Epoxy resin compositions for fiber-reinforced composites, fiber-reinforced composite materials, and methods for manufacturing fiber-reinforced composite materials.

By adding a specific proportion of tetraglycidyl diaminodiphenylmethane, bisphenol F epoxy resin, and a specific curing agent to the epoxy resin composition, the problems of resin viscosity and curing speed in the prior art are solved, and the high-performance properties of fiber-reinforced composite materials are achieved.

CN116829622BActive Publication Date: 2026-11-10TORAY INDUSTRIES INC
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202280014123.3
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2021-02-18
Filing Date
2022-02-10
Publication Date
2026-11-10
Estimated Expiration
2042-02-10

AI Technical Summary

Technical Problem

Existing single-component epoxy resin compositions, due to their low viscosity over long periods and slow heating rate during curing, cannot simultaneously meet the requirements of aircraft structural materials for high heat resistance, high compressive strength, impact resistance, and durability.

Method used

An epoxy resin containing tetraglycidyl diaminodiphenylmethane and bisphenol F is used, with 4,4'-methylenebis(3-chloro-2,6-diethylaniline) and 4,4'-methylenebis(2,6-diisopropylaniline) added as curing agents to adjust the viscosity and curing properties of the resin, so as to maintain high mechanical properties at low viscosity.

Benefits of technology

It achieves long-term resin injectability at low viscosity and imparts excellent heat resistance, high compressive strength, impact resistance and durability to fiber-reinforced composites during slow temperature curing.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_64
    Figure SMS_64
  • Figure SMS_65
    Figure SMS_65
  • Figure SMS_66
    Figure SMS_66
Patent Text Reader

Abstract

The object of the present invention is to provide an epoxy resin composition that maintains low viscosity for a long time during resin injection into a fiber-reinforced matrix, and imparts high levels of physical properties (heat resistance, high compressive strength, impact resistance, durability) required for structural material applications to fiber-reinforced composite materials, even when the heating rate during heat curing is slow, and fiber-reinforced composite materials using the epoxy resin composition. To achieve the above object, the epoxy resin composition for fiber-reinforced composite materials of the present invention comprises [A] tetraglycidyl diaminodiphenylmethane in a proportion of 70% to 90% by mass relative to 100% of the total epoxy resin components, [B] bisphenol F type epoxy resin in a proportion of 10% to 30% by mass relative to 100% of the total epoxy resin components, and comprises [C] 4,4'-methylenebis(3-chloro-2,6-diethylaniline) and [D] 4,4'-methylenebis(2,6-diisopropylaniline).
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to an epoxy resin composition for fiber-reinforced composite materials, a fiber-reinforced composite material using the epoxy resin composition, and a method for manufacturing the fiber-reinforced composite material. Background Technology

[0002] Fiber-reinforced composite materials, which consist of reinforcing fibers and matrix resins, can be designed to leverage the advantages of both materials. As a result, their applications have expanded from the aerospace field to sports, general industry, and other sectors.

[0003] As reinforcing fibers, glass fibers, aramid fibers, carbon fibers, boron fibers, etc., can be used. As matrix resins, both thermosetting resins and thermoplastic resins can be used, but thermosetting resins that are easy to impregnate the reinforcing fibers are often used. As thermosetting resins, epoxy resins, unsaturated polyester resins, vinyl ester resins, phenolic resins, bismaleimide resins, cyanate ester resins, etc., can be used.

[0004] Methods for molding fiber-reinforced composites include prepreg molding, hand lay-up, fiber winding, pultrusion, and RTM (Resin Transfer Molding). The prepreg method involves laminating prepregs impregnated with an epoxy resin composition into the reinforcing fibers into a desired shape and then heating the layers to obtain a molded article. While this method is geared towards producing fiber-reinforced composites with high material strength required for structural applications in aircraft, automobiles, etc., it requires multiple processes such as prepreg preparation and lamination, limiting production to small batches and hindering mass production. On the other hand, the RTM method involves injecting a liquid epoxy resin composition into a reinforcing fiber substrate placed in a heated mold, impregnating it, and then heating and curing it within the mold to obtain a molded article. This method allows for molding fiber-reinforced composites in a short time without the need for prepreg preparation, and also offers the advantage of easily molding even complex shapes.

[0005] As a liquid epoxy resin composition, either a one-component or a two-component epoxy resin composition can be used. A one-component epoxy resin composition is one containing epoxy resin and a curing agent, all components of which are pre-mixed into a single unit. In contrast, a two-component epoxy resin composition is an epoxy base liquid containing epoxy resin as the main component and a curing agent liquid containing a curing agent as the main component, which is mixed together just before use.

[0006] In the RTM process, single-component epoxy resin compositions are often used. To apply these compositions to large structural materials such as aircraft main wings and tail fins, a material must simultaneously meet the following two conditions: First, to obtain large structural materials without any unimpregnated components, the resin viscosity injected into the reinforcing fiber matrix must remain low for an extended period. Second, for large structural materials, the heating rate during curing is sometimes slow; therefore, even in this case, the fiber-reinforced composite material must possess the high levels of physical properties (heat resistance, high compressive strength, impact resistance, durability) required for its structural applications.

[0007] To address this situation, a one-component epoxy resin composition containing methylenebis(3-chloro-2,6-diethylaniline) (M-CDEA) as a curing agent has been disclosed, and a method for suppressing the increase in viscosity over a long period of time has been proposed (Patent Document 1). Furthermore, a one-component epoxy resin composition in which fluoreneamine curing agent is dispersed as a partial solid component has been disclosed, and a method for suppressing the increase in viscosity over a long period of time has been proposed (Patent Document 2). In addition, a one-component epoxy resin composition containing 4,4'-methylenebis(2-isopropyl-6-methylaniline) (M-MIPA) and 4,4'-methylenebis(2,6-diisopropylaniline) (M-DIPA) has been disclosed, and a method has been proposed that allows for sufficient high-speed curing at 180°C, and that the resin is fully cured during the demolding process after molding, thereby imparting high-level properties to the fiber-reinforced composite material (Patent Documents 3 and 4).

[0008] Existing technical documents

[0009] Patent documents

[0010] Patent Document 1: Japanese Patent No. 5808057

[0011] Patent Document 2: Japanese Patent Publication No. 11-511503

[0012] Patent Document 3: Japanese Patent Application Publication No. 2010-150310

[0013] Patent Document 4: International Publication No. 2020 / 008847 Summary of the Invention

[0014] The problem that the invention aims to solve

[0015] While the method described in Patent Document 1 can suppress the increase in viscosity over a long period of time, it suffers from the following problems due to the use of only methylene bis(3-chloro-2,6-diethylaniline) (M-CDEA), which has low reactivity: low curability; when the heating rate is slow during curing, the adhesive that binds the reinforcing fiber substrate sometimes melts excessively in the resin, resulting in uneven interlayer thickness of the fiber-reinforced composite material and insufficient post-impact compressive strength.

[0016] While the method described in Patent Document 2 above can suppress the increase in viscosity over a long period of time, it has the following problems: the fluoreneamine curing agent, which is sometimes dispersed as a part of the solid, agglomerates and is sometimes filtered out by the substrate when the resin is injected into the reinforcing fiber substrate; the melting point of the fluoreneamine curing agent is 201°C, which is very high, and even at a high temperature of 180°C, some of it sometimes dissolves and remains, resulting in poor curing and insufficient heat resistance.

[0017] While the methods described in Patent Documents 3 and 4 above can achieve sufficient high-speed curing and fully cure the molded resin, thus imparting high heat resistance and high mechanical properties to fiber-reinforced composite materials, they have the following problems: when the heating rate during curing is slow, the surface of the adhesive that bonds the reinforcing fiber substrate cannot melt in the resin, resulting in poor adhesion between the resin and the adhesive. Consequently, the fiber-reinforced composite material does not exhibit sufficient compressive strength, post-impact compressive strength, or resistance to microcracks.

[0018] Thus, in the prior art, there is no single-component epoxy resin composition that simultaneously satisfies both of the above conditions. Therefore, the object of the present invention is to provide an epoxy resin composition that maintains a low viscosity for a long time during resin injection into a fiber-reinforced matrix, and imparts the high level of physical properties (heat resistance, high compressive strength, impact resistance, durability) required for structural material applications to fiber-reinforced composite materials, even when the heating rate during heat curing is slow. Furthermore, by using such an epoxy resin composition, fiber-reinforced composite materials with excellent glass transition temperature, 0°C compressive strength under humid heat, post-impact compressive strength, and microcrack resistance of the cured resin are provided.

[0019] Methods for solving problems

[0020] To solve the above-mentioned problems, the epoxy resin composition for fiber-reinforced composite materials of the present invention has the following structure. That is, an epoxy resin composition for fiber-reinforced composite materials comprises [A] tetraglycidyl diaminodiphenylmethane in a mass percentage of 70% to 90% of 100% of the total epoxy resin components, [B] bisphenol F type epoxy resin in a mass percentage of 10% to 30% of 100% of the total epoxy resin components, and comprises [C] 4,4'-methylenebis(3-chloro-2,6-diethylaniline) and [D] 4,4'-methylenebis(2,6-diisopropylaniline).

[0021] Furthermore, the fiber-reinforced composite material of the present invention comprises a cured product of the epoxy resin composition for fiber-reinforced composite materials of the present invention, and a reinforcing fiber substrate.

[0022] The effects of the invention

[0023] According to the present invention, an epoxy resin composition for fiber-reinforced composite materials is provided that can maintain low viscosity for a long time during resin injection into a fiber-reinforced matrix, and impart high levels of physical properties (heat resistance, high compressive strength, impact resistance, durability) required for structural material applications to the fiber-reinforced composite material even when the heating rate during heat curing is slow. Detailed Implementation

[0024] The preferred embodiments of the present invention will be described below.

[0025] First, the epoxy resin composition for fiber-reinforced composite materials in this invention will be described.

[0026] The epoxy resin composition for fiber-reinforced composite materials of the present invention comprises [A] tetraglycidyl diaminodiphenylmethane in an amount of 70% to 90% by mass relative to 100% of all epoxy resin components, [B] bisphenol F type epoxy resin in an amount of 10% to 30% by mass relative to 100% of all epoxy resin components, and comprises [C] 4,4'-methylenebis(3-chloro-2,6-diethylaniline) and [D] 4,4'-methylenebis(2,6-diisopropylaniline). Hereinafter, the above components will sometimes be referred to simply as component [A], component [B], component [C], and component [D]. Furthermore, the epoxy resin composition for fiber-reinforced composite materials will sometimes be referred to simply as epoxy resin composition.

[0027] By using an epoxy resin composition containing the aforementioned percentages of components [A] and [B], and also containing components [C] and [D], the resin viscosity during resin injection into the fiber-reinforced matrix, which is difficult to achieve in the prior art, is kept low for a long time. Even when the heating rate during heat curing is slow, the fiber-reinforced composite material can be endowed with the high level of physical properties (heat resistance, high compressive strength, impact resistance, durability) required for structural material applications.

[0028] In this invention, component [A] is tetraglycidyldiaminodiphenylmethane. Component [A] is a necessary component for imparting high heat resistance and mechanical properties to epoxy resin cured products and fiber-reinforced composites. The tetraglycidyldiaminodiphenylmethane of component [A] referred to herein means N,N,N',N'-tetraglycidyldiaminodiphenylmethane, or its derivatives or isomers. Examples of such formulations include N,N,N',N'-tetraglycidyl-4,4'-diaminodiphenylmethane, N,N,N',N'-tetraglycidyl-3,3'-dimethyl-4,4'-diaminodiphenylmethane, N,N,N',N'-tetraglycidyl-3,3'-diethyl-4,4'-diaminodiphenylmethane, N,N,N',N'-tetraglycidyl-3,3'-diisopropyl-4,4'-diaminodiphenylmethane, and N,N,N',N'-tetraglycidyl-3, 3'-Di-tert-butyl-4,4'-diaminodiphenylmethane, N,N,N',N'-tetraglycidyl-3,3'-dimethyl-5,5'-diethyl-4,4'-diaminodiphenylmethane, N,N,N',N'-tetraglycidyl-3,3'-diisopropyl-5,5'-diethyl-4,4'-diaminodiphenylmethane, N,N,N',N'-tetraglycidyl-3,3'-diisopropyl-5,5'-dimethyl-4,4'-diaminodiphenylmethane, N,N,N', N'-Tetraglycidyl-3,3'-di-tert-butyl-5,5'-diethyl-4,4'-diaminodiphenylmethane, N,N,N',N'-tetraglycidyl-3,3'-di-tert-butyl-5,5'-dimethyl-4,4'-diaminodiphenylmethane, N,N,N',N'-tetraglycidyl-3,3',5,5'-tetramethyl-4,4'-diaminodiphenylmethane, N,N,N',N'-tetraglycidyl-3,3',5,5'-tetramethyl-4,4'-diaminodiphenylmethane, N,N,N',N'-tetraglycidyl-3,3',5,5'-tetraethyl-4,4'-diaminodiphenylmethane The composition may include tetraglycidyl diaminodiphenylmethane, N,N,N',N'-tetraglycidyl-3,3',5,5'-tetraisopropyl-4,4'-diaminodiphenylmethane, N,N,N',N'-tetraglycidyl-3,3',5,5'-tetra-tert-butyl-4,4'-diaminodiphenylmethane, N,N,N',N'-tetraglycidyl-3,3'-dichloro-4,4'-diaminodiphenylmethane, N,N,N',N'-tetraglycidyl-3,3'-dibromo-4,4'-diaminodiphenylmethane, etc. Furthermore, as component [A], two or more of these tetraglycidyl diaminodiphenylmethanes may be included.

