A folded three-dimensional MoS2 field-effect transistor and its fabrication method

By constructing a folded three-dimensional structure MoS2 field-effect transistor and adopting a "convex" shaped buried gate and gold semi-contact architecture, the problems of short-channel effect and excessive power consumption in ultra-small MoS2 field-effect transistors are solved, realizing a low-power and high-performance transistor device.

CN116825643BActive Publication Date: 2026-11-17QINGDAO UNIV
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
CN202310982407.8
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-08-04
Publication Date
2026-11-17
Estimated Expiration
2043-08-04

AI Technical Summary

Technical Problem

Existing technologies struggle to effectively suppress short-channel effects and regulate threshold voltage in extremely small MoS2 field-effect transistors, resulting in excessively high device power consumption and failing to meet low-power requirements.

Method used

A folded three-dimensional structure MoS2 field-effect transistor is adopted. By constructing a "convex" shaped buried gate structure and a gold-semiconductor contact architecture, the vertical channel length is increased. Combined with the high work function metal gate and the Schottky contact of the MoS2 channel, impurity scattering during atomic layer deposition is avoided, thus achieving effective control of the MoS2 channel.

Benefits of technology

It effectively suppresses short-channel effects, reduces gate leakage current and static power consumption, improves device density and electrical performance, and meets low power consumption requirements.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116825643B_ABST
    Figure CN116825643B_ABST
Patent Text Reader

Abstract

This invention relates to a method for fabricating a folded three-dimensional MoS2 field-effect transistor, comprising the following steps: S1. Substrate preparation; S2. Ultraviolet photolithography of a "convex" shaped buried metal gate pattern; S3. Vacuum thermal evaporation of the buried metal gate; S4. Mechanical lift-off of the MoS2 thin film; S5. MoS2 thin film slicing; S6. Electron beam exposure of source and drain electrodes; S7. Vacuum thermal evaporation of source and drain electrodes. This invention employs a non-planar folded three-dimensional "convex" shaped buried gate structure, increasing the effective channel length in the vertical direction, thereby suppressing the short-channel effect of extremely small field-effect transistors. Combined with a gold-semiconductor contact buried gate architecture, no additional atomic layer deposition of the gate insulating dielectric is required, ensuring the quality of the MoS2 channel interface, maintaining the device's electrical performance, improving the quality of the metal gate / MoS2 Schottky interface, and solving the performance degradation of extremely small two-dimensional semiconductor field-effect transistors caused by impurity scattering at the channel interface.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the fields of semiconductor materials technology and integrated circuit architecture technology, and in particular to a method for fabricating a folded three-dimensional MoS2 field-effect transistor. Background Technology

[0002] In the modern integrated circuit industry, the number of transistors per unit area on a chip increases dramatically with the shrinking of process nodes, leading to increasingly severe cumulative power loss problems for transistor devices per unit area. Constructing field-effect transistors with low threshold voltages, suppressing gate leakage current, and achieving near-ideal subthreshold swing are crucial for reducing power loss in extremely small field-effect transistor devices. However, existing research on extremely small MoS2 field-effect transistors cannot meet the stringent requirements of low-power field-effect transistor devices.

[0003] In existing technologies, silicon-based configurations are mature and exhibit better gate control capabilities, effectively suppressing short-channel effects in transistor devices. However, on the one hand, because the sub-nanometer-thick atomic layer structure of two-dimensional semiconductors is particularly sensitive to factors such as the interface environment, the atomic layer deposition techniques used in directly constructing two-dimensional semiconductor FinFETs or gate-all-around-around-around-FETs can severely affect the channel interface of the two-dimensional semiconductor, leading to a decrease in the electrical performance of the device itself. On the other hand, conventional MoS2 metal-oxide-semiconductor field-effect transistors (MOSFETs) based on MOS structures are typically depletion-mode devices, and their threshold voltage is difficult to adjust effectively, resulting in more severe static power loss problems, which is detrimental to their future application in the large-scale integrated circuit industry.

