A densely scattered ceramic coating process
Through the intensive spreading ceramic coating process, preheating and surface dry heating is used to form a diffused spreading point structure, the problem of easy cracking of the surface layer in the prior art is solved, the connection strength and earthquake resistance of the coating are improved, and the connection strength and earthquake resistance of the coating are improved, and the The aesthetics of the ceramic coating and the brightness and three-dimensional texture of the dotted paint pattern.
Patent Information
- Application Number
- CN202310808689.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-07-04
- Publication Date
- 2024-11-19
- Estimated Expiration
- 2043-07-04
AI Technical Summary
The existing dot spraying process is performed after the primer is completely cured, resulting in dot spraying only for aesthetics and cannot improve the coating performance, especially the problem of the surface layer being prone to cracking.
The intensive dot-spread ceramic coating process is adopted to form a diffused dot-spread structure through preheating and surface dry heating, spraying primer and topcoat to form a dense ring-shaped reinforced structure, improving connection strength and shock resistance, and reducing cracking risks.
It effectively improves the connection strength and overall earthquake resistance between the coatings, reduces the hidden danger of surface cracking, and at the same time improves the three-dimensional aesthetics of the ceramic coating and the brightness and three-dimensional texture of the dotted paint pattern.
Smart Images

Figure CN116851233B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to ceramic coating, and more particularly to a dense spot-sprinkling ceramic coating process. Background Art
[0002] Ceramic coatings are widely used in products such as automobiles, trains, kitchen equipment and air conditioners due to their good wear resistance, stain resistance and stability.
[0003] Spot spraying is an improvement in the ceramic coating process. The main difference is that a spot layer is set between the primer and the topcoat by spot spraying, which can give the coating a three-dimensional pattern in appearance and change the consistency of the topcoat thickness in performance, so that it has better connection strength and crack resistance with the primer layer.
[0004] Regarding the dot-spraying process, the Chinese patent announcement with announcement number CN106423791B discloses an automatic spray dot-spraying method, the technical points of which are: subjecting the product to electrostatic dust removal; clamping the product online, and then spraying the primer on the product in a suspended state; baking and drying the product sprayed with primer online and then removing it from the line, replacing it with a flat spray fixture to fix it; bringing the fixed product online, rotating it according to the set product, and performing flat spray dot-spraying operations at the same time, which is controlled by adjusting the air pressure and fog pressure of the large-caliber spray gun, and adjusting the pressure according to the size of the product area.
[0005] The above technical solution is sprayed after the primer is completely cured. The applicant found in actual experiments that it can form Figure 4 The granular dot structure shown in the figure is a coating process in which a dot paint pattern and a topcoat are sprayed on top of the primer, so that the dot paint can only play an aesthetic role but cannot improve the coating performance. Therefore, a new solution is needed to solve this problem. Summary of the invention
[0006] In view of the shortcomings of the prior art, the purpose of the present invention is to provide a densely scattered ceramic coating process, which not only improves the three-dimensional aesthetics, but also effectively improves the connection strength between coatings, improves the overall seismic resistance of the coating, and reduces the risk of cracking of the surface layer.
[0007] The above technical objectives of the present invention are achieved through the following technical solutions: a dense dot-sprinkling ceramic coating process for producing a diffuse dot-sprinkling ceramic coating, wherein the diffuse dot-sprinkling ceramic coating includes a primer layer, a dot and a topcoat layer, wherein a single dot is disc-shaped and has a thickened edge and a thinned center; the process steps include: step 1: polishing the surface of the workpiece; step 2: preheating the product at a preheating temperature of 50-60°C; step 3: atomizing and evenly spraying the primer, maintaining the preheating temperature of the workpiece, and using a spray gun to sprinkle and spray paint on the primer; step 4: surface drying heating the product at a surface drying temperature of 80-150°C and a surface drying time of 5-8min; step 5: atomizing and evenly spraying the topcoat; step 6: curing and heating the product at a curing temperature of 260-280°C and a curing time of 8-15min.