[0029] Commercially available products containing tetraglycidyl diaminodiphenylmethane include: "Sumitomo Chemical Co., Ltd." ELM434 (registered trademark), YH434L (Nippon Steel & Sumitomo Chemical Co., Ltd.), "jER" 604 (registered trademark), "Araldite" MY720, and "Araldite" MY721 (and above). アドバンズド Made by MATRIARA Co., Ltd.), etc.

[0030] In this invention, component [A] needs to be present in a concentration of 70% to 90% by mass out of 100% by mass of the total epoxy resin composition. When component [A] is present in a concentration of 70% or more out of 100% by mass of the total epoxy resin composition, the cured epoxy resin exhibits high heat resistance, and the 0° compressive strength of the fiber-reinforced composite material under humid heat is improved. Furthermore, when component [A] is present in a concentration of 90% or less out of mass of the total epoxy resin composition, the viscosity of the epoxy resin composition at the resin impregnation temperature decreases, and the impregnation into the reinforcing fiber matrix is ​​improved. From this viewpoint, the content of component [A] is preferably in the range of 80% to 90% by mass out of 100% by mass of the total epoxy resin composition. It should be noted that, in this invention, the term "cured epoxy resin" refers to a cured product obtained by curing an epoxy resin composition.

[0031] In this invention, component [B] is a bisphenol F type epoxy resin. Component [B] is required to reduce the viscosity of the epoxy resin composition at the resin impregnation temperature, thereby improving the impregnation properties to the reinforcing fiber substrate. Furthermore, component [B] is required to impart high mechanical properties to the epoxy resin cured product and the fiber-reinforced composite material. The bisphenol F type epoxy resin referred to herein as component [B] is a substance having a structure in which the two phenolic hydroxyl groups of bisphenol F are glycidylated.

[0032] Commercially available bisphenol F type epoxy resins include: "jER (registered trademark)" 806, "jER (registered trademark)" 807, "jER (registered trademark)" 1750, "jER (registered trademark)" 4004P, "jER (registered trademark)" 4007P, "jER (registered trademark)" 4009P (all manufactured by Mitsubishi Chemical Co., Ltd.), "EPICLON (registered trademark)" 830 (manufactured by DIC Co., Ltd.), "Epoxy (registered trademark)" YDF-170, "Epoxy (registered trademark)" YDF2001, "Epoxy (registered trademark)" YDF2004 (all manufactured by Nippon Steel & Sumitomo Chemical Co., Ltd.), and "Araldito (registered trademark)" GY282 (Hantsuman). Made by Sebron Co., Ltd.), etc.

[0033] In this invention, the preferred resin viscosity η (mPa) of component [B] at 50°C is... s) satisfies 1000≤η≤10000. When η is 1000mPa At temperatures above η, the viscosity at the resin injection temperature will not be too low, making it less likely for unimpregnated areas to occur due to air entrapment during injection into the reinforcing fiber substrate. Furthermore, if the epoxy resin composition is highly reactive at the resin injection temperature, viscosity may increase during injection, reducing impregnation and resulting in unimpregnated areas, or causing molding time to increase, making molding difficult. However, this is not the case when η is 10000 mPa. Below s, the viscosity of the resin at the injection temperature is sufficiently low, thus improving the impregnation of the reinforcing fiber substrate and reducing the likelihood of incomplete impregnation. From this perspective, a resin viscosity η (mPa) is more preferable. s) satisfies 1000≤η≤8000. As the resin viscosity η (mPa) s) Commercially available resins that meet the above-mentioned criteria include, for example, "EPICLON (registered trademark)" 830 (manufactured by DIC Co., Ltd.) and "Alardite (registered trademark)" GY282 (Hantsuman). (Manufactured by Japan Co., Ltd.). It should be noted that the resin viscosity η (mPa) in this invention... s) Viscosity was measured using a type B viscometer in accordance with JIS Z8803 (1991), “Viscosity Measurement Method Using a Cone-Plate Rotation Viscometer”. Furthermore, commercially available products using tetramethylbisphenol F type epoxy resin as an alkyl substituted group include “Epoteto” YSLV-80XY (Nippon Steel & Sumitomo Chemical Co., Ltd.).

[0034] In this invention, component [B] needs to be present in a range of 10% by mass or more and 30% by mass or less out of 100% by mass of the total epoxy resin composition. When component [B] is present in a range of 10% by mass or more out of 100% by mass of the total epoxy resin composition, the viscosity of the epoxy resin composition at the resin impregnation temperature can be reduced, improving impregnation into the reinforcing fiber substrate, preventing incomplete impregnation, and further exhibiting high toughness and elastic modulus in the cured epoxy resin. Furthermore, when component [B] is 30% by mass or less, high heat resistance is exhibited. From this viewpoint, the content of component [B] is preferably in the range of 10% by mass or more and 25% by mass or less out of 100% by mass of the total epoxy resin composition.

[0035] Furthermore, the epoxy resin composition for fiber-reinforced composite materials of the present invention may contain epoxy resins other than components [A] and [B], provided that the epoxy resin content is 20% by mass or less out of 100% by mass of all epoxy resin components. Examples of such epoxy resins other than components [A] and [B] include bisphenol type epoxy resins, phenolic varnish type epoxy resins, cresol phenolic varnish type epoxy resins, resorcinol type epoxy resins, phenolic aralkyl type epoxy resins, naphthol aralkyl type epoxy resins, dicyclopentadiene type epoxy resins, epoxy resins having a biphenyl backbone, isocyanate modified epoxy resins, tetraphenylethane type epoxy resins, triphenylmethane type epoxy resins, and triglycidylamine type epoxy resins. It may contain one or more epoxy resins other than components [A] and [B].

[0036] As epoxy resins other than components [A] and [B], more specifically, examples include bisphenol A diglycidyl ether, tetrabromobisphenol A diglycidyl ether, bisphenol AD ​​diglycidyl ether, 2,2',6,6'-tetramethyl-4,4'-biphenyl diglycidyl ether, 9,9-bis(4-hydroxyphenyl)fluorene diglycidyl ether, tri(p-hydroxyphenyl)methane triglycidyl ether, tetra(p-hydroxyphenyl)ethane tetraglycidyl ether, phenolic varnish glycidyl ether, cresolic varnish glycidyl ether, glycidyl ether of the condensate of phenol and dicyclopentadiene, glycidyl ether of biphenyl aralkyl resin, triglycidyl isocyanurate, 5-ethyl-1,3-diglycidyl-5-methylhydantoin, and those obtained by the addition of bisphenol A diglycidyl ether to toluene isocyanate. Epoxy resins include azole ketone type, phenolic aralkyl type, and triglycidylaminophenol. Among these, bisphenol type epoxy resins (excluding component [B]) are preferred because they readily contribute to a good balance of toughness and heat resistance in the cured epoxy resin. In particular, liquid bisphenol type epoxy resins are preferred as epoxy resins other than components [A] and [B] because they contribute excellent impregnation properties to reinforcing fibers. It should be noted that in this invention, "liquid" refers to a viscosity of 1000 Pa at 25°C. Below s. Furthermore, the term "solid" refers to a substance that is non-flowable or has extremely low flowability at 25°C; specifically, its viscosity at 25°C is greater than 1000 Pa. Here, the viscosity is measured according to the “Viscosity Measurement Method Using a Conical-Plate Rotational Viscometer” in JIS Z8803 (1991), using an E-type viscometer (e.g., Tokimek Corporation TVE-30H) with a standard conical rotor (1°34'×R24) mounted on it.

[0037] Here, the term "bisphenol-type epoxy resin other than component [B]" refers to a substance in which the two phenolic hydroxyl groups of a bisphenol compound other than bisphenol F are glycidylated. Examples of bisphenol-type epoxy resins other than component [B] include bisphenol A type epoxy resin, bisphenol AD ​​type epoxy resin, and bisphenol S type epoxy resin, as well as substances in these bisphenol-type epoxy resins in which the bisphenol compound is partially substituted with halogens, substituted with alkyl groups, or hydrogenated. Furthermore, the bisphenol-type epoxy resin is not limited to monomers; high molecular weight derivatives with multiple repeating units can also be used. From the viewpoint of balancing the toughness and heat resistance of the cured epoxy resin, the content of bisphenol-type epoxy resin other than component [B] is preferably 20% by mass or less out of 100% by mass of the total epoxy resin composition.

[0038] Commercially available bisphenol A type epoxy resins include: "jER (registered trademark)" 825, "jER (registered trademark)" 826, "jER (registered trademark)" 827, "jER (registered trademark)" 828, "jER (registered trademark)" 834, "jER (registered trademark)" 1001, "jER (registered trademark)" 1002, "jER (registered trademark)" 1003, "jER (registered trademark)" 1004, and "jER..." "(Registered Trademark)" 1004AF, "jER (Registered Trademark)" 1007, "jER (Registered Trademark)" 1009 (all manufactured by Mitsubishi Chemical Co., Ltd.), "EPICLON (Registered Trademark)" 850 (manufactured by DIC Co., Ltd.), "Epototo (Registered Trademark)" YD-128 (manufactured by Nippon Steel & Sumitomo Chemical Co., Ltd.), "DER (Registered Trademark)"-331, "DER (Registered Trademark)"-332 (manufactured by Dooke Mikael Co., Ltd.), etc.

[0039] Commercially available products made of bisphenol S-type epoxy resin include "EPICLON (registered trademark)" EXA-1515 (manufactured by DIC Corporation).

[0040] The component [C] in this invention is 4,4'-methylenebis(3-chloro-2,6-diethylaniline). Component [C] is necessary to maintain a low viscosity of the resin injected into the resin of the reinforcing fiber matrix for a long period of time, and to impart high mechanical properties to the epoxy resin cured product and the fiber-reinforced composite material. Commercially available products containing such 4,4'-methylenebis(3-chloro-2,6-diethylaniline) include "Lonzakyu" M-CDEA (manufactured by Lonza Co., Ltd., a registered trademark).

[0041] In this invention, component [C] preferably comprises 60% to 90% by mass or more out of 100% by mass of all curing agent components. When component [C] comprises 60% or more out of 100% by mass of all curing agent components, it is easier to moderately suppress the reactivity of the epoxy resin composition, and the resin viscosity injected into the reinforcing fiber matrix is ​​particularly easy to maintain at a low viscosity for a long time. Furthermore, when component [C] comprises 90% or less out of mass, the adhesive binding the reinforcing fiber matrix does not excessively melt in the resin when the heating rate during heat curing is slow, making it easier to maintain the shape of the adhesive. Therefore, it is easier to uniformly ensure an interlaminar thickness capable of sufficient plastic deformation in the fiber-reinforced composite material, and it is easier to exhibit sufficient post-impact compressive strength. From this viewpoint, the content of component [C] is more preferably in the range of 70% to 90% by mass or more out of 100% by mass of all curing agent components.

[0042] The component [D] in this invention is 4,4'-methylenebis(2,6-diisopropylaniline). Component [D] is necessary to impart high heat resistance and mechanical properties to epoxy resin cured products and fiber-reinforced composites. Commercially available products containing such 4,4'-methylenebis(2,6-diisopropylaniline) include "Lonzakyu" M-DIPA (manufactured by Lonza Co., Ltd., a registered trademark).

[0043] In this invention, component [D] is preferably contained in a range of 5% by mass or more and 40% by mass or less in 100% by mass of all curing agent components. When component [D] is contained in 5% by mass or more in 100% by mass of all curing agent components, high heat resistance is readily exhibited. Furthermore, when it is contained in 40% by mass or less, the adhesive surface layer binding the reinforcing fiber matrix is ​​melted in the resin due to the slow heating rate during heat curing, resulting in good adhesion between the resin and the adhesive. Therefore, sufficient compressive strength, post-impact compressive strength, and microcrack resistance are readily exhibited. From this perspective, the content of component [D] is more preferably in the range of 5% by mass or more and 30% by mass or less in 100% by mass of all curing agent components.

[0044] The epoxy resin composition for fiber-reinforced composite materials of the present invention preferably further comprises [E] 4,4'-methylenebis(2-isopropyl-6-methylaniline). Hereinafter, [E] 4,4'-methylenebis(2-isopropyl-6-methylaniline) is sometimes simply referred to as component [E]. By including component [E], the epoxy resin cured product and the fiber-reinforced composite material can easily obtain higher heat resistance and higher mechanical properties. Commercially available products containing such 4,4'-methylenebis(2-isopropyl-6-methylaniline) include "Lonzakyua" M-MIPA (manufactured by Lonzakyua Co., Ltd.).