[0004] Therefore, further research is needed to realize high-performance, low-power, ultra-small two-dimensional semiconductor transistor devices. New ultra-small two-dimensional semiconductor transistor device configurations are required that can perfectly guarantee the interface quality of the two-dimensional semiconductor channel and effectively suppress the short-channel effect. Summary of the Invention

[0005] To address the shortcomings of existing technologies, this invention provides a folded three-dimensional MoS2 field-effect transistor and its fabrication method. This invention employs a non-planar folded three-dimensional "convex"-shaped buried gate structure, increasing the effective channel length in the vertical direction, thereby suppressing the short-channel effect of extremely small field-effect transistors. Combined with a gold-semiconductor contact buried gate architecture, no additional atomic layer deposition of the gate insulating dielectric is required, ensuring the quality of the MoS2 channel interface, maintaining the device's electrical performance, improving the metal gate / MoS2 Schottky interface quality, and solving the performance degradation of extremely small two-dimensional semiconductor field-effect transistors caused by impurity scattering at the channel interface.

[0006] To achieve this objective, the present invention adopts the following technical solution:

[0007] In a first aspect, the present invention provides a method for fabricating a folded three-dimensional structure MoS₂ field effect transistor, comprising the following fabrication steps:

[0008] S1. Substrate preparation;

[0009] S2. Ultraviolet lithography of a "convex"-shaped buried metal gate pattern;

[0010] S3. Vacuum thermal evaporation of the buried metal gate;

[0011] S4. Mechanical exfoliation of MoS₂ thin film;

[0012] S5. MoS₂ thin film segmentation;

[0013] S6. Electron beam lithography of source and drain electrodes;

[0014] S7. Vacuum thermal evaporation of the source and drain electrodes.

[0015] Further, the substrate in step S1 is the SiO₂ side of P-type low-resistance silicon with one side polished and one side oxidized, a diamond scriber is used to cut the substrate into a size of 1cm×1cm, the substrate is ultrasonically cleaned sequentially with acetone and isopropanol, then rinsed with deionized water and blown dry with high-purity nitrogen.

[0016] Further, in the step S2 of ultraviolet lithography of the "convex"-shaped buried metal gate pattern, the substrate obtained in S1 is placed on a spin coater, photoresist is spin-coated on the SiO₂ layer for homogenization treatment, and then placed on a hot plate for baking to cure the photoresist; then the substrate is placed in an ultraviolet lithography apparatus for ultraviolet irradiation under a dedicated mask, the sample is taken out and placed on the hot plate for baking, then the sample is placed again in the ultraviolet lithography apparatus for ultraviolet irradiation in a maskless state, and after the sample is taken out, it is rinsed sequentially with developer and deionized water, and then blown dry with high-purity nitrogen.

[0017] Further, in the step S3 of vacuum thermal evaporation of the buried metal gate, high work function metal platinum is placed on a tungsten boat; the sample prepared in S2 is placed into an evaporation chamber, which is pumped to a vacuum degree lower than 1*10-4pa; the tungsten boat is heated with a 270A current to melt the platinum on the tungsten boat at a rate of 0.1- to be evaporated onto the sample after the lithography treatment in S2, to form a 60-80nm thick "convex"-shaped buried gate; after the evaporation is completed, the excess metal outside the gate is removed by rinsing with acetone and isopropanol respectively, followed by rinsing with deionized water and blowing dry with high-purity nitrogen.

[0018] Furthermore, in step S4, the MoS2 film is mechanically peeled off. Metal-assisted mechanical peeling technology is used to mechanically peel off the bulk MoS2 material into a single-layer two-dimensional semiconductor at the millimeter level. The sample obtained in S3 is placed on a transfer platform, and the mechanically peeled MoS2 film is transferred to a "convex" shaped metal buried gate electrode using a fixed-point physical transfer process. The sample is then left to stand for 90-120 seconds.

[0019] Furthermore, in step S5, MoS2 film segmentation, ultraviolet lithography is used in conjunction with CF4 reactive ion etching technology to cut and segment the millimeter-scale MoS2 film to form independent channels. After etching, the prepared sample is placed on a spin coater and photoresist is spin-coated onto the sample for homogenization. Then, the sample is placed on a baking tray for baking to cure the photoresist.