[0008] By adopting the above-mentioned technical scheme, the diffusion-type dot-sprinkling ceramic coating formed by the processing of the present application, due to the thick outer and thin inner structure of the dotted points, a dense annular reinforcement structure is formed between the primer layer and the topcoat layer, on the one hand, the three-dimensional adhesion of the topcoat layer is realized, and its connection strength is improved, and on the other hand, the interval support of the primer layer and the topcoat layer is realized, thereby improving the overall seismic resistance of the coating and reducing the risk of cracking; the specific process principle of the diffusion-type dot-sprinkling ceramic coating is to preheat the product first, and spray the primer in the preheated state, so as to improve the fluidity of the paint on the surface of the workpiece when the primer is atomized and sprayed, thereby improving the uniformity and smooth texture of the primer layer; the dot-sprinkling spraying of the paint is carried out at the preheating temperature, so that the dot paint impacts on the fluid primer, forming a wave that spreads outward from the impact point, thereby driving the dot paint to be in a diffused state, that is, forming a thinning medium The paint dots have disc-shaped centers and thickened edges, and each paint dot is cellular when viewed straight on; after the paint dot spraying is completed, the workpiece is surface dried and heated to reduce the fluidity of the primer and the paint dots, thereby avoiding the paint dots being scattered when the topcoat is sprayed, causing the paint dots to fail to have a predetermined shape; the topcoat is sprayed after surface dried and heated. It should be noted that when the topcoat is sprayed, the primer and the paint dots have not yet been completely cured. Therefore, the topcoat sprayed on the primer and the paint dots can produce material penetration with the two, thereby ensuring the adhesion of the topcoat; after the topcoat is atomized and sprayed, the workpiece is cured and heated to achieve simultaneous curing of the primer, the paint dots and the topcoat, thereby ensuring the connection strength of the three; in summary, the ceramic coating process provided by the present application effectively improves the connection strength between coatings, improves the overall shock resistance of the coating, and reduces the risk of cracking of the surface layer compared to the prior art.
[0009] The present invention is further configured as follows: in step 1, 60-80# corundum is used for sandblasting and polishing, so that the surface roughness of the product is maintained at 2.5-3.5 μm.
[0010] The present invention is further configured as follows: the weight percentages of the components of the primer are: silica sol: 25-40; pigment: 12-30; filler: 20-30; deionized water: 2-10; alcohol solvent: 2-10; silane: 30-34; acid catalyst: 0-2; the weight percentages of the components of the spot paint are: silica sol: 25-40; pigment: 12-30; filler: 5-15; deionized water: 2-10; alcohol solvent: 10-30; silane: 30-34; acid catalyst: 0-2; the weight percentages of the components of the topcoat are: silica sol: 40-45; deionized water: 2-10; alcohol solvent: 2-10; silane: 45-50; acid catalyst: 0-5; alcohol solvent: 5-7; non-stick additive: 1-3.
[0011] The present invention is further configured as follows: the weight percentage of the solid content of the primer silica sol is 40-50, and the particle size is 20-25nm; the weight percentage of the solid content of the spot paint silica sol is 30-35, and the particle size is 10-20nm; the weight percentage of the solid content of the topcoat silica sol is 40-50, and the particle size is 10-15nm.
[0012] The present invention is further configured as follows: the primer pigment is white, and the spot paint pigment is a bright color.
[0013] The present invention is further configured as follows: the filler is a mixture of mica powder, fumed silica, alumina powder, cellulose, whisker silicon, precipitated barium sulfate, kaolin, bentonite and silicon carbide.
[0014] The present invention is further configured as follows: the alcohol solvent is selected from several of methanol, ethanol, isopropanol, n-butanol and ethylene glycol monobutyl ether.
[0015] The present invention is further configured as follows: the silane is selected from several kinds of methyltrimethoxysilane, dimethyldimethoxysilane, methyltriethoxysilane, aminosilane, anilinemethyltrimethoxysilane, and ethyl orthosilicate.
[0016] The present invention is further configured as follows: the acidic catalyst is selected from one or more of formic acid, acetic acid, oxalic acid, hydrochloric acid, benzoic acid, salicylic acid, phosphoric acid, and citric acid.
[0017] The present invention is further configured as follows: the non-stick auxiliary agent is selected from several kinds of methyl silicone oil, hydroxy silicone oil and phenyl silicone oil.