[0045] In the case of the epoxy resin composition for fiber-reinforced composite materials of the present invention, the content of component [E] is preferably 5% by mass or more and 20% by mass or less out of 100% by mass of all curing agent components. When component [E] is 5% by mass or more out of 100% by mass of all curing agent components, the heat resistance and compressive strength of the fiber-reinforced composite material are more easily improved. Furthermore, when it is 20% by mass or less, component [E] is less likely to precipitate even if the homogeneous epoxy resin composition in which component [E] is dissolved is frozen for a long time, resulting in excellent workability. In addition, it is easy to exhibit high-speed curing properties at high temperatures of 180°C. From this point of view, the content of component [E] is more preferably 5% by mass or more and 15% by mass or less out of 100% by mass of all curing agent components.

[0046] Furthermore, the epoxy resin composition for fiber-reinforced composite materials of the present invention may contain a compound having an active group capable of reacting with epoxy resin as a curing agent other than components [C], [D], and [E]. Examples of active groups capable of reacting with epoxy resin include, for example, amino groups and anhydride groups. Higher storage stability of the epoxy resin composition is preferred. Generally, liquid curing agents are more reactive; therefore, curing agents other than components [C], [D], and [E] are preferably solid at room temperature.

[0047] The curing agent, other than components [C], [D], and [E], is preferably an aromatic amine. Furthermore, from the viewpoint of heat resistance and mechanical properties, the curing agent, other than components [C], [D], and [E], is more preferably an aromatic polyamine compound having 1 to 4 phenyl groups within its molecule. Further, considering that increasing the elastic modulus of the resin by imparting flexibility to the molecular backbone can contribute to improved mechanical properties, it is further preferred that the curing agent for the epoxy resin contains at least one aromatic polyamine compound with an amino group at the ortho or meta position within its backbone.

[0048] Specific examples of aromatic polyamine compounds include m-phenylenediamine, diaminodiphenylmethane, diaminodiphenyl sulfone, m-phenylenediamine, diphenyl-p-diphenylamine, their alkyl-substituted derivatives, and isomers with different amino positions. These curing agents can be used alone or in combination of two or more. Among these, diaminodiphenylmethane and diaminodiphenyl sulfone are preferred from the perspective of imparting high heat resistance to epoxy resin cured products.

[0049] Commercially available products that serve as curing agents for aromatic polyamine compounds include Seikakua S (manufactured by Wakayama Seika Kogyo Co., Ltd.), MDA-220 (manufactured by Mitsui Chemicals Co., Ltd.), "jERKua" W (manufactured by Mitsubishi Chemical Co., Ltd.), 3,3'-DAS (manufactured by Mitsui Chemicals Co., Ltd.), "LonzaKua" M-DEA (manufactured by Lonza Co., Ltd.), "Kayahad" AA(PT) (manufactured by Nippon Kayaku Co., Ltd.), and "LonzaKua" DETDA 80 (manufactured by Lonza Co., Ltd.), among others.

[0050] Furthermore, the epoxy resin composition for fiber-reinforced composite materials of the present invention may include curing accelerators, plasticizers, dyes, pigments, inorganic fillers, antioxidants, ultraviolet absorbers, coupling agents, surfactants, etc. as other components as needed.

[0051] The epoxy resin composition for fiber-reinforced composite materials of the present invention can be a composition containing components [A], [B], [C], and [D] just before being injected into a reinforcing fiber substrate. It can be stored as a composition containing all the components as a monomer, or as a multiple composition containing any selected components. When stored as a multiple composition, for example, it can be stored as two compositions: an epoxy base liquid containing components [A] and [B], and a curing agent group containing components [C] and [D]. Just before being injected into a reinforcing fiber substrate, the epoxy base liquid and the curing agent group are mixed to prepare a composition containing all the components for use. When stored as a multiple composition, the combination of components contained in each composition can be arbitrarily selected. When stored as a multiple composition, from the viewpoint of preventing thickening caused by the curing reaction, it is preferable to include components [A] and [B] as epoxy resin and components [C] and [D] as curing agent in separate compositions as the combination of components contained in each composition.

[0052] In this invention, the H / E ratio, which is the ratio of the total number of epoxy groups (E) contained in the epoxy resin to the total number of active hydrogens (H) of the amine compounds contained in the curing agent, is preferably 1.1 or more and 1.4 or less. More preferably, the H / E ratio is 1.1 or more and 1.3 or less. When the H / E ratio is 1.1 or more, it is easier to obtain an effect that improves the plastic deformation capacity of the cured epoxy resin. Furthermore, when the H / E ratio is 1.4 or less, it is easier to exhibit high heat resistance.

[0053] In the epoxy resin composition for fiber-reinforced composite materials of the present invention, considering the significant effect of the present invention, the total content of components [A] to [D] is preferably 70 to 100% by mass, more preferably 80 to 100% by mass.

[0054] The epoxy resin composition for fiber-reinforced composite materials of the present invention may contain core-shell rubber particles. Core-shell rubber particles are excellent in readily imparting high toughness to fiber-reinforced composite materials. Here, core-shell rubber particles refer to particles in which a part or all of the core surface is coated with a particle-shaped core portion, which is mainly composed of a polymer such as cross-linked rubber, and a polymer different from the core portion through methods such as graft polymerization.

[0055] As components constituting the core portion of the aforementioned core-shell rubber particles, examples include polymers polymerized from one or more selected from conjugated diene monomers, acrylate monomers, and methacrylate monomers, or silicone resins. Specific examples of conjugated diene monomers include butadiene, isoprene, and chloroprene. The polymer used as a component of the core portion is preferably a cross-linked polymer formed by using these conjugated diene monomers alone or in combination. Particularly considering the good properties of the resulting polymer and its ease of polymerization, butadiene is preferably used as such a conjugated diene monomer; that is, the polymer used as a component of the core portion is a polymer polymerized from monomers containing butadiene.

[0056] The shell portion of the core-shell rubber particles is preferably grafted and polymerized with the aforementioned core portion, chemically bonded to the polymer particles constituting the core portion. Examples of components constituting such a shell portion include polymers selected from (meth)acrylates, aromatic vinyl compounds, etc. Furthermore, for ease of stabilizing the dispersion, it is preferable to introduce functional groups that react with components included in the epoxy resin composition for fiber-reinforced composites of the present invention, i.e., the epoxy resin or its curing agent, into the components constituting the shell portion. With the introduction of such functional groups, the affinity with the epoxy resin is improved, and it can ultimately react with the epoxy resin composition and be introduced into the cured epoxy resin, thus achieving good dispersibility. As a result, even small amounts of mixing achieve a sufficient improvement in toughness, maintaining the glass transition temperature Tg and elastic modulus while improving toughness. Examples of such functional groups include hydroxyl, carboxyl, and epoxy groups. Among these, epoxy groups are preferred for improving the affinity of the shell component with the epoxy resin composition of the present invention and for exhibiting good dispersibility. That is, the above-mentioned core-shell rubber particles are preferably core-shell rubber particles whose shell portion contains epoxy groups.

[0057] As a method for introducing such functional groups into the shell portion, examples include graft polymerization of one or more components, such as acrylates or methacrylates containing such functional groups, as part of a monomer onto the core surface.

[0058] The volume average particle size of the core-shell rubber particles is preferably 50 nm or more and 300 nm or less, more preferably 50 nm or more and 150 nm or less. It should be noted that the volume average particle size is measured using a nanotraffic particle size distribution measuring apparatus (manufactured by Nikkiso Co., Ltd., dynamic light scattering method). In cases where the volume average particle size of core-shell rubber particles cannot be measured using the nanotraffic particle size distribution measuring apparatus, thin sections of epoxy resin cured material produced by a slicing mechanism are observed using TEM, and the volume average particle size is measured from the obtained TEM image using image processing software. In this case, the average value of at least 100 particles is required. When the volume average particle size is 50 nm or more, the core-shell rubber particles have a moderately small specific surface area, which is energy-advantageous, making aggregation less likely and resulting in a high degree of toughness improvement. On the other hand, when the volume average particle size is 300 nm or less, the distance between the core-shell rubber particles is moderately smaller, resulting in a high degree of toughness improvement.

[0059] More preferably, the epoxy resin composition for fiber-reinforced composite materials of the present invention includes core-shell rubber particles whose shell portion contains epoxy groups, wherein the volume average particle size of the core-shell rubber particles is in the range of 50 nm or more and 300 nm or less. That is, the epoxy resin composition for fiber-reinforced composite materials of the present invention more preferably further includes [F] core-shell rubber particles whose shell portion contains epoxy groups and whose volume average particle size is in the range of 50 nm or more and 300 nm or less. Hereinafter, the core-shell rubber particles whose shell portion contains epoxy groups and whose volume average particle size is in the range of 50 nm or more and 300 nm or less will sometimes be simply referred to as component [F]. By including core-shell rubber particles that meet such conditions in the epoxy resin composition for fiber-reinforced composite materials, they are particularly easy to disperse well in the epoxy resin composition, and thus easily exhibit excellent toughness-enhancing effects.

[0060] There are no particular restrictions on the manufacturing method of core-shell rubber particles, and substances manufactured by known methods can be used. Commercially available core-shell rubber particles include, for example, "Paraloid" EXL-2655 (manufactured by Rohm & Haas) composed of butadiene / alkyl methacrylate / styrene copolymer; "Staffy" AC-3355 and TR-2122 (manufactured by Ganz Kasei Corporation) composed of acrylate / methacrylate copolymer; and "Paraloid" EXL-2611 and EXL-3387 (manufactured by Rohm & Haas Corporation) composed of butyl acrylate / methyl methacrylate copolymer. Alternatively, core-shell rubber particles with a three-layer structure can be created by covering a core layer of a glassy polymer with a glass transition temperature above room temperature with an intermediate layer of a rubbery polymer with a low Tg, using Staphyrod IM-601, IM-602 (manufactured by Ganz Chemical Co., Ltd.). These core-shell rubber particles are typically processed as powder by pulverizing the material taken out in lumps, often resulting in the powdered core-shell rubber being redispersed in the thermosetting resin composition. However, this method suffers from the problem of stably dispersing the particles in a non-agglomerated state, i.e., in a primary particle state. To address this problem, a preferred dispersion state can be obtained by using a material that is never taken out in lumps during the core-shell rubber particle manufacturing process, and can ultimately be processed as a masterbatch dispersed in a primary particle state in a component of a thermosetting resin, such as epoxy resin. Core-shell rubber particles that can be manipulated in such a masterbatch state can be manufactured, for example, by the method described in any of Examples 1 to 3 of Japanese Patent Application Publication No. 2004-315572. In this manufacturing method, firstly, the core-shell rubber is polymerized in an aqueous medium using methods such as emulsion polymerization, dispersion polymerization, and suspension polymerization to obtain a suspension in which the core-shell rubber particles are dispersed. Next, an organic solvent that is partially soluble in water, such as acetone, ketone solvents like methyl ethyl ketone, tetrahydrofuran, etc., is mixed into this suspension. After contacting an ether-based solvent such as an alkane with a water-soluble electrolyte such as sodium chloride or potassium chloride, the organic solvent layer and the aqueous layer are separated. The aqueous layer is then removed to obtain the organic solvent containing the core-shell rubber particles. Next, after mixing with epoxy resin, the organic solvent is evaporated to obtain a masterbatch in which the core-shell rubber particles are dispersed in the epoxy resin as primary particles. The core-shell rubber particle dispersed epoxy masterbatch manufactured by this method can be "KaneAce" (registered trademark) commercially available from Kaneka Co., Ltd.

[0061] When component [F] is included, its content is preferably 1 part by mass or more and 10 parts by mass or less relative to 100 parts by mass of the total epoxy resin composition, more preferably 1 part by mass or more and 8 parts by mass or less. When it is 1 part by mass or more, it is easy to obtain a high-toughness epoxy resin cured product. Furthermore, when it is 10 parts by mass or less, it is easy to obtain an epoxy resin cured product with a high elastic modulus, and the dispersibility of the core-shell rubber particles in the resin is also easily improved. It should be noted that even when the core-shell rubber particles have epoxy groups, the core-shell rubber particles are not equivalent to the epoxy resin composition.

[0062] As a method for mixing core-shell rubber particles into an epoxy resin composition for fiber-reinforced composites, commonly used dispersion methods can be used. Examples include the use of three-roll mills, ball mills, bead mills, jet mills, homogenizers, and rotary / revolutionary mixers. Furthermore, methods for dispersing epoxy masterbatches by mixing the aforementioned core-shell rubber particles are also preferred. However, sometimes even when dispersed in a primary particle state, re-agglomeration occurs due to excessive heating and a decrease in viscosity. Therefore, in the dispersion / blending of core-shell rubber particles, and in the subsequent mixing / kneading with other components, it is preferable to perform the process within a temperature / viscosity range where re-agglomeration of the core-shell rubber particles does not occur. Specifically, although this varies depending on the composition, for example, if kneading is performed at temperatures above 150°C, there is a possibility of a decrease in the viscosity of the composition and agglomeration; therefore, kneading at temperatures below this level is preferred. However, regarding the case of reaching temperatures above 150°C during the curing process, gelation during heating hinders re-agglomeration, so temperatures exceeding 150°C are permissible.