[0020] Furthermore, in step S6, the source and drain electrodes are exposed by electron beam exposure. The sample obtained in S5 is photographed under an optical microscope, and the source and drain electrodes are patterned using an electron beam exposure system. The processed sample is placed in the electron beam exposure system, and the source and drain electrode areas are patterned using electron beam exposure technology. After exposure, the sample is taken out and rinsed with developer and isopropanol, then rinsed with deionized water, and dried with high-purity nitrogen to complete the patterned design of the source and drain electrodes.

[0021] Furthermore, in step S7, vacuum thermal evaporation of the source and drain electrodes, metallic indium is placed in a tungsten boat as the source and drain electrode material. The sample treated in S6 is placed in the evaporation chamber, and a vacuum of 1*10-4 Pa is applied. The tungsten boat is heated with a current of 60 A to melt the indium and then... The source and drain electrodes are deposited onto the substrate at a rate of 10-30 nm. After the deposition is completed, the excess metal outside the source and drain electrodes is removed by rinsing with acetone and isopropanol, respectively, and then rinsed with deionized water and dried with high-purity nitrogen.

[0022] In a second aspect, the present invention provides a folded three-dimensional MoS2 field-effect transistor prepared by the method described in the first aspect.

[0023] Thirdly, the present invention provides a folded three-dimensional structure MoS2 field-effect transistor, including a substrate, a high work function buried metal gate, a MoS2 thin film, and source / drain electrodes. The MoS2 thin film and the source / drain electrodes form a bottom-up "convex" structure. The high work function buried metal gate is placed at the middle of the bottom surface of the MoS2 thin film to form a Schottky contact, so that the transistor does not need to be inserted into a dielectric layer and has good rectification and capacitance characteristics. The source / drain electrodes are respectively placed at both ends of the top surface of the MoS2 thin film to form an ohmic contact, so that the contact resistance between the source / drain electrodes and MoS2 is extremely small and will not affect the electrical performance of the transistor.

[0024] The present invention has the following advantages:

[0025] 1. This invention, in the design of extremely small devices, innovatively expands the planar channel of the two-dimensional semiconductor MoS2 into a three-dimensional pleated form by constructing a folded three-dimensional structure and combining it with a buried metal gate. This is equivalent to increasing the effective channel length for the same layout area, which can both reduce the short-channel effect of field-effect transistors of the same size and increase device density.

[0026] 2. In terms of gate structure design, this invention utilizes a high work function metal / MoS2 Schottky barrier contact structure as the gate to achieve effective control of the MoS2 channel. By matching different high work function metal gate and MoS2 channel layer thicknesses, the transistor threshold voltage is adjusted, the gate leakage current is reduced, and an enhancement-mode MoS2 short-channel device is realized, thereby reducing the device's static power consumption loss.

[0027] 3. This invention eliminates the need to deposit an insulating gate dielectric on the MoS2 surface, thereby avoiding the introduction of impurity scattering during atomic layer deposition and ensuring that device performance does not degrade.

[0028] 4. This invention explores the influence mechanism of local strain on carrier transport in MoS2 under a "convex" gate architecture. It elucidates the potential changes in the local multi-valley band structure, the shift between exciton spin-allowed and spin-forbidden states, the scattering changes of exciton-phonon intervalleys, and the changes in exciton coherence. This provides theoretical support for the modification of carrier transport characteristics caused by strain in two-dimensional semiconductors. Attached Figure Description

[0029] To more clearly illustrate the technical solutions in the embodiments of the present invention or the prior art, the drawings used in the description of the embodiments or the prior art will be briefly introduced below. Obviously, the drawings described below are only one embodiment of the present invention. For those skilled in the art, other embodiments can be derived from the provided drawings without creative effort.

[0030] Figure 1 : A schematic diagram of the structure of the present invention;

[0031] Figure 2 Top view of the structure of this invention;

[0032] Figure 3 : A three-dimensional view of the structure of the present invention;

[0033] Figure 4 : A front view of the structure of this invention;

[0034] Figure 5 : Left view of the structure of this invention.

[0035] Figure 6 The transfer characteristic curve of the folded three-dimensional structure MoS2 field-effect transistor of the present invention.

[0036] Figure 7 Transfer characteristic curves of conventional MoS2 metal-oxide-semiconductor field-effect transistors (MOSFETs).