[0018] In summary, the present invention has the following beneficial effects: due to the thick outer and thin inner structure of the scattered dots, a dense annular reinforcement structure is formed between the primer layer and the topcoat layer, which, on the one hand, realizes the three-dimensional adhesion of the topcoat layer and improves its connection strength, and on the other hand, realizes the interval support of the primer layer and the topcoat layer, thereby improving the overall seismic resistance of the coating and reducing the risk of cracking; the ceramic coating process provided by the present application, compared with the prior art, effectively improves the connection strength between coatings, improves the overall seismic resistance of the coating, and reduces the risk of cracking of the surface layer; by optimizing the components of the primer, spot paint and topcoat, the brightness of the spot paint pattern of the ceramic coating is effectively improved; by optimizing the silica sol selection of the primer, spot paint and topcoat, the three-dimensional texture of the spot paint pattern of the ceramic coating is improved. BRIEF DESCRIPTION OF THE DRAWINGS
[0019] Figure 1 This is a cross-sectional view of the ceramic coating formed by the present application, and the two sprinkled points shown in this figure are in an independent state;
[0020] Figure 2 This is a cross-sectional view of the ceramic coating formed by the present application, and the three scattered points shown in the figure are in an intersecting state;
[0021] Figure 3 A diagram showing the dotted state of the ceramic coating formed by the processing of this application;
[0022] Figure 4 A scattered state diagram of the technology in the background technology.
[0023] Description of the drawings: 101, primer layer; 102, sprinkled spots; 103, topcoat layer; 104, thickened edge; 105, thinned center. DETAILED DESCRIPTION
[0024] The present invention is further described in detail below in conjunction with the accompanying drawings.
[0025] A densely scattered ceramic coating process, such as Figure 1 , Figure 2 , Figure 3As shown, it is used to produce a diffused dotted ceramic coating, which includes a primer layer 101, dotted spots 102 and a topcoat layer 103. A single dotted spot 102 is disc-shaped, having a thickened edge 104 and a thinned center 105. The ceramic coating structure presents a denser three-dimensional dotted pattern in appearance. In this embodiment, the primer layer 101 is white, and the dotted spots 102 are blue with a transparent base. The entire coating presents a blue and white porcelain color texture when viewed from a distance. In terms of performance, the ceramic coating structure has a thick outer and thin inner structure of the dotted spots 102, thereby forming a dense annular reinforcement structure between the primer layer 101 and the topcoat layer 103. On the one hand, it realizes the three-dimensional adhesion of the topcoat layer 103 and improves its connection strength. On the other hand, it realizes the interval support of the primer layer 101 and the topcoat layer 103, thereby improving the overall seismic resistance of the coating and reducing the risk of cracking.
[0026] A densely scattered ceramic coating process, the process steps include:
[0027] Step 1: Grind the workpiece surface, specifically use 60-80# diamond sand for sandblasting to keep the surface roughness of the product at 2.5-3.5μm.
[0028] Step 2: Preheat the product at a temperature of 50-60°C.
[0029] Step 3: spray the primer evenly through atomization. The air pressure of the spray gun during primer spraying is 2-3 kg. The workpiece is kept at the preheating temperature. The paint is dotted on the primer using a spray gun. The air pressure of the spray gun during dot spraying is 0.3-0.4 kg. Use high air pressure to spray the primer to ensure its density, thereby preventing the primer from being completely washed away by the dot paint. Use low air pressure to spray the dot paint to avoid the dot paint completely washing away the primer or embedding the primer in the form of dots, effectively ensuring the smooth spreading of the dot paint. It should be noted here that the diameter of a single dot 102 can be controlled by adjusting the air pressure. The smaller the spraying air pressure, the larger the diameter of the single dot 102.
[0030] Step 4: Heat the product to dry it on the surface. The surface drying heating temperature is 80-150℃ and the surface drying time is 5-8min.
[0031] Step 5: Atomize and evenly spray the topcoat. The air pressure of the spray gun during topcoat spraying is 2-3 kg, which ensures the density of the coating surface and improves the smoothness of the coating.
[0032] Step 6: Heat the product for curing, the curing temperature is 260-280℃, and the curing time is 8-15min.
[0033] The specific principle of the intensive spot-sprinkling ceramic coating process is to preheat the product first, and then spray the primer in the preheated state, so as to improve the fluidity of the paint on the workpiece surface when the primer is atomized and sprayed, thereby improving the uniformity and smooth texture of the primer layer; the spot spraying of the paint is carried out at the preheating temperature, so that the paint impacts on the primer with fluidity, forming a wave that spreads outward from the impact point, thereby driving the paint to diffuse, that is, forming a disc-shaped paint spot with a thinned center and a thickened edge, and each paint spot is cellular when viewed straight on; after the paint spot spraying is completed, the workpiece is surface-dried and heated to reduce the fluidity of the primer and the paint spot, thereby avoiding When spraying the topcoat, the spot paint is scattered, resulting in the spot paint being unable to have a predetermined shape; the topcoat is sprayed after surface drying and heating. It should be noted that when the topcoat is sprayed, the primer and the spot paint have not yet been completely cured. Therefore, the topcoat sprayed on the primer and the spot paint can produce material penetration with the two, thereby ensuring the adhesion of the topcoat; after completing the atomized spraying of the topcoat, the workpiece is cured and heated to achieve simultaneous curing of the primer, the spot paint and the topcoat, thereby ensuring the connection strength of the three; in summary, the ceramic coating process provided by the present application effectively improves the connection strength between coatings compared to the prior art, and improves the overall seismic resistance of the coating, reducing the risk of cracking of the surface layer.