[0063] The epoxy resin composition for fiber-reinforced composite materials of the present invention preferably has a resin viscosity η (mPa) obtained by isothermal measurement using an E-type viscometer after being kept constant at 120°C for 240 minutes. s) satisfies 20 ≤ η ≤ 200. When η is 20 mPa At temperatures above η, the viscosity at the resin injection temperature is not too low, making it less likely for unimpregnated areas caused by air entrapment during injection into the reinforcing fiber substrate to occur. Furthermore, if the epoxy resin composition has high reactivity at the resin injection temperature, viscosity may increase during injection, reducing impregnation and resulting in unimpregnated areas, or causing molding time to increase, making molding difficult. However, this is not the case when η is 200 mPa. When the viscosity is below s, the impregnation of the resin into the reinforcing fiber substrate is good due to the sufficiently low viscosity at the resin injection temperature, and non-impregnation is less likely to occur. From this point of view, it is more preferable to satisfy 20≤η≤180. It should be noted that the viscosity in this invention is measured according to the "Viscosity Measurement Method Using a Cone-Plate Rotation Viscometer" in JIS Z8803 (1991), using a Type E viscometer (manufactured by Tokyo Keiki Co., Ltd., TVE-30H) equipped with a standard conical rotor (1°34'×R24), at a rotation speed of 50 rpm.

[0064] The epoxy resin composition for fiber-reinforced composite materials of the present invention preferably has a gelation temperature in the range of 170°C or higher and 185°C or lower when heated from 70°C at a heating rate of 0.5°C / min. Here, gelation of the epoxy resin composition refers to the reaction between the epoxy resin and the curing agent, resulting in the loss of fluidity. Specifically, the dynamic viscoelasticity of the epoxy resin composition was measured using a thermosetting measuring device such as an ATD-1000 (manufactured by Alpha Technologies, Inc.) by heating from 70°C at a heating rate of 0.5°C / min, and the complex viscosity, calculated from the torque increase accompanying the curing reaction, reached 1.0 × 10⁻⁶. 5 Pa The temperature at time s is set as the gelation temperature. When the gelation temperature is above 170°C, it tends to be higher than the melting point of the adhesive binding the reinforcing fiber matrix. When the gelation temperature is higher than the melting point of the adhesive, the adhesive binding the reinforcing fiber matrix melts at a temperature lower than the gelation temperature of the epoxy resin composition. Therefore, the epoxy resin composition enters the gaps between the loosened polyamide molecular chains. In this state, the epoxy resin gels and solidifies, resulting in increased interfacial bond strength between the resin and polyamide molecular chains, and improved compressive strength, impact resistance, and microcrack resistance. Furthermore, when the gelation temperature is below 185°C, the gelation temperature is less likely to be too high relative to the melting point of the adhesive binding the reinforcing fiber matrix. In such cases, the adhesive binding the reinforcing fiber matrix does not over-melt in the resin, maintaining the adhesive shape. Therefore, a uniform interlaminar thickness capable of sufficient plastic deformation can be ensured in the fiber-reinforced composite material, easily exhibiting sufficient post-impact compressive strength. From this perspective, a gelation temperature in the range of 175°C or higher and 185°C or lower is more preferable.

[0065] The epoxy resin composition for fiber-reinforced composite materials of the present invention preferably has a glass transition temperature (Tg) of 170°C or higher and 190°C or lower, obtained by curing the epoxy resin cured product at 180°C for 120 minutes. The heat resistance of the fiber-reinforced composite material depends on the glass transition temperature of the epoxy resin cured product obtained by curing the epoxy resin composition. By setting Tg to 170°C or higher, the heat resistance of the epoxy resin cured product is easily ensured. Furthermore, by setting it to 190°C or lower, the curing shrinkage of the epoxy resin composition is suppressed, and it is easy to prevent the deterioration of the surface quality of the fiber-reinforced composite material caused by the difference in thermal expansion between the epoxy resin composition and the reinforcing fibers. Furthermore, based on the relationship between heat resistance and surface quality, a glass transition temperature (Tg) of 175°C or higher and 190°C or lower is more preferable. Here, the glass transition temperature (Tg) of the epoxy resin cured product obtained by curing the epoxy resin composition is determined by measurement using a dynamic viscoelasticity (DMA) measuring device. That is, using rectangular test pieces cut from resin-cured plates, DMA was measured at elevated temperatures, and the inflection point of the obtained storage modulus G' was set as Tg. The measurement conditions were as described in the examples.

[0066] The fiber-reinforced composite material of the present invention comprises a cured product of the epoxy resin composition for fiber-reinforced composite materials of the present invention, and a reinforcing fiber substrate.

[0067] The fiber-reinforced composite material of the present invention can be obtained, for example, by injecting an epoxy resin composition consisting of epoxy resin and a curing agent into a reinforcing fiber substrate disposed within a heated molding die, thereby impregnating it, and then curing it within the molding die. As a specific molding method, as described above, the RTM method is suitable from the viewpoint of productivity and the degree of freedom in the shape of the resulting molded article. Furthermore, in the method of manufacturing such a fiber-reinforced composite material, it is preferable to use a molding die having multiple injection ports, injecting the epoxy resin composition simultaneously from multiple injection ports, or sequentially with a time difference, etc., selecting appropriate conditions according to the desired fiber-reinforced composite material, as this allows for a degree of freedom corresponding to molded articles of various shapes and sizes. There are no limitations on the number or shape of such injection ports, but more injection ports are better for enabling injection in a short time, and their arrangement is preferably at positions that minimize the resin flow length according to the shape of the molded article.

[0068] As the reinforcing fiber substrate used in fiber-reinforced composites, it is often formed by laminating and shaping sheet-like substrates such as reinforcing fiber woven fabrics using a hot-melt adhesive (tackifier) ​​to create preforms that closely resemble the desired product shape. Both thermoplastic and thermosetting resins can be used as the hot-melt adhesive. The form of the adhesive is not particularly limited and can take the form of film, tape, long fibers, short fibers, yarn, woven fabric, knitted fabric, nonwoven fabric, mesh, particles, etc. Among these, particle form or nonwoven form is particularly suitable. It should be noted that when the adhesive is in particle form, it is called adhesive particles, and when the adhesive is in nonwoven form, it is called adhesive nonwovens.

[0069] When using particles as the adhesive, the average particle size is preferably 10 μm or more and 500 μm or less. Here, average particle size refers to the median particle size. The average particle size of the adhesive particles can be measured, for example, using a laser diffraction particle size analyzer. If the average particle size is 10 μm or more, the bond strength and workability when forming preforms are easily improved. From this perspective, an average particle size of 30 μm or more is more preferable. If the average particle size is 500 μm or less, the reinforcing fibers are less prone to unevenness when forming preforms, and the mechanical properties of the resulting fiber-reinforced composite material are easily improved. From this perspective, an average particle size of 300 μm or less is more preferable.

[0070] When using a nonwoven fabric as the adhesive, the average diameter of the fibers constituting the nonwoven fabric is preferably 10 μm or more and 300 μm or less. Here, the average diameter is calculated by observing the cross-section of the adhesive nonwoven fabric using a scanning electron microscope, measuring the lengths of the diameters of arbitrarily selected 100 fibers, and then calculating their arithmetic mean. If the cross-sectional shape of the fiber is not perfectly circular, the minor axis is used as its diameter. If the average diameter is 10 μm or more, the bond strength of the preform is easily improved. If the average diameter is 300 μm or less, the reinforcing fibers of the preform are less prone to unevenness, and the mechanical properties of the resulting fiber-reinforced composite material are easily improved. From this perspective, an average diameter of 100 μm or less is more preferable.

[0071] The adhesive is adhered to at least the surface of the reinforcing fiber substrate, thus serving as a reinforcing fiber substrate with adhesive. Furthermore, the reinforcing fiber substrate with adhesive, having the aforementioned adhesive on at least its surface, is used in preforms.

[0072] In the fiber-reinforced composite material of the present invention, a preform formed by bonding the aforementioned reinforcing fiber substrates with a nonwoven adhesive is preferred. By forming a preform by bonding the reinforcing fiber substrates with a nonwoven adhesive, the adhesive can be uniformly distributed on the substrate, thus ensuring the impregnation flow path of the epoxy resin composition. Therefore, impregnation is particularly excellent, and voids are extremely unlikely to occur. Furthermore, even with a smaller amount of adhesive adhering compared to a particle-based adhesive, the morphological fixation effect when forming the preform can be maintained equally, making it easier to exhibit the inherent high heat resistance and mechanical properties of the matrix resin when forming the fiber-reinforced composite material.

[0073] The fiber-reinforced composite material of the present invention preferably has a gelation temperature above the melting point of the adhesive that bonds the reinforcing fiber matrix when the cured epoxy resin composition for fiber-reinforced composite materials is heated from 70°C at a heating rate of 0.5°C / min. The difference between the gelation temperature and the melting point (gelation temperature - melting point) is more preferably 1°C or more, and even more preferably 4°C or more. Furthermore, the difference between the gelation temperature and the melting point is preferably 20°C or less, and even more preferably 15°C or less. Within the aforementioned temperature range, the adhesive binding the reinforcing fiber matrix is ​​melted at a temperature lower than the gelation temperature of the epoxy resin composition. As a result, the epoxy resin composition enters the gaps between the loosened polyamide molecular chains. In this state, the epoxy resin is gelled and cured, thereby increasing the interfacial bond strength between the resin and the polyamide molecular chains. Compressive strength, impact resistance, and microcrack resistance are easily improved. Furthermore, the adhesive binding the reinforcing fiber matrix does not over-melt in the resin and maintains the shape of the adhesive. Therefore, a uniform interlayer thickness that allows for sufficient plastic deformation can be ensured in the fiber-reinforced composite material, making it easy to exhibit sufficient post-impact compressive strength.

[0074] In the fiber-reinforced composite material of the present invention, the nonwoven adhesive is preferably composed of polyamide with a melting point of 165°C or higher and 180°C or lower. When the melting point of the polyamide is 165°C or higher, the nonwoven form can be maintained during curing, easily ensuring a uniform interlayer thickness sufficient for adequate plastic deformation, or, since the nonwoven fabric is a continuous phase, it can easily and efficiently prevent cracking and readily exhibit impact resistance. When the melting point of the polyamide is 180°C or lower, the melting point of the polyamide is easily lower than the gelation temperature of the epoxy resin composition. When the melting point of the polyamide is lower than the gelation temperature of the epoxy resin composition, since the polyamide melts at a temperature lower than the gelation temperature of the epoxy resin composition, the epoxy resin composition enters the gaps between the loosened polyamide molecular chains. In this state, the epoxy resin gels and cures, thereby sometimes resulting in entanglement between the resin and the polyamide molecular chains, increasing interfacial bond strength, compressive strength, impact resistance, and microcrack resistance.

[0075] In the fiber-reinforced composite material of the present invention, it is preferable that the adhesive in the form of the above-mentioned nonwoven fabric is attached to one or both sides of the fiber-reinforced substrate.

[0076] In the fiber-reinforced composite material of the present invention, it is preferable that the amount of the nonwoven adhesive attached to the surface of the fiber-reinforced substrate is 0.5 g / m² per side. 2 Above and 10g / m 2 The following is a preferred adhesion amount: 1 g / m³. 2 Above and 7g / m 2 The following applies when the adhesion amount is 0.5 g / m². 2 Under the above conditions, it becomes easier to fix the shape when making preforms. Furthermore, at 10 g / m²... 2 In the following cases, the matrix resin readily exhibits sufficient impregnation and is less prone to voids. Furthermore, as mentioned above, when using a nonwoven fabric as the adhesive form, the same effect can be maintained even with a smaller adhesive application amount compared to using a particle form. Specifically, when a conventional adhesive in particle form or the like is applied to the surface, the preferred application amount is 0.5 g / m² per surface. 2 Above and 50g / m 2 The following is preferred: 1g / m 2 Above and 30g / m 2 The following adhesion amount, in contrast, for nonwoven fabrics, can maintain the same shape retention effect when making preforms while achieving an adhesion amount of 0.5 g / m². 2 Above and 10g / m 2 the following.

[0077] As a method for obtaining a preform, one example is to laminate a reinforced fiber substrate with adhesive on at least one surface, thereby fixing its shape. More specifically, for example, after forming a reinforced fiber substrate with adhesive by applying adhesive to at least one surface of at least one side of the reinforced fiber substrate through heating, multiple sheets of such substrate are laminated to obtain a laminate with adhesive at least between the layers of the laminate. Another example is to fix the shape by heating and cooling the substrate to fix the adhesive between the substrate layers, thereby obtaining a preform with adhesive at least between the layers of the laminate.

[0078] Typically, preforms are made by cutting adhesive-coated reinforcing fiber substrates into a specified shape, stacking them on a mold, and applying appropriate heat and pressure. Pressurization can be achieved using a press or by enclosing the preform in a vacuum bag and then using a vacuum pump to pressurize it to atmospheric pressure.

[0079] The fiber volume content of the reinforcing fibers in the fiber-reinforced composite material of the present invention is preferably in the range of 45% or more and 70% or less, more preferably in the range of 50% or more and 65% or less. When the fiber volume content is 45% or more, a fiber-reinforced composite material with further high elastic modulus and excellent lightweight effect can be obtained. Furthermore, when it is 70% or less, there is no strength reduction caused by friction between the reinforcing fibers, and a fiber-reinforced composite material with further excellent mechanical properties such as tensile strength can be obtained.