[0037] Figure 8 The rectification characteristic curve of the folded three-dimensional structure MoS2 field-effect transistor of the present invention.

[0038] Figure 9 Rectification characteristic curve of a conventional MoS2 MOSFET.

[0039] Figure 10 The subthreshold swing curve of the folded three-dimensional structure MoS2 field-effect transistor of this invention.

[0040] Figure 11 Subthreshold swing curve of a conventional MoS2 MOSFET.

[0041] Labeling Explanation: 1. Source / Drain Electrode, 2. MoS2 Thin Film, 3. High Work Function Buried Metal Gate, 4. SiO2, 5. P-type Low-Resistivity Silicon Detailed Implementation

[0042] The present invention will be further described below with reference to the accompanying drawings and examples:

[0043] Embodiments of the present invention are described in detail below. Examples of these embodiments are shown in the accompanying drawings, wherein the same or similar reference numerals denote the same or similar elements or elements having the same or similar functions throughout. The embodiments described below with reference to the accompanying drawings are exemplary and are only used to explain the present invention, and should not be construed as limiting the present invention.

[0044] In the description of this invention, it should be noted that, unless otherwise explicitly specified and limited, the terms "installation," "connection," and "joining" should be interpreted broadly. For example, they can refer to a fixed connection, a detachable connection, or an integral connection; they can refer to a direct connection or an indirect connection through an intermediate medium. Those skilled in the art can understand the specific meaning of the above terms in this invention based on the specific circumstances.

[0045] In the description of this invention, it should be understood that the terms "upper", "lower", "front", "rear", "left", "right", "vertical", "horizontal", "top", "bottom", "inner", "outer", etc., indicate the orientation or positional relationship based on the orientation or positional relationship shown in the accompanying drawings. They are only for the convenience of describing this invention and simplifying the description, and do not indicate or imply that the device or element referred to must have a specific orientation, or be constructed and operated in a specific orientation. Therefore, they should not be construed as limitations on this invention.

[0046] Example 1:

[0047] This invention provides a method for fabricating a folded three-dimensional MoS2 field-effect transistor, comprising the following steps:

[0048] S1: Substrate preparation:

[0049] A single-sided polished, single-sided oxidized P-type low-resistivity silicon SiO2 surface was used as the substrate. A 1cm×1cm substrate was cut out with a diamond pen. The substrate was ultrasonically cleaned with acetone and isopropanol in sequence, then rinsed with deionized water and dried with high-purity nitrogen.

[0050] S2: Ultraviolet photolithography of a "convex" shaped embedded metal grid pattern:

[0051] Place the substrate prepared in S1 on a spin coater and spin coat the photoresist onto the SiO2 layer. Spin coat the photoresist at a slow speed of 300-500 rpm for 15-30 seconds, then spin coat the photoresist at a high speed of 4000-6000 rpm for 60-90 seconds. After that, place the sample on a baking tray and bake at 90-120℃ for 1-5 minutes to cure the photoresist.

[0052] The spin-coated photoresist sample is placed in a UV lithography apparatus and irradiated with UV light for 3-5 seconds under a dedicated mask. The sample is then removed and baked at 100-120℃ for 90-120 seconds. Next, the sample is placed back in the UV lithography apparatus without a mask and irradiated with UV light for 40-50 seconds. After removal, the sample is rinsed sequentially with developer and deionized water for 40-60 seconds, and then dried with high-purity nitrogen gas. This completes the patterning design of the "convex" shaped buried metal gate electrode.

[0053] S3: Vacuum thermally deposited metal buried gate:

[0054] Platinum (Pt), a high work function metal, was placed on a tungsten boat; the sample prepared by S2 was placed in an evaporation chamber, and the vacuum level was reduced to below 1 × 10⁻⁴ Pa; the tungsten boat was heated using a current of 270 A to melt the platinum on it, and then... The evaporation rate is applied to the sample after S2 photolithography to deposit a 60-80nm "convex" shaped buried gate. After the evaporation is completed, the excess metal outside the gate is removed by rinsing with acetone and isopropanol, respectively, and then rinsed with deionized water and dried with high-purity nitrogen.