[0034] In order to improve the brightness of the spot paint pattern of the ceramic coating, the present application optimizes the components of the primer, spot paint and topcoat, as follows:
[0035] The weight percentage of the components of the primer is: silica sol: 25-40; pigment: 12-30; filler: 20-30; deionized water: 2-10; alcohol solvent: 2-10; silane: 30-34; acid catalyst: 0-2;
[0036] The weight percentages of the components of the spot paint are: silica sol: 25-40; pigment: 12-30; filler: 5-15; deionized water: 2-10; alcohol solvent: 10-30; silane: 30-34; acid catalyst: 0-2;
[0037] The weight percentage of the components of the topcoat is: silica sol: 40-45; deionized water: 2-10; alcohol solvent: 2-10; silane: 45-50; acid catalyst: 0-5; alcohol solvent: 5-7; non-stick additive: 1-3;
[0038] The difference in components between primer and spot paint mainly lies in the weight percentage of fillers and alcohol solvents. The primer increases the filler content and reduces the alcohol solvent content. On the one hand, it prevents the primer from being completely penetrated by the spot paint, and on the other hand, it reduces the transparency of the primer, improves the covering effect on the workpiece, and effectively prevents the color difference between the primer and the area impacted by the spot paint due to the original color of the workpiece, mainly to ensure the consistency of the primer color in the area corresponding to the dilution center 105 with the overall color; the spot paint reduces the filler content and increases the alcohol solvent content. On the one hand, it ensures the transparency and color uniformity of the spot paint, and on the other hand, it improves the flowability of the spot paint, so that the spot paint can be better spread out when it impacts the primer, and has a filter-like perspective texture; the topcoat eliminates the use of fillers and pigments, so that it has the best transparency, and adds non-stick additives, so that the coating surface has better anti-fouling ability and smoothness.
[0039] In order to improve the three-dimensional texture of the ceramic coating spot paint pattern, this application optimizes the selection of silica sol for primer, spot paint and topcoat, as follows:
[0040] The solid content weight percentage of the primer silica sol is: 40-50, and the particle size is: 20-25nm;
[0041] The solid content weight percentage of the silica sol for spot painting is: 30-35, and the particle size is: 10-20nm;
[0042] The solid content weight percentage of the topcoat silica sol is: 40-50, and the particle size is: 10-15nm;
[0043] The primer uses silica sol with a high solid content and large particle size to further improve its masking effect on the original color of the workpiece, thereby providing better base color conditions for the spot paint pattern; the spot paint uses silica sol with a low solid content and small particle size to ensure its excellent perspective and uniform color distribution, so that the different thickness areas of the spot paint can present different perspective color depths, thereby enhancing the three-dimensional texture of the spot paint pattern; the topcoat uses silica sol with a high solid content and small particle size to achieve the perspective of the topcoat while ensuring the surface hardness of the ceramic coating.
[0044] It should be noted that in this embodiment, the primer pigment is white and the spot paint pigment is sky blue.
[0045] The filler is specifically composed of mica powder, fumed silica, alumina powder, cellulose, silicon whisker, precipitated barium sulfate, kaolin, bentonite, and silicon carbide.
[0046] The specific components of the alcohol solvent are as follows. The alcohol solvent is selected from several of methanol, ethanol, isopropanol, n-butanol and ethylene glycol monobutyl ether.
[0047] The specific components of silane are as follows. Silane is selected from several kinds of methyltrimethoxysilane, dimethyldimethoxysilane, methyltriethoxysilane, aminosilane, anilinemethyltrimethoxysilane, and ethyl orthosilicate.
[0048] The specific components of the acidic catalyst are as follows. The acidic catalyst is selected from one or more of formic acid, acetic acid, oxalic acid, hydrochloric acid, benzoic acid, salicylic acid, phosphoric acid, and citric acid.