[0080] The reinforcing fibers constituting the reinforcing fiber matrix in this invention are not particularly limited, and examples include glass fibers, carbon fibers, graphite fibers, aramid fibers, boron fibers, alumina fibers, and silicon carbide fibers. Two or more of these reinforcing fibers can be used in combination. Among these, carbon fibers and graphite fibers are preferred for obtaining lighter and more durable fiber-reinforced composite materials. In particular, for applications requiring high lightweight and high strength, considering excellent specific modulus of elasticity and specific strength, carbon fibers are preferred as the reinforcing fibers constituting the reinforcing fiber matrix in the fiber-reinforced composite material of this invention.

[0081] As carbon fiber, all types of carbon fiber can be used depending on the application, but from the perspective of impact resistance, carbon fibers with a tensile modulus of elasticity of 230 GPa or more and 400 GPa or less are preferred. Furthermore, from the viewpoint of strength, to obtain a composite material with high rigidity and mechanical strength, carbon fibers with a tensile strength of 4.4 GPa or more and 6.5 GPa or less are preferred. In addition, tensile elongation is also an important factor, and high-strength, high-elongation carbon fibers with 1.7% or more and 2.3% or less are preferred. Therefore, carbon fibers possessing the characteristics of a tensile modulus of elasticity of at least 230 GPa, a tensile strength of at least 4.4 GPa, and a tensile elongation of at least 1.7% are most suitable.

[0082] Commercially available carbon fiber products include "Treka" T800G-24K, "Treka" T800S-24K, "Treka" T700G-24K, "Treka" T300-3K, and "Treka" T700S-12K (all manufactured by Toreka Co., Ltd.).

[0083] The fiber-reinforced composite material of the present invention, as described above, comprises an epoxy resin cured product of the epoxy resin composition for fiber-reinforced composite materials of the present invention, and a reinforcing fiber matrix. In applications of fiber-reinforced composite materials, particularly in the aerospace field, high heat resistance and mechanical properties are required. Preferably, the glass transition temperature of the epoxy resin cured product, which serves as the matrix resin in the fiber-reinforced composite material of the present invention, is 170°C or higher and 190°C or lower. This range of glass transition temperatures results in excellent heat resistance and reflects the high mechanical properties inherent in the epoxy resin cured product. Therefore, the fiber-reinforced composite material of the present invention exhibits a high H / W0° compressive strength (0° compressive strength under humid heat), preferably 1000 MPa or higher, and in more preferred embodiments, a high H / W0° compressive strength of 1100 MPa or higher. Furthermore, the post-impact compressive strength exhibits a high post-impact compressive strength, preferably 260 MPa or higher, and more preferably 270 MPa or higher.

[0084] The fiber-reinforced composite material of this invention exhibits excellent resistance to microcracks. Microcracks, referred to here, are tiny cracks, approximately tens of micrometers in size, that sometimes occur in fiber-reinforced composite materials used in aerospace applications. They are known to readily develop upon repeated exposure to environments with temperature variations ranging from approximately 70°C to approximately -50°C. If the matrix resin within the fiber-reinforced composite material is exposed to an atmosphere ranging from approximately 70°C to approximately -50°C, the matrix resin itself desires to shrink. However, because it is surrounded by reinforcing fibers that hardly shrink, it cannot shrink. As a result, internal tensile stress (thermal residual stress) accumulates within the matrix resin itself. If this is repeated, environmental fatigue can accumulate, leading to the formation of microcracks within the fiber-reinforced composite material. This phenomenon is particularly pronounced in resin-rich regions, where microcracks tend to develop. If environmental fatigue is further applied under conditions where microcracks have already formed, these microcracks may grow into larger cracks, ultimately reducing the mechanical properties of the fiber-reinforced composite material through these larger cracks. Due to the limitations of the RTM method, a resin flow path is required during molding, making it difficult to mold fiber-reinforced composites that have no resin-rich portions. In order to prevent microcracks caused by environmental fatigue, it is effective to improve the destructive toughness of the cured matrix resin and to moderately suppress the elastic modulus in a way that avoids excessive residual thermal stress generated in the matrix resin.

[0085] In the fiber-reinforced composite material of the present invention, from the viewpoint of long-term durability, the number of microcracks is preferably less than 10, more preferably 5 or less. The specific method for calculating the number of microcracks is as described below.

[0086] The manufacturing method of the fiber-reinforced composite material of the present invention involves injecting an epoxy resin composition for fiber-reinforced composite materials of the present invention, heated to 50°C or higher and 130°C or lower, into a reinforcing fiber substrate disposed in a molding die heated to 90°C or higher and 180°C or lower, thereby impregnating it, and then curing it within the molding die. Considering the impregnation properties into the reinforcing fiber substrate, the epoxy resin composition for fiber-reinforced composite materials is heated to a temperature selected from the range of 50°C or higher and 130°C or lower before injection, based on the relationship between the initial viscosity and viscosity increase of the epoxy resin composition. At this temperature, if the epoxy resin composition has high reactivity at the injection temperature, the viscosity may increase during injection, making molding difficult. Therefore, the resin viscosity of the epoxy resin composition for fiber-reinforced composite materials of the present invention after being kept constant at 120°C for 240 minutes is preferably 200 mPa. Below s, more preferably 180 mPa Below s. It should be noted that in this invention, viscosity measurement is performed by the method described later. If the viscosity 240 minutes after injection is higher than the above range, the impregnation of the epoxy resin composition may sometimes become insufficient. Furthermore, the resin viscosity after maintaining a constant temperature of 120°C for 240 minutes is preferably 20 mPa. At a temperature of s or higher, the viscosity of the resin at the injection temperature will not be too low, preventing incomplete impregnation caused by air entrapment during injection into the reinforcing fiber substrate. Furthermore, the molding die temperature is preferably 90°C or higher and 180°C or lower. By maintaining a molding die temperature of 90°C or higher and 180°C or lower, the curing time required is shortened, and thermal shrinkage after demolding is mitigated, thereby obtaining a fiber-reinforced composite material with excellent surface quality.

[0087] The injection pressure of the epoxy resin composition for fiber-reinforced composites is typically 0.1 MPa or higher and 1.0 MPa or lower. VaRTM (Vacuum Assisted Resins Transfer Molding), which involves injecting the epoxy resin composition while evacuating the mold, can also be used. Considering the economics of injection time and equipment, the injection pressure of the epoxy resin composition for fiber-reinforced composites is preferably 0.1 MPa or higher and 0.6 MPa. Furthermore, in the case of pressurized injection, it is preferable to evacuate the mold before injecting the epoxy resin composition for fiber-reinforced composites to suppress the formation of voids.

[0088] The fiber-reinforced composite material of the present invention has excellent heat resistance, high compressive strength, impact resistance, and durability. Therefore, it can be preferentially used in a large number of structural materials such as aircraft components such as fuselage, main wing, tail wing, moving wing, fairing, fairing, door, seat, and interior materials; spacecraft components such as motor housing, main wing, and structure; artificial satellite components such as antenna; outer plate, chassis, aerodynamic components; automobile components such as seat; railway vehicle components such as seat; ship components such as hull and seat.

[0089] Example

[0090] The following examples further illustrate the epoxy resin compositions for fiber-reinforced composite materials of the present invention in detail, but the present invention is not limited to them.

[0091] <Resin Raw Materials>

[0092] The following resin raw materials were used to obtain the epoxy resin compositions of each embodiment / comparative example. It should be noted that the values ​​of each component in the column of epoxy resin composition in the table represent the content, and the unit is "parts by mass" unless otherwise specified.

[0093] 1. [A] Tetraglycidyldiaminodiphenylmethane "Araldite (registered trademark)" MY721 (N,N,N',N'-tetraglycidyl-4,4'-diaminodiphenylmethane, epoxy equivalent: 113 g / mol, hantsman) Made by Seboron Co., Ltd.) 2. [B] Bisphenol F type epoxy resin "EPICLON (registered trademark)" 830 (Bisphenol F diglycidyl ether, epoxy equivalent: 170 g / mol, manufactured by DIC Co., Ltd.) "Araldite (registered trademark)" GY282 (Bisphenol F diglycidyl ether, epoxy equivalent: 171 g / mol, hantsman) Made by Seboron Co., Ltd.) 3. Epoxy resins other than component [A] and component [B]. "EPICLON (registered trademark)" 850 (Bisphenol A diglycidyl ether, epoxy equivalent: 188 g / mol, manufactured by DIC Co., Ltd.).

[0094] 4. [C] 4,4'-Methylenebis(3-chloro-2,6-diethylaniline) “Lonzakyu (registered trademark)” M-CDEA (4,4'-methylenebis(3-chloro-2,6-diethylaniline, active hydrogen equivalent: 95g / mol, manufactured by Lonza Co., Ltd.).

[0095] 5. [D] 4,4'-Methylenebis(2,6-diisopropylaniline) "Lonzakyu (registered trademark)" M-DIPA (4,4'-methylenebis(2,6-diisopropylaniline)), active hydrogen equivalent: 93 g / mol, manufactured by Lonza Co., Ltd. 6. [E] 4,4'-Methylenebis(2-isopropyl-6-methylaniline) "Lonzakyua (registered trademark)" M-MIPA (3,3'-diisopropyl-5,5'-dimethyl-4,4'-diaminodiphenylmethane, active hydrogen equivalent: 78 g / mol, manufactured by Lonza Co., Ltd.) 7. Curing agents other than components [C], [D], and [E]. "Lonzakyua (registered trademark)" M-DEA (3,3',5,5'-tetraethyl-4,4'-diaminodiphenylmethane, active hydrogen equivalent: 78 g / mol, manufactured by Lonza Co., Ltd.) "Kayahad (registered trademark)" AA(PT) (a mixture with 2,2'-diethyl-4,4'-diaminodiphenylmethane as the main component, active hydrogen equivalent: 64 g / mol, liquid, manufactured by Nippon Kayaku Co., Ltd.) 8. Additives "Kaneasu (registered trademark)" MX-416 ("Araldito (registered trademark)" MY721: 75% by mass / core-shell rubber particles (volume average particle size: 100nm, core part: cross-linked polybutadiene, shell part: methyl methacrylate / glycidyl methacrylate / styrene copolymer): 25% by mass masterbatch, (Kanea Co., Ltd.) “Staffy Road (registered trademark)” AC-3355 (Core-shell rubber particles (volume average particle size: 500nm, core part: cross-linked polybutyl acrylate, shell part: cross-linked polystyrene, manufactured by Iika Kogyo Co., Ltd.).

[0096] <Preparation of Epoxy Resin Compositions>

[0097] Mix the components according to the proportions listed in the table to prepare an epoxy resin composition.

[0098] <Preparation of Resin Curing Board>

[0099] After degassing the prepared epoxy resin composition under reduced pressure, it was injected into a mold with a thickness of 2mm, achieved by using a 2mm thick "Teflon" spacer. The mold was then cured at 180°C for 120 minutes to obtain a 2mm thick resin-cured board.

[0100] <The Making of Adhesives>

[0101] An adhesive is produced according to the following manufacturing method.

[0102] (Making Adhesive 1)

[0103] 1.2 g of caprolactam, 18.8 g of dodecanoic acid, and 10 g of deionized water were added to a pressure vessel and sealed. Nitrogen purging was then performed. Heating was initiated, and the pressure inside the vessel reached 10 kg / cm². 2 Then, while releasing water out of the system, the pressure inside the tank is increased to 10.0 kg / cm². 2If the internal temperature reaches 170°C, the pressure inside the tank is restored to atmospheric pressure after 50 minutes, and the reaction is further carried out under a nitrogen flow for 2 hours to complete the polymerization. Then, the polymer is discharged from the pressure vessel in strips to form granules, which are then vacuum dried at 80°C for 24 hours to obtain a copolymer PA-1 of nylon 6 / 12 (=6 / 94 mass%). PA-1 fibers (melting point: 170°C) discharged from a die with one orifice are stretched using a suction device with an impact plate at the front end and compressed air, and then dispersed on a metal mesh for collection. The fiber sheets collected on the metal mesh are thermally bonded using a heated press to produce an adhesive 1 in the form of a nonwoven fabric.

[0104] (Making Adhesive 2)

[0105] PES (Sumitomo Chemical Co., Ltd. "Sumica Eccell" 5003P, melting point: none) fibers discharged from a mold with one orifice were stretched using a suction device with an impact plate at the front end and compressed air, and then dispersed onto a metal mesh for collection. The fiber sheets collected on the metal mesh were then thermally bonded using a heated and pressurized machine to create an adhesive 2 in the form of a nonwoven fabric.

[0106] (Making Adhesive 3)

[0107] PA-2 (Amiran CM1001, melting point: 225°C) fibers, discharged from a die with one opening, were stretched using a suction device with an impact plate at the front end and compressed air, and then collected by spreading them on a metal mesh. The fiber sheets collected on the metal mesh were then thermally bonded using a heated and pressurized machine to create an adhesive 3 in the form of a nonwoven fabric.

[0108] (Making Adhesive 4)

[0109] PA-3 fibers (Alkema Co., Ltd. "Platamid" M1657, melting point: 110°C), discharged from a die with one opening, were stretched using a suction device with an impact plate at the front end and compressed air, and then collected by spreading them on a metal mesh. The fiber sheets collected on the metal mesh were then thermally bonded using a heated and pressurized machine to create an adhesive 4 in the form of a nonwoven fabric.