[0055] Optionally, the high work function metal platinum (Pt) used in the above steps can also be other high work function metals such as gold (Au) or nickel (Ni).

[0056] The above steps form the gold-semiconductor contact architecture design: when fabricating the buried metal gate, a high work function metal such as platinum (Pt) is selected, and the metal gate has an extremely narrow width and an extremely high height. This allows the planar MoS2 to be bent and folded in the Z-axis space, increasing the effective channel length within the same layout area. This can suppress the short-channel effect and improve device density. A perfect Schottky barrier contact interface between the metal gate and the MoS2 channel is constructed to reduce the impact of interface impurity scattering on device performance. A built-in potential and channel depletion region are formed at the interface. By effectively controlling the width of the channel depletion region, the transport of charge carriers in the channel is ultimately controlled.

[0057] S4: Mechanical peeling of MoS2 film:

[0058] Metal-assisted mechanical exfoliation (MAMEI) technology was used to mechanically exfoliate bulk MoS2 material into millimeter-scale single-layer two-dimensional semiconductors. The transfer platform was preheated to 30-50°C, and the S3 sample was placed on the platform. The mechanically exfoliated MoS2 film was then transferred onto a convex-shaped buried metal gate electrode using a point-to-point physical transfer process. After waiting 90-120 seconds, the MoS2 and buried metal gate were allowed to bond more tightly, achieving perfect Schottky interface contact between the MoS2 channel and the convex-shaped high work function buried metal gate. This effectively avoided the introduction of impurities and the Fermi level pinning effect, resulting in a large Schottky barrier height.

[0059] The above steps form a three-dimensional architecture, shaping the planar MoS2 thin film around a convex buried gate. Within a limited gate length, this increases the number of gate-controlled MoS2 semiconductor channels along the Z-axis, effectively suppressing the short-channel effect in extremely small MoS2 field-effect transistor devices. Furthermore, it eliminates the need for an insulating dielectric layer on the gate oxide and redundant etching processes, ensuring a perfect channel interface and maintaining stable electrical performance.

[0060] S5: MoS2 film segmentation:

[0061] Using ultraviolet lithography combined with CF4 reactive ion etching, millimeter-scale MoS2 films are cut and segmented to form independent channels. Because the etched areas are where the MoS2 films will be isolated and insulated, and do not participate in device current transmission, damage caused by the etching boundaries will not affect the performance of the MoS2 films. After etching, the prepared samples are placed on a spin coater, and photoresist is spin-coated onto the samples. The spin coater is then used for slow spin coating at 300-500 rpm for 15-30 seconds, followed by high spin coating at 4000-6000 rpm for 60-90 seconds. Finally, the samples are placed in a baking oven at 90-120℃ for 3-5 minutes to cure the photoresist.

[0062] S6: Electron beam exposure source drain electrode:

[0063] The S5 sample was photographed under an optical microscope, and the source and drain electrodes were patterned using an electron beam exposure system. The processed sample was placed in the electron beam exposure system with the current adjusted to 2.1 nA, and the source and drain electrode regions were patterned using electron beam exposure technology. After exposure, the sample was removed and rinsed with developer and isopropanol for 15-45 seconds, then rinsed with deionized water and dried with high-purity nitrogen gas, completing the patterned design of the source and drain electrodes.

[0064] S7: Vacuum thermal evaporation source and drain electrodes:

[0065] Low-melting-point metallic indium (In) was placed in a tungsten boat as the source and drain electrode material. The S6-treated sample was placed in the evaporation chamber, and the vacuum was evacuated to 1*10-4 Pa. The tungsten boat was heated with a current of 60 A to melt the indium and then evaporate it at 0.3- The source and drain electrodes, measuring 10-30 nm, are deposited onto the substrate at a high rate. After deposition, excess metal is removed from the source and drain electrodes by rinsing with acetone and isopropanol, respectively, followed by rinsing with deionized water and drying with high-purity nitrogen. This process minimizes the Fermi level pinning effect on the MoS2 source and drain electrode surfaces, reduces the source and drain Schottky barrier height and contact resistance, and achieves ohmic contact between the source and drain electrodes.

