge is 60% to 80%; The method for preparing the hazardous waste-based high-strength lightweight aggregate specifically comprises the following steps: (1) Put the formulated amount of aluminum ash, waste incineration fly ash, electroplating sludge, oily sludge, construction waste soil and contaminated soil into a dryer, dry them using the residual heat from the rotary kiln, grind them and sieve them with a 200-mesh sieve to ensure uniform particle size; (2) After screening, the dry material, river sludge, and domestic municipal sludge are placed in a vertical mixer and stirred evenly to obtain a mixed wet material; (3) The mixed wet materials are aged at room temperature for 2 days and conveyed to a disc granulator by belt conveyor to obtain spherical green bodies with a diameter of 5 to 15 mm; (4) The aggregate balls are conveyed to the fluidized bed dryer with a controlled temperature of 350°C for 1 hour, and then conveyed to the tail of the rotary kiln with a controlled firing temperature of 1200°C for 15 minutes. The fired aggregate balls are discharged from the head of the kiln and enter the cooler to be rapidly cooled to below 80°C.

2. The hazardous waste-based high-strength lightweight aggregate according to claim 1, Features: In step (4), the moisture content of the spherical green body after drying is ≤3%.

Citation Information

Patent Citations

  • Sintering expansion type light ceramsite produced by using oily sludge and manufacture method of sintering expansion type light ceramsite

    CN103241970B

  • A preparation method of high-strength ceramsite solidified by waste incineration ash

    CN104402403B

  • Sulfur-fixing ceramsite and its preparation method

    CN111517752B

  • Method for preparing ceramsite by utilizing dried sludge and burnt fly ash

    CN102060426A

  • Harmless treatment method for garbage incinerating fly ash and product produced in harmless treatment method

    CN102320855A