[0110] (Making Adhesive 5)

[0111] A binder resin composition was prepared by mixing 15 parts by weight of cresol phenolic varnish-type epoxy resin (DIC Co., Ltd. "EPICLON (registered trademark)" N-660), 25 parts by weight of bisphenol type epoxy resin (Mitsubishi Kemica Co., Ltd. "jER (registered trademark)" 825), and 60 parts by weight of polyethersulfone (Sumitomo Chemical Co., Ltd. "Smica Eccell (registered trademark)" PES5200P) at 180°C using a small twin-screw extruder (S1KRC kneader, Kurimoto Iron Works Co., Ltd.). The prepared binder resin composition was then subjected to cryogenic pulverization using a hammer mill (PULVERIZER, Hosokawa Miklon Co., Ltd.) with a 1mm mesh screen and liquid nitrogen to obtain a particle-shaped binder 5. The particles were passed through sieves with aperture sizes of 150 μm and 75 μm. The binder particles remaining on the sieve with an aperture size of 75 μm were used for evaluation.

[0112] <Fabrication of Reinforced Fiber Substrates with Adhesives>

[0113] The resulting adhesive is applied to a carbon fiber unidirectional woven fabric (plain weave, warp: carbon fiber T800S-24K-10C, manufactured by Tore Co., Ltd., carbon fiber mesh 295g / m). 2 The warp density is 7.2 yarns / 25mm, and the weft yarn is glass fiber ECE225 1 / 01Z (manufactured by Nittobo Co., Ltd., with a weft density of 7.5 yarns / 25mm). The adhesion amount is set to 5g / m² when using adhesives 1 to 4. 2 In the case of adhesive 5, it is set at 10 g / m 2 Then, a far-infrared heater is used to heat the material, causing the adhesive to fuse and resulting in an adhesive-reinforced fiber substrate with adhesive applied to one side of the surface.

[0114] <Evaluation>

[0115] The evaluations in each embodiment are performed as follows. It should be noted that unless otherwise specified, the number n is n=1.

[0116] (1) Determination of gelation temperature of epoxy resin composition

[0117] The specimens to be tested were placed in an ATD-1000 thermosetting testing apparatus (manufactured by Alpha Technologies, Inc.) at a temperature of 70°C. Dynamic viscoelasticity was measured simultaneously at a frequency of 1.0 Hz and a strain of 1%, while simultaneously increasing the temperature at a rate of 0.5°C / min. The complex viscosity was then determined. At this point, the complex viscosity was considered to be 1.0 × 10⁻⁶. 5 Pa The temperature s is set as the gelation temperature. It should be noted that, as the specimen, an epoxy resin composition was used after mixing the components and stirring for 1 minute.

[0118] (2) Determination of the viscosity of the epoxy resin composition after holding at 120℃ for 240 minutes

[0119] The sample to be tested was measured according to the "Viscosity Measurement Method Using a Conical-Plate Rotary Viscometer" in JIS Z8803 (1991), using a Type E viscometer fitted with a standard conical rotor (1°34'×R24), and at a temperature maintained at 120°C. The Type E viscometer used was a TVE-30H manufactured by Tokyo Keiki Co., Ltd. It should be noted that the sample used was an epoxy resin composition in which all components were mixed and stirred for 1 minute.

[0120] (3) Determination of glass transition temperature (Tg) of epoxy resin cured products

[0121] Test pieces with a width of 12.7 mm and a length of 40 mm were cut from the resin-cured plate, and Tg was measured using a DMA apparatus ARES (manufactured by TA Instrument Menthols). The measurement conditions were a heating rate of 5 °C / min. The temperature at which the inflection point of the storage modulus G' obtained in the measurement was defined as Tg.

[0122] (4) Determination of compressive strength of fiber-reinforced composite materials at 0°C under damp heat

[0123] In a mold with a plate-shaped cavity of 400mm × 400mm × 1.2mm, four pieces of the aforementioned adhesive-coated reinforcing fiber substrate, cut to 395mm × 395mm, were stacked and aligned along the 0° direction with the fiber orientation at 0°. The mold was then closed. Next, after heating the mold to 120°C, an epoxy resin composition, separately preheated to 120°C, was injected into the mold using a resin injection device at an injection pressure of 0.2MPa. After injection, the mold was heated from 120°C to 180°C at a rate of 0.5°C / min. After curing at 180°C for 2 hours, the temperature was lowered to 30°C to obtain the fiber-reinforced composite material.

[0124] From the fiber-reinforced composite material obtained by the above method, test pieces with a width of 12.7 mm and a length of 79.4 mm were cut in a manner where the 0° direction and the length direction became the same, thus producing test pieces for 0° compressive strength. The 0° compressive strength of the fiber-reinforced composite material was measured after immersion in warm water at 72°C for 14 days. The 0° compressive strength was determined according to ASTM D695 using a universal testing machine (Instron). The crosshead speed during measurement was set to 1.27 mm / min, and the measurement temperature was set to 82°C. (Japanne Corporation 4208 type Instron)

[0125] (5) Determination of post-impact compressive strength of fiber-reinforced composite materials

[0126] In a mold with a plate-shaped cavity of 400mm × 400mm × 4.8mm, 12 pieces of the aforementioned adhesive-coated reinforcing fiber substrate, cut to 395mm × 395mm, were stacked by repeating the process three times (45° / 0° / -45° / 90°) with the fiber direction at 0°, and then repeated three times (90° / -45° / 0° / 45°) to stack another 12 pieces. The mold was then closed. Next, after heating the mold to 120°C, an epoxy resin composition, preheated to 120°C, was injected into the mold using a resin injection device at an injection pressure of 0.2MPa. After injection, the mold was heated from 120°C to 180°C at a rate of 0.5°C / min, cured at 180°C for 2 hours, and then cooled to 30°C to obtain a fiber-reinforced composite material.

[0127] From the fiber-reinforced composite material obtained by the above method, test pieces with a width of 101.6 mm and a length of 152.4 mm were cut in such a manner that the 0° direction and the length direction become the same. The compressive strength after impact was determined according to SACMA SRM 2R-94. An inductor was used as the testing machine. Made by Japan Co., Ltd. (Type 1128 Tenshiron). Here, the energy of the falling hammer impact is set to 6.7 J / mm, and the crosshead velocity is set to 1.27 mm / min.

[0128] (6) Number of microcracks in fiber-reinforced composites

[0129] From the fiber-reinforced composite material obtained by (5) above, test pieces with a width of 75 mm and a length of 50 mm are cut in such a way that the 0° direction becomes the same as the length direction. The resulting test pieces are exposed to the environmental conditions shown in steps a, b, and c below using a commercially available temperature and humidity chamber and environmental testing machine.

[0130] a. Use a commercially available temperature and humidity bath to expose the product to an environment of 49°C and 95% RH for 12 hours.

[0131] b. After exposure, transfer to a commercially available environmental testing machine and initially expose to -54°C for 1 hour. Then, heat to 71°C at a rate of 10°C ± 2°C / min. After heating, hold at 71°C for 5 minutes ± 1 minute, then cool to -54°C at a rate of 10°C ± 2°C / min, and hold at -54°C for 5 minutes ± 1 minute. This cycle of heating from -54°C to 71°C and cooling back to -54°C is defined as one cycle, and this cycle is repeated 200 times.

[0132] c. Combine the environmental exposure in the constant temperature and humidity bath and the cycle in the environmental testing machine into 1 block, and repeat 5 blocks.

[0133] A 25mm wide section was cut from the longitudinal direction of the test piece subjected to the aforementioned environmental exposure, within ±10mm of the center. The cut surface was then ground and observed using a commercially available microscope at 200x magnification. The number of cracks generated was then measured. From the viewpoint of the long-term durability of fiber-reinforced composite materials, the number of microcracks observed by the above method is preferably less than 10, more preferably less than 5. Therefore, the case of less than 5 is designated as A, the case of 6 or more but less than 10 is designated as B, and the case of more than 10 is designated as C.

[0134] (Example 1)

[0135] As shown in Table 1-1, 70 parts by weight of "Araldito (registered trademark)" MY721 as component [A], 30 parts by weight of "EPICLON (registered trademark)" 830 as component [B], 59 parts by weight of "Lonzakyu (registered trademark)" M-CDEA as component [C], and 25 parts by weight of "Lonzakyu (registered trademark)" M-DIPA as component [D] were added, and the mixture was stirred at 80°C for 1 hour to prepare an epoxy resin composition. As described above, the gelation temperature of the epoxy resin composition was measured, and the result was 177°C. This indicates good interfacial adhesion between the adhesive and the resin, and the adhesive shape is maintained. Therefore, this is a particularly preferred temperature for ensuring a uniform interlayer thickness capable of sufficient plastic deformation in fiber-reinforced composites. Next, the viscosity of the epoxy resin composition after holding at 120°C for 240 minutes was measured, and the result was 140 mPa. The resin exhibits good impregnation properties, particularly towards the reinforcing fibers. Furthermore, the cured resin produced using the above method was tested, and its Tg was measured to be 175°C, indicating excellent heat resistance. Further, fiber-reinforced composite materials were prepared using this epoxy resin composition, and the compressive strength at 0°C under humid heat, the compressive strength after impact, and the number of microcracks were measured. The results showed a good compressive strength at 0°C under humid heat of 1060 MPa, a good compressive strength after impact of 280 MPa, and a particularly good number of microcracks (less than 5).

[0136] (Examples 2-5)

[0137] The contents of each component were changed as shown in Table 1-1, and the epoxy resin composition was prepared in the same manner as in Example 1. As described above, the gelation temperature of the epoxy resin composition was measured, and the results were all above 170°C and below 185°C. This indicates good interfacial adhesion between the adhesive and the resin, and the adhesive maintains its shape. Therefore, this temperature range ensures a uniform interlayer thickness capable of sufficient plastic deformation in fiber-reinforced composites. Examples 2, 3, and 5, with temperatures above 175°C and below 185°C, are particularly preferred results. Next, the viscosity of the epoxy resin composition after holding at 120°C for 240 minutes was measured, and the results were all 200 mPa. Below s, the impregnation properties of the reinforcing fibers are also good. Examples 2, 3, and 5 have a pressure of 180 mPa. The results below s are particularly preferred. Furthermore, the cured resin products prepared by the above method were tested, and the Tg of the cured products were all above 175°C, indicating particularly good heat resistance. Further, fiber-reinforced composite materials were prepared using this epoxy resin composition, and the compressive strength at 0°C under humid heat, the compressive strength after impact, and the number of microcracks were measured. The results showed that the compressive strength at 0°C under humid heat was above 1000 MPa, the compressive strength after impact was above 260 MPa, and the number of microcracks was less than 10, indicating good mechanical properties and durability. Among these, the compressive strength at 0°C under humid heat of Examples 2, 3, and 5, which were above 1100 MPa, above 270 MPa, and had fewer than 5 microcracks, were particularly preferred results.

[0138] (Example 6)

[0139] As shown in Table 1-1, 80 parts by weight of "Araldito (registered trademark)" MY721 as component [A], 20 parts by weight of "EPICLON (registered trademark)" 830 as component [B], 52 parts by weight of "Lonzakyua (registered trademark)" M-CDEA as component [C], 17 parts by weight of "Lonzakyua (registered trademark)" M-DIPA as component [D], and 15 parts by weight of "Lonzakyua (registered trademark)" M-MIPA as component [E] were added, and the mixture was stirred at 80°C for 1 hour to prepare an epoxy resin composition. As described above, the gelation temperature of the epoxy resin composition was determined to be 170°C. This indicates good interfacial adhesion between the adhesive and resin, and the adhesive maintains its shape. Therefore, this temperature is suitable for ensuring a uniform interlayer thickness capable of sufficient plastic deformation in fiber-reinforced composites. Next, the viscosity of the epoxy resin composition after holding at 120°C for 240 minutes was measured, and the result was 200 mPa. The impregnation properties of the epoxy resin composition with reinforcing fibers are also good. Furthermore, the cured resin produced by the above method was tested, and the Tg of the cured product was measured to be 186°C, indicating particularly good heat resistance. Further, fiber-reinforced composite materials were prepared using this epoxy resin composition, and the compressive strength at 0°C under humid heat, the compressive strength after impact, and the number of microcracks were measured. The results showed that the compressive strength at 0°C under humid heat was 1030 MPa, the compressive strength after impact was 260 MPa, and the number of microcracks was 6 or more but less than 10, which is excellent.

[0140] (Examples 7 and 8)

[0141] The contents of each component were changed as shown in Tables 1-1 and 1-2, and the epoxy resin composition was prepared in the same manner as in Example 6. As described above, the gelation temperature of the epoxy resin composition was measured, and the results were all above 175°C and below 185°C. This indicates good interfacial adhesion between the adhesive and the resin, and the adhesive maintains its shape. Therefore, this is a particularly preferred temperature for ensuring a uniform interlayer thickness capable of sufficient plastic deformation in fiber-reinforced composites. Next, the viscosity of the epoxy resin composition after holding at 120°C for 240 minutes was measured, and the results were all 180 mPa. The resin exhibits excellent impregnation properties, particularly with reinforcing fibers. Furthermore, the cured resin produced using the above method was tested, and the Tg of the cured product was measured, showing values ​​above 175°C, indicating particularly good heat resistance. Moreover, fiber-reinforced composite materials were prepared using this epoxy resin composition, and the compressive strength at 0°C under humid heat, the compressive strength after impact, and the number of microcracks were measured. The results showed that the compressive strength at 0°C under humid heat was above 1100 MPa, the compressive strength after impact was above 270 MPa, and the number of microcracks was below 5, demonstrating particularly good mechanical properties and durability.