[0066] Example 2:

[0067] This invention provides a folded three-dimensional structure MoS2 field-effect transistor, such as... Figures 1 to 5As shown, the transistor includes a substrate, a high work function buried metal gate, a MoS2 thin film, and source / drain electrodes. The MoS2 thin film and the source / drain electrodes form a bottom-up "convex" structure. The high work function buried metal gate is placed at the middle of the bottom surface of the MoS2 thin film to form a Schottky contact, which eliminates the need for a dielectric layer and provides excellent rectification and capacitance characteristics. The source / drain electrodes are placed at both ends of the top surface of the MoS2 thin film to form ohmic contacts, resulting in minimal contact resistance between the source / drain electrodes and the MoS2 film, thus not affecting the electrical performance of the transistor.

[0068] Comparative Example 1:

[0069] like Figure 6 The figure shows the transfer characteristic curve of the folded three-dimensional structure MoS2 field-effect transistor of the present invention. Figure 7 The transfer characteristic curves are for a conventional MoS2 MOSFET. (The text abruptly ends here.) Figure 6 and Figure 7 The comparison shows that the folded three-dimensional structure MoS2 field-effect transistor has a lower threshold voltage, which means that it can be turned on with only a small gate voltage, better meeting the requirements of low power consumption.

[0070] like Figure 8 The figure shows the rectification characteristic curve of the folded three-dimensional structure MoS2 field-effect transistor of the present invention. Figure 9 The output shows the rectification characteristic curves of a conventional MoS2 MOSFET. Figure 8 and Figure 9 The comparison shows that the folded 3D structure MoS2 field-effect transistor has a significantly better rectification effect at 10... 3 Around 100%, while conventional MoS2MOSFETs do not have obvious rectification characteristics.

[0071] like Figure 10 The figure shows the subthreshold swing curve of a folded 3D MoS2 field-effect transistor. Figure 11 This is the subthreshold swing curve of a conventional MoS2 MOSFET. (The text abruptly ends here.) Figure 10 and Figure 11 The comparison shows that the folded three-dimensional structure MoS2 field-effect transistor has a lower subthreshold swing (SS) and is close to the physical limit of 60mV / dec; while the MoS2 MOSFET has a large number of interface traps at the oxide / MoS2 interface due to the presence of the oxide layer, which leads to a large hysteresis of the transistor and a larger subthreshold swing, resulting in higher power consumption and more heat.

[0072] Therefore, the present invention proposes a folded three-dimensional structure MoS2 field-effect transistor that simultaneously meets the requirements of threshold voltage, gate leakage current, rectification characteristics and subthreshold swing of ultra-small size low power field-effect transistor devices, thereby increasing the possibility of applying two-dimensional semiconductors to the integrated circuit industry.

[0073] The present invention has been described above by way of example, but the present invention is not limited to the specific embodiments described above. Any modifications or variations made based on the present invention shall fall within the scope of protection claimed by the present invention.

Claims

1. A method for fabricating a folded three-dimensional MoS2 field-effect transistor, characterized in that, comprising the following preparation steps: S1. Substrate preparation; S2. Performing ultraviolet lithography to form a "convex"-shaped buried metal gate pattern; S3. Performing vacuum thermal evaporation to deposit the buried metal gate; S4. Mechanically exfoliating the MoS2 thin film; S5. Dividing the MoS2 thin film; S6. Performing electron beam exposure for the source and drain electrodes; S7. Performing vacuum thermal evaporation to deposit the source and drain electrodes; The step S3 is vacuum thermal evaporation of metal buried gate, high work function metal platinum is placed on a tungsten boat; the sample prepared in S2 is put into an evaporation chamber, vacuum degree is extracted to be lower than 1×10 -4 pa; 270 A current heating is used for the tungsten boat, platinum on the tungsten boat is melted and evaporated to the sample after the photolithography treatment in S2 at a rate of 0.1-0.3 Å, 60-80 nm "convex” shaped buried gate is evaporated; After the evaporation is completed, acetone and isopropanol are used respectively for rinsing to remove excess metal outside the gate electrode, followed by rinsing with deionized water and then blow-drying with high-purity nitrogen; In the step S4 of mechanically exfoliating the MoS2 thin film, bulk MoS2 material is mechanically exfoliated into a millimeter-scale single-layer two-dimensional semiconductor by using a metal-assisted mechanical exfoliation technology; the sample obtained in S3 is placed on a transfer platform, and the mechanically exfoliated MoS2 thin film is transferred onto the "convex"-shaped buried metal gate electrode in combination with a fixed-point physical transfer process, and left to stand for 90-120s.