[0049] The specific ingredients of the non-stick aid are as follows. The non-stick aid is selected from several kinds of methyl silicone oil, hydroxy silicone oil and phenyl silicone oil.
[0050] The specific embodiments are merely explanations of the present invention and are not limitations of the present invention. After reading this specification, those skilled in the art may make modifications to the embodiments without any creative contribution as needed. However, such modifications are protected by the patent law as long as they are within the scope of the claims of the present invention.
Claims
1. A densely scattered ceramic coating process, Features: Used for producing a diffused dotted ceramic coating, the diffused dotted ceramic coating comprising a primer layer (101), dotted dots (102) and a topcoat layer (103), wherein each dotted dot (102) is in the shape of a disk and has a thickened edge (104) and a thinned center (105); The weight percentage of the components of the primer is: Silica sol: 25-40; Pigment: 12-30; Filler: 20-30; Deionized water: 2-10; Alcohol solvent: 2-10; Silane: 30-34; Acid catalyst: 0-2; The weight percentages of the components of the spot paint are: Silica sol: 25-40; Pigment: 12-30; Filler: 5-15; Deionized water: 2-10; Alcohol solvent: 10-30; Silane: 30-34; Acid catalyst: 0-2; The components of the topcoat are in percentage by weight: Silica sol: 40-45; Deionized water: 2-10; Alcohol solvent: 2-10; Silane: 45-50; Acid catalyst: 0-5; Alcohol solvent: 5-7; Non-stick additive: 1-3; The process steps include: Step 1: Grind the surface of the workpiece; Step 2: Preheat the product at a temperature of 50-60°C; Step 3: Atomize and spray the primer evenly, keep the workpiece at the preheating temperature, and use a spray gun to spray the paint on the primer; spray the paint at the preheating temperature, so that the paint impacts the primer with fluidity, forming a wave that spreads outward from the impact point, and then drives the paint to diffuse, that is, to form a disc-shaped paint with a thin center and a thickened edge, and each paint point is cell-shaped when viewed from the front; Step 4: Heat the product to dry surface, the surface drying heating temperature is 80-150℃, and the surface drying time is 5-8min; Step 5: Atomize and evenly spray the topcoat; Step 6: Heat the product for curing, the curing temperature is 260-280℃, and the curing time is 8-15min.
2. A densely scattered ceramic coating process according to claim 1, Features: In step 1, 60-80# corundum is used for sandblasting and polishing to keep the surface roughness of the product at 2.5-3.5 μm.
3. A densely scattered ceramic coating process according to claim 1, Features: The solid content weight percentage of the primer silica sol is: 40-50, and the particle size is: 20-25nm; The solid content weight percentage of the paint-pointing silica sol is: 30-35, and the particle size is: 10-20nm; The solid content weight percentage of the topcoat silica sol is 40-50, and the particle size is 10-15 nm.
4. A densely scattered ceramic coating process according to claim 1, Features: The primer pigment is white, and the spot paint pigment is bright color.
5. A densely scattered ceramic coating process according to claim 1, Features: The filler is a mixture of mica powder, fumed silica, alumina powder, cellulose, whisker silicon, precipitated barium sulfate, kaolin, bentonite and silicon carbide.
6. A densely scattered ceramic coating process according to claim 1, Features: The alcohol solvent is selected from methanol, ethanol, isopropanol, n-butanol and ethylene glycol monobutyl ether.
7. A densely scattered ceramic coating process according to claim 1, Features: The silane is selected from methyltrimethoxysilane, dimethyldimethoxysilane, methyltriethoxysilane, aminosilane, anilinemethyltrimethoxysilane, and ethyl orthosilicate.
8. The intensive spot-sprinkling ceramic coating process according to claim 1, Features: The acidic catalyst is selected from one or more of formic acid, acetic acid, oxalic acid, hydrochloric acid, benzoic acid, salicylic acid, phosphoric acid and citric acid.
9. A densely scattered ceramic coating process according to claim 1, Features: The non-stick auxiliary agent is selected from methyl silicone oil, hydroxy silicone oil and phenyl silicone oil.
Citation Information
Patent Citations
An automatic spraying and dotting method
CN106423791B
Construction and application of spread-point coloring archaized effect on surface of stair and wood floor
CN102019801A
Waterproof plate and preparation method thereof
CN108641424A
Dot scattering and spraying device of imitation stone stripe aluminum plateand spraying technology of imitation stone stripe aluminum plate
CN109865612A
Stone grain imitated fluorine-carbon spot-scattering spraying process
CN112122036A