[0142] (Example 9)

[0143] As component [B], "Araldito (registered trademark)" GY282 was used. Otherwise, the epoxy resin composition was prepared in the same manner as in Example 7. As described above, the gelation temperature of the epoxy resin composition was measured and found to be 175°C. This temperature indicates good interfacial adhesion between the adhesive and resin and maintains the shape of the adhesive. Therefore, it is a particularly preferred temperature for ensuring a uniform interlayer thickness capable of sufficient plastic deformation in fiber-reinforced composites. Next, the viscosity of the epoxy resin composition after holding at 120°C for 240 minutes was measured and found to be 170 mPa. The resin exhibits good impregnation properties, particularly towards the reinforcing fibers. Furthermore, the cured resin produced using the above method was tested, and its Tg was measured to be 184°C, indicating good heat resistance. Further, fiber-reinforced composite materials were prepared using this epoxy resin composition, and the compressive strength at 0°C under humid heat, the compressive strength after impact, and the number of microcracks were measured. The results showed that the compressive strength at 0°C under humid heat was 1150 MPa, which is good; the compressive strength after impact was 270 MPa; and the number of microcracks was less than 5, which is particularly good.

[0144] (Example 10)

[0145] Instead of component [E], "Lonzakyu (registered trademark)" M-DEA was used, and the epoxy resin composition was prepared in the same manner as in Example 7. As described above, the gelation temperature of the epoxy resin composition was measured and found to be 176°C. This temperature indicates good interfacial adhesion between the adhesive and resin and maintains the shape of the adhesive, making it a particularly preferred temperature for ensuring a uniform interlayer thickness capable of sufficient plastic deformation in fiber-reinforced composites. Next, the viscosity of the epoxy resin composition after holding at 120°C for 240 minutes was measured and found to be 160 mPa. The resin exhibits good impregnation properties, particularly towards the reinforcing fibers. Furthermore, the cured resin produced using the above method was tested, and the Tg of the cured product was measured to be 174°C, indicating good heat resistance. Further, fiber-reinforced composite materials were prepared using this epoxy resin composition, and the compressive strength at 0°C under humid heat, the compressive strength after impact, and the number of microcracks were measured. The results showed that the compressive strength at 0°C under humid heat was 1040 MPa, which is good; the compressive strength after impact was 270 MPa; and the number of microcracks was less than 5, which is particularly good.

[0146] (Examples 11-13)

[0147] The contents of each component and the H / E ratio were changed as shown in Tables 1-2. Otherwise, the epoxy resin composition was prepared in the same manner as in Example 2. As described above, the gelation temperature of the epoxy resin composition was measured, and the results were all above 170°C and below 185°C. This indicates good interfacial adhesion between the adhesive and the resin, and the adhesive maintains its shape. Therefore, this temperature range ensures a uniform interlayer thickness capable of sufficient plastic deformation in fiber-reinforced composites. Examples 11 and 12, with temperatures above 175°C and below 185°C, are particularly preferred results. Next, the viscosity of the epoxy resin composition after holding at 120°C for 240 minutes was measured, and the results were all 200 mPa. Below s, the impregnation properties of the reinforcing fibers are also good. Examples 11 and 12 show a pressure of 180 mPa. The results below s are particularly preferred. Furthermore, the cured resin products prepared by the above method were tested, and the Tg of the cured products was consistently above 170°C, indicating good heat resistance. Among them, Examples 11 and 12 showed Tg above 175°C, which is particularly preferred. Further, fiber-reinforced composite materials were prepared using this epoxy resin composition, and the compressive strength at 0°C under humid heat, the compressive strength after impact, and the number of microcracks were measured. The results showed that the compressive strength at 0°C under humid heat was above 1000 MPa, the compressive strength after impact was above 260 MPa, and the number of microcracks was less than 10, indicating good mechanical properties and durability. Among them, Example 11 showed a microcrack count of 5 or less, and Example 12 showed a compressive strength at 0°C under humid heat of 1100 MPa or more, a compressive strength after impact of 270 MPa or more, and a microcrack count of 5 or less, which are particularly preferred results.

[0148] (Examples 14-16)

[0149] The contents of each component and the H / E ratio were changed as shown in Tables 1-2 and 1-3. Otherwise, the epoxy resin composition was prepared in the same manner as in Example 7. As described above, the gelation temperature of the epoxy resin composition was measured, and the results were all above 170°C and below 185°C. This indicates good interfacial adhesion between the adhesive and the resin, and the adhesive maintains its shape. Therefore, this temperature range ensures a uniform interlayer thickness capable of sufficient plastic deformation in fiber-reinforced composites. Examples 14 and 15, with temperatures above 175°C and below 185°C, are particularly preferred results. Next, the viscosity of the epoxy resin composition after holding at 120°C for 240 minutes was measured, and the results were all 200 mPa. Below s, the impregnation properties of the reinforcing fibers are also good. In Examples 14 and 15, the impregnation is 180 mPa. The results below s are particularly preferred. Furthermore, the cured resin products prepared by the above method were tested, and the Tg of the cured products was consistently above 170°C, indicating good heat resistance. Among them, Examples 14 and 15 showed Tg above 175°C, which is particularly preferred. Further, fiber-reinforced composite materials were prepared using this epoxy resin composition, and the compressive strength at 0°C under humid heat, the compressive strength after impact, and the number of microcracks were measured. The results showed that the compressive strength at 0°C under humid heat was above 1000 MPa, the compressive strength after impact was above 260 MPa, and the number of microcracks was less than 10, indicating good mechanical properties and durability. Among them, Example 14 showed a microcrack count of 5 or less, and Example 15 showed a compressive strength at 0°C under humid heat of 1140 MPa, a compressive strength after impact of 275 MPa, and a microcrack count of 5 or less, which are particularly preferred results.

[0150] (Example 17)

[0151] As shown in Table 1-3, 65 parts by weight of "Araldito (registered trademark)" MY721 as component [A], 20 parts by weight of "EPICLON (registered trademark)" 830 as component [B], 61 parts by weight of "Lonzakyua (registered trademark)" M-CDEA as component [C], 26 parts by weight of "Lonzakyua (registered trademark)" M-DIPA as component [D], and 20 parts by weight of "CaneAce (registered trademark)" MX-416 as component [F] are added, and the mixture is stirred at 80°C for 1 hour to prepare an epoxy resin composition. As described above, the gelation temperature of the epoxy resin composition was measured and found to be 177°C. This indicates good interfacial adhesion between the adhesive and resin, and the adhesive maintains its shape. Therefore, this is a particularly preferred temperature for ensuring a uniform interlayer thickness capable of sufficient plastic deformation in fiber-reinforced composites. Next, the viscosity of the epoxy resin composition after holding at 120°C for 240 minutes was measured and found to be 170 mPa. The resin exhibits excellent impregnation properties, particularly with the reinforcing fibers. Furthermore, the cured resin produced using the above method was tested, and its Tg was measured to be 182°C, indicating good heat resistance. Additionally, fiber-reinforced composite materials were prepared using this epoxy resin composition, and the compressive strength at 0°C under humid heat, the compressive strength after impact, and the number of microcracks were measured. The results showed a compressive strength of 1100 MPa at 0°C under humid heat, a compressive strength of 280 MPa after impact, and a number of microcracks of 5 or fewer, demonstrating good mechanical properties and durability.

[0152] (Examples 18 and 19)

[0153] The contents of each component and the types of core-shell rubber particles were changed as shown in Tables 1-3. Otherwise, the epoxy resin composition was prepared in the same manner as in Example 17. As described above, the gelation temperature of the epoxy resin composition was measured, and the results were all above 175°C and below 185°C. This indicates good interfacial adhesion between the adhesive and the resin, and the adhesive maintains its shape. Therefore, this is a particularly preferred temperature for ensuring a uniform interlayer thickness capable of sufficient plastic deformation in fiber-reinforced composites. Next, the viscosity of the epoxy resin composition after holding at 120°C for 240 minutes was measured, and the results were all 200 mPa. Below s, the impregnation properties of the reinforcing fibers are also good. In Example 19, the impregnation level is 170 mPa. The result is particularly preferred. Furthermore, the cured resin products prepared by the above method were tested, and the Tg of the cured products was consistently above 175°C, indicating excellent heat resistance. Further, fiber-reinforced composite materials were prepared using this epoxy resin composition, and the compressive strength at 0°C under humid heat, the compressive strength after impact, and the number of microcracks were measured. The results showed that the compressive strength at 0°C under humid heat was above 1000 MPa, the compressive strength after impact was above 260 MPa, indicating good mechanical properties, and the number of microcracks was below 5, indicating excellent durability. In Example 18, the compressive strength after impact was 280 MPa, which is a particularly preferred result.

[0154] (Example 20)

[0155] As shown in Table 1-3, 65 parts by weight of "Araldito (registered trademark)" MY721 as component [A], 20 parts by weight of "EPICLON (registered trademark)" 830 as component [B], 78 parts by weight of "Lonzakyua (registered trademark)" M-CDEA as component [C], 5 parts by weight of "Lonzakyua (registered trademark)" M-DIPA as component [D], 4 parts by weight of "Lonzakyua (registered trademark)" M-MIPA as component [E], and 20 parts by weight of "CaneAce (registered trademark)" MX-416 as component [F] were added, and the mixture was stirred at 80°C for 1 hour to prepare an epoxy resin composition. As described above, the gelation temperature of the epoxy resin composition was measured and found to be 184°C. This indicates good interfacial adhesion between the adhesive and resin, and the adhesive maintains its shape. Therefore, this is a particularly preferred temperature for ensuring a uniform interlayer thickness capable of sufficient plastic deformation in fiber-reinforced composites. Next, the viscosity of the epoxy resin composition after holding at 120°C for 240 minutes was measured and found to be 120 mPa. The resin exhibits excellent impregnation properties, particularly with the reinforcing fibers. Furthermore, the cured resin produced using the above method was tested, and its Tg (heat resistance) was measured to be 180°C, demonstrating particularly good heat resistance. Moreover, fiber-reinforced composite materials were prepared using this epoxy resin composition, and the compressive strength at 0°C under humid heat, the compressive strength after impact, and the number of microcracks were measured. The results showed a compressive strength of 1120 MPa at 0°C under humid heat, a compressive strength of 280 MPa after impact, and a number of microcracks of 5 or fewer, indicating particularly good mechanical properties and durability.

[0156] (Examples 21 and 22)

[0157] The contents of each component and the types of core-shell rubber particles were changed as shown in Tables 1-4. Otherwise, the epoxy resin composition was prepared in the same manner as in Example 20. As described above, the gelation temperature of the epoxy resin composition was measured, and the results were all above 175°C and below 185°C. This indicates good interfacial adhesion between the adhesive and the resin, and the adhesive maintains its shape. Therefore, this is a particularly preferred temperature for ensuring a uniform interlayer thickness capable of sufficient plastic deformation in fiber-reinforced composites. Next, the viscosity of the epoxy resin composition after holding at 120°C for 240 minutes was measured, and the results were all 180 mPa. The resin composition exhibits good impregnation properties, particularly towards the reinforcing fibers. Furthermore, the cured resin produced using the above method was tested, and the Tg of the cured product was measured, showing values ​​above 175°C, indicating excellent heat resistance. Further, fiber-reinforced composite materials were prepared using this epoxy resin composition, and the compressive strength at 0°C under humid heat, the compressive strength after impact, and the number of microcracks were measured. The results showed that the compressive strength at 0°C under humid heat was above 1000 MPa, the compressive strength after impact was above 260 MPa, and the mechanical properties were excellent. The number of microcracks was 5 or less, and the durability was particularly good. In Example 21, the compressive strength at 0°C under humid heat was 1140 MPa, and the compressive strength after impact was 275 MPa, which are particularly preferred results.

[0158] (Examples 23-26)

[0159] The type of adhesive was changed, but the epoxy resin composition was prepared in the same manner as in Example 2. As described above, the gelation temperature of the epoxy resin composition was measured, and the results were all above 175°C and below 185°C. The interfacial adhesion between the adhesive and the resin is good and the adhesive shape is maintained when the melting point of the adhesive is above 165°C and below 180°C. Therefore, this is a particularly preferred temperature for ensuring a uniform interlayer thickness capable of sufficient plastic deformation in fiber-reinforced composites. Next, the viscosity of the epoxy resin composition after holding at 120°C for 240 minutes was measured, and the results were all 180 mPa. The resin composition exhibits excellent impregnation properties, particularly with the reinforcing fibers. Furthermore, the cured resin produced using the above method was tested, and the Tg of the cured product was consistently above 175°C, demonstrating excellent heat resistance. Further, fiber-reinforced composite materials were prepared using this epoxy resin composition, and the compressive strength at 0°C under humid heat, the compressive strength after impact, and the number of microcracks were measured. The results showed that the compressive strength at 0°C under humid heat was above 1000 MPa, the compressive strength after impact was above 260 MPa, and the number of microcracks was less than 10, indicating good mechanical properties and durability. Of particular preference are the results of Example 21 (5 or fewer microcracks), Example 25 (1100 MPa compressive strength at 0°C under humid heat and 5 or fewer microcracks), and Example 26 (5 or fewer microcracks).