2. The method for fabricating a folded three-dimensional MoS2 field-effect transistor according to claim 1, characterized in that, In the step S1, the substrate is the SiO2 surface of single-side polished and single-side oxidized P-type low-resistance silicon, the substrate is cut into a size of 1 cm×1 cm with a diamond pen, the substrate is ultrasonically cleaned sequentially with acetone and isopropanol, then rinsed with deionized water and blow-dried with high-purity nitrogen.

3. The method for fabricating a folded three-dimensional MoS2 field-effect transistor according to claim 1, characterized in that, In the step S2 of performing ultraviolet lithography to form the "convex"-shaped buried metal gate pattern, the substrate obtained in S1 is placed on a spin coater, photoresist is spin-coated on the SiO2 layer for homogenization treatment, and then placed on a hot plate for baking to cure the photoresist; then the substrate is placed in an ultraviolet lithography apparatus, irradiated with ultraviolet light under a dedicated mask, the sample is taken out and placed on the hot plate for baking, then the sample is placed again in the ultraviolet lithography apparatus for ultraviolet irradiation in a maskless state, and after taking out the sample, it is rinsed sequentially with a developer and deionized water, and then blow-dried with high-purity nitrogen.

4. The method for fabricating a folded three-dimensional MoS2 field-effect transistor according to claim 1, characterized in that, In the step S5 of dividing the MoS2 thin film, an ultraviolet lithography process is adopted in combination with CF4 reactive ion etching technology to cut and divide the millimeter-scale MoS2 thin film to form mutually independent channels; after the etching is completed, the prepared sample is placed on a spin coater, photoresist is spin-coated on the sample for homogenization treatment, and then the sample is placed on a hot plate for baking to cure the photoresist.

5. The method for fabricating a folded three-dimensional MoS2 field-effect transistor according to claim 1, characterized in that, In the step S6 of performing electron beam exposure for the source and drain electrodes, the sample obtained in S5 is placed under an optical microscope for photographing, and the source and drain electrodes are subjected to patterning design by using an electron beam exposure system; the processed sample is placed in the electron beam exposure system, and the source and drain electrode regions are subjected to patterning design by using electron beam exposure technology; After the exposure is completed, the sample is taken out and rinsed sequentially with a developer and isopropanol, then rinsed with deionized water, and blow-dried with high-purity nitrogen to complete the patterning design of the source and drain electrodes.

6. The method for fabricating a folded three-dimensional MoS2 field-effect transistor according to claim 1, characterized in that, In step S7, vacuum thermal evaporation is used to deposit the source and drain electrodes. Indium metal is placed in a tungsten boat as the source and drain electrode material. The sample treated in S6 is then placed in the evaporation chamber, and the vacuum is evacuated to 1×10⁻⁶. -4 pa; The tungsten boat is heated with a current of 60 A to melt indium and deposit it onto the substrate at a rate of 0.3-0.7 Å, depositing source and drain electrodes of 10-30 nm. After the evaporation is completed, acetone and isopropanol are used respectively for rinsing to remove excess metal outside the source and drain electrodes, followed by rinsing with deionized water and then blow-drying with high-purity nitrogen.

7. A MoS2 field-effect transistor with a folded three-dimensional structure manufactured by the preparation method according to any one of claims 1 to 6.

8. A folded three-dimensional structure MoS2 field-effect transistor according to claim 7, characterized in that, The device includes a substrate, a high work function buried metal gate, a MoS2 thin film, and source / drain electrodes. The MoS2 thin film and the source / drain electrodes form a "convex" structure from bottom to top. The high work function buried metal gate is placed at the middle of the bottom surface of the MoS2 thin film to form a Schottky contact, and the source / drain electrodes are placed at both ends of the top surface of the MoS2 thin film to form ohmic contacts.

Citation Information

Patent Citations

  • Manufacturing method of organic field effect transistor with plane structure