[0160] (Compare Examples 1 and 2)

[0161] The contents of each component were changed as shown in Table 2-1, and the epoxy resin composition was prepared in the same manner as in Example 1. As described above, the gelation temperature of the epoxy resin composition was measured, and the results showed that it was above 175°C and below 185°C. This indicates good interfacial adhesion between the adhesive and the resin, and the adhesive maintains its shape. Therefore, this is a particularly preferred temperature for ensuring a uniform interlayer thickness capable of sufficient plastic deformation in fiber-reinforced composites. Next, the viscosity of the epoxy resin composition after holding at 120°C for 240 minutes was measured. The results showed that Comparative Example 1 had a viscosity of 100 mPa. s, especially the impregnation properties of the reinforcing fibers are also good, but Comparative Example 2 has a pressure of 210 mPa. s, exceeding 200 mPa The impregnation of the reinforcing fibers was poor. Furthermore, the cured resin was prepared using the above method, and the Tg of the cured product was measured. The results showed that Comparative Example 1 had a Tg of 168°C, which is below 170°C, indicating poor heat resistance, while Comparative Example 2 had a Tg of 196°C, showing particularly good heat resistance. Further, fiber-reinforced composite materials were prepared using this epoxy resin composition, and the compressive strength at 0°C under humid heat, the compressive strength after impact, and the number of microcracks were measured. Regarding the compressive strength at 0°C under humid heat, Comparative Example 1 had a compressive strength of 990 MPa, which is below 1000 MPa, indicating poor compressive strength at 0°C under humid heat, while Comparative Example 2 had a compressive strength of 1270 MPa, which is a particularly preferred result. Next, regarding the compressive strength after impact, Comparative Example 1 had a compressive strength of 285 MPa, which is a particularly preferred result, while Comparative Example 2 had a compressive strength of 245 MPa, which is below 260 MPa, indicating poor impact resistance. Furthermore, regarding the number of microcracks, Comparative Examples 1 and 2 both had 5 or fewer, indicating particularly good durability.

[0162] (Comparative Example 3)

[0163] Instead of component [B], "EPICLON (registered trademark)" 850 was used, and the proportions of each component were changed. Otherwise, the epoxy resin composition was prepared in the same manner as in Example 2. As described above, the gelation temperature of the epoxy resin composition was measured and found to be 177°C. This indicates good interfacial adhesion between the adhesive and resin, and the adhesive maintains its shape. Therefore, this is a particularly preferred temperature for ensuring a uniform interlayer thickness capable of sufficient plastic deformation in fiber-reinforced composites. Next, the viscosity of the epoxy resin composition after holding at 120°C for 240 minutes was measured and found to be 180 mPa. The resin exhibits good impregnation properties, particularly towards the reinforcing fibers. Furthermore, a cured resin product prepared using the above method was tested, and its Tg was measured to be 187°C, indicating excellent heat resistance. Further, a fiber-reinforced composite material was prepared using this epoxy resin composition, and its 0° compressive strength under humid heat, post-impact compressive strength, and microcrack count were measured. The results showed that the 0° compressive strength under humid heat was 980 MPa, below 1000 MPa, indicating poor 0° compressive strength under humid heat. However, the post-impact compressive strength was 275 MPa, demonstrating excellent impact resistance, and the number of microcracks was less than 5, indicating good durability.

[0164] (Comparative Example 4)

[0165] As a curing agent, only component [C] was used, and the proportions of each component were changed. Otherwise, the epoxy resin composition was prepared in the same manner as in Example 2. As described above, the gelation temperature of the epoxy resin composition was measured, and the result was 195°C. The adhesive excessively melted in the resin and did not maintain its shape; therefore, this was a temperature at which the interlaminar thickness, which cannot be uniformly ensured for sufficient plastic deformation in fiber-reinforced composites, was not adequately measured. Next, the viscosity of the epoxy resin composition after holding at 120°C for 240 minutes was measured, and the result was 90 mPa. The resin exhibits good impregnation properties, particularly towards the reinforcing fibers. Furthermore, the cured resin produced using the above method was tested, and its Tg was measured to be 178°C, indicating particularly good heat resistance. Further, fiber-reinforced composite materials were prepared using this epoxy resin composition, and the compressive strength at 0°C under humid heat, post-impact compressive strength, and microcrack count were measured. The results showed a particularly good compressive strength at 0°C under humid heat of 1100 MPa, a very good result; a post-impact compressive strength of 255 MPa, below 260 MPa, indicating poor impact resistance; and a microcrack count of 5 or fewer, indicating particularly good durability.

[0166] (Comparative Examples 5-8)

[0167] As a curing agent, only one curing agent other than component [D] or component [E], or component [C] / component [D] / component [E], was used, and the content ratio of each component was changed. Otherwise, the epoxy resin composition was prepared in the same manner as Comparative Example 4. As described above, the gelation temperature of the epoxy resin composition was measured, and the results were all below 170°C. At temperatures higher than the gelation temperature of the epoxy resin composition, the adhesive that reinforces the fiber matrix melts out, which is a temperature at which the interfacial bond strength decreases. Next, the viscosity of the epoxy resin composition after holding at 120°C for 240 minutes was measured, and the results were all greater than 1000 mPa. s, exceeding 200 mPa The impregnation of the reinforcing fibers is poor. Furthermore, the cured resin was prepared using the above method, and the Tg of the cured product was measured. The results showed a Tg of 170°C or higher, indicating good heat resistance. Comparative Examples 5, 6, and 7 showed a Tg of 175°C or higher, which is a particularly preferred result. Further, fiber-reinforced composite materials were prepared using this epoxy resin composition, and the compressive strength at 0°C under humid heat, the compressive strength after impact, and the number of microcracks were measured. The results showed that the compressive strength at 0°C under humid heat was less than 1000 MPa, the compressive strength after impact was less than 260 MPa, and the number of microcracks was more than 10, indicating poor mechanical properties and durability.

[0168] (Comparative Examples 9-11)

[0169] As a curing agent, component [E] or a curing agent other than component [C] / component [D] / component [E] was used instead of component [D], and the proportions of each component were changed. Otherwise, the epoxy resin composition was prepared in the same manner as in Example 2. As described above, the gelation temperature of the epoxy resin composition was measured, and the results were all below 170°C. At temperatures higher than the gelation temperature of the epoxy resin composition, the adhesive that reinforces the fiber matrix melts out, which is a temperature at which the interfacial bond strength decreases. Next, the viscosity of the epoxy resin composition after holding at 120°C for 240 minutes was measured, and the results were all above 200 mPa. The impregnation of the reinforcing fibers is poor. Furthermore, the cured resin produced by the above method was tested, and the Tg of the cured product was measured, showing a temperature above 175°C, indicating particularly good heat resistance. Further, fiber-reinforced composite materials were prepared using this epoxy resin composition, and the compressive strength at 0°C under humid heat, the compressive strength after impact, and the number of microcracks were measured. The results showed that the compressive strength at 0°C under humid heat was below 1000 MPa, the compressive strength after impact was below 260 MPa, and the number of microcracks was above 10, indicating poor mechanical properties and durability.

[0170] (Compare Examples 12 and 13)

[0171] As a curing agent, instead of component [D], one curing agent other than component [C] / component [D] / component [E] was used, and the content ratio of each component was changed. Otherwise, the epoxy resin composition was prepared in the same manner as in Example 7. As described above, the gelation temperature of the epoxy resin composition was measured, and the results were all below 170°C. At temperatures higher than the gelation temperature of the epoxy resin composition, the adhesive that reinforces the fiber matrix melts out, which is a temperature at which the interfacial bond strength decreases. Next, the viscosity of the epoxy resin composition after holding at 120°C for 240 minutes was measured, and the results were all above 200 mPa. The impregnation of the reinforcing fibers is poor. Furthermore, the cured resin produced by the above method was tested, and the Tg of the cured product was measured, showing a temperature above 175°C, indicating particularly good heat resistance. Further, fiber-reinforced composite materials were prepared using this epoxy resin composition, and the compressive strength at 0°C under humid heat, the compressive strength after impact, and the number of microcracks were measured. The results showed that the compressive strength at 0°C under humid heat was below 1000 MPa, the compressive strength after impact was below 260 MPa, and the number of microcracks was above 10, indicating poor mechanical properties and durability.

[0172] [Table 1-1]

[0173] [Table 1-2]

[0174] [Table 1-3]

[0175] [Table 1-4]

[0176] [Table 2-1]

[0177] [Table 2-2]

[0178] Industry availability

[0179] The epoxy resin composition for fiber-reinforced composite materials of the present invention exhibits excellent processability because the resin viscosity injected into the reinforcing fiber matrix remains low for an extended period. Furthermore, it can impart high levels of physical properties (heat resistance, high compressive strength, impact resistance, and durability) to fiber-reinforced composite materials in large structural materials such as aircraft main wings, where the heating rate during curing is sometimes slow. Consequently, advancements in the application of fiber-reinforced composite materials, particularly for aircraft applications, can further be expected to contribute to reduced fuel consumption and reduced emissions of global warming gases due to weight reduction.

Claims

1. An epoxy resin composition for fiber-reinforced composite materials, comprising [A] tetraglycidyl diaminodiphenylmethane, comprising [B] bisphenol F type epoxy resin, comprising [C] 4,4'-methylenebis(3-chloro-2,6-diethylaniline), comprising [D] 4,4'-methylenebis(2,6-diisopropylaniline), comprising [D] 4,4'-methylenebis(2,6-diisopropylaniline), comprising [C] 4,4'-methylenebis(3-chloro-2,6-diethyl ...C] 4,4'-methylenebis(2,6-diisopropylaniline), comprising [C] 4,4'-methylenebis(2,6-diisopropylaniline), comprising [C] 4,4'-methylenebis(2,6-diisopropylaniline), comprising [C] 4,4'-methylenebis(2,6-diisopropylaniline), comprising [C] 4,4'-methylenebis(2,6-diisopropylaniline), comprising [C] 4,4'-methylenebis(2,6-diisopropylaniline), comprising [C] 4,4'-methylenebis(2,6-diisopropylaniline), comprising [C] 4,4'-methylenebis(2,6-diisopropylaniline), comprising [C] 4,4'-methylenebis(2,6-di 2. The epoxy resin composition for fiber-reinforced composite materials according to claim 1, further comprising [E] 4,4'-methylenebis(2-isopropyl-6-methylaniline).

3. The epoxy resin composition for fiber-reinforced composite materials according to claim 1 or 2, further comprising [F] core-shell rubber particles with a volume average particle size in the range of 50 nm or more and 300 nm or less, and whose shell portion comprises epoxy groups.

4. The epoxy resin composition for fiber-reinforced composite materials according to claim 1 or 2, wherein the resin viscosity η, obtained by isothermal measurement using an E-type viscometer after being kept constant at 120°C for 240 minutes, satisfies 20 ≤ η ≤ 200, and the unit of resin viscosity η is mPa. s.

5. The epoxy resin composition for fiber-reinforced composite materials according to claim 1 or 2, wherein the gelation temperature when heated from 70°C at a heating rate of 0.5°C / min is in the range of 170°C or higher and 185°C or lower.

6. A fiber-reinforced composite material comprising a cured product of the epoxy resin composition for fiber-reinforced composite materials according to any one of claims 1 to 5, and a reinforcing fiber substrate.

7. The fiber-reinforced composite material according to claim 6, wherein the reinforcing fiber substrate is a preform formed by bonding together a nonwoven adhesive.

8. The fiber-reinforced composite material according to claim 7, wherein the nonwoven adhesive is made of polyamide with a melting point above 165°C and below 180°C.

9. The fiber-reinforced composite material according to claim 7 or 8, wherein the amount of the nonwoven adhesive attached to the surface of the reinforcing fiber substrate is 0.5 g / m² per side. 2 Above and 10g / m 2 the following.

10. The fiber-reinforced composite material according to claim 6 or 7, wherein the reinforcing fiber constituting the reinforcing fiber substrate is carbon fiber.

11. A method for manufacturing a fiber-reinforced composite material, wherein, An epoxy resin composition for fiber-reinforced composite materials, as described in any one of claims 1 to 5, heated to 50°C or higher and 130°C or lower, is injected into a reinforcing fiber substrate disposed in a molding die heated to 90°C or higher and 180°C or lower, thereby impregnating it and curing it within the molding die.

Citation Information

Patent Citations

  • Sulfur-containing cyclopentenone compound and its preparation

    JP1983008057A

  • Epoxy resin compositions, prepregs, cured composites, and methods of making the same

    JP1999511503A

  • Method for producing epoxy resin composition

    JP2004315572A

  • Epoxy resin composition, fiber-reinforced composite material and method for manufacturing the same

    JP2010150310A

  • Epoxy resin composition for fiber-reinforced composite material, fiber-reinforced composite material, and production method therefor

    CN112313270A