A kind of rigid heat insulation material and preparation method thereof
Through the combination of quartz yarn surface treatment and boron nitride fibers and alumina-based fibers, the problems of high cost and low thermal insulation performance of traditional thermal insulation materials are solved, and the preparation of rigid thermal insulation materials with high strength and good thermal insulation performance are achieved. .
Patent Information
- Application Number
- CN202310646181.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-06-02
- Publication Date
- 2024-11-26
- Estimated Expiration
- 2043-06-02
AI Technical Summary
Traditional rigid thermal insulation materials have high cost and low thermal insulation performance. Although the addition of reinforcement improves strength, it leads to a decrease in porosity and affects the thermal insulation performance.
Using quartz yarn as raw material for surface treatment and drying and sintering, combining boron nitride fibers and alumina-based fibers as reinforced fibers, improve the strength and porosity of the material through interlacing and surface adhesion of silica, and avoid impregnation process. The porosity decreases due to increased medium strength.
A rigid thermal insulation material with low cost, high strength and good thermal insulation performance has been realized, with thermal conductivity of room temperature≤0.055W/(m·K), thermal conductivity of 1100℃≤0.08W/(m·K), compressive strength ≥1.5MPa, tensile strength ≥1.3MPa, density is 0.3-0.5g/cm3.
Smart Images

Figure CN116854494B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of heat-insulating materials, and in particular relates to a rigid heat-insulating material and a preparation method thereof. Background Art
[0002] Traditional rigid thermal insulation materials are mainly made of fiber, binder and dispersed solvent, and are made by filtration or filter pressing followed by drying and sintering. The fiber raw material is usually made of thin-diameter, expensive quartz fiber wool, and the prepared thermal insulation material is expensive. In addition, in order to enhance the strength of the thermal insulation material, additional reinforcing agents need to be added. Although the addition of reinforcing agents enhances the strength, it also brings about the problem of reduced porosity and significantly reduced thermal insulation performance of rigid thermal insulation materials.
[0003] Therefore, how to produce thermal insulation materials with low cost, high strength and high thermal insulation performance has become a technical problem that needs to be solved urgently in this field. Summary of the invention
[0004] In order to solve the disadvantages of the above technical problems, the present invention provides a method for preparing a rigid thermal insulation material. The rigid thermal insulation material prepared by the method has significantly improved strength, and the internal porosity of the rigid thermal insulation material is not reduced, and the thermal insulation performance is good.
[0005] In one aspect, the present invention provides a method for preparing a rigid thermal insulation material, comprising the following steps: surface treating quartz yarn to obtain modified quartz yarn; preparing a thermal insulation material matrix based on the modified quartz yarn and reinforcing fibers; drying and sintering the thermal insulation material matrix to obtain a rigid thermal insulation material;
[0006] Wherein, the reinforcing fiber includes boron nitride fiber, the aspect ratio of the quartz yarn is (100-500):1, and the aspect ratio of the boron nitride fiber is (10-50):1.
[0007] Compared with the prior art, the technical solution of the present invention has the beneficial effect that, by using quartz yarn as a raw material to make the heat insulation material matrix, the strength of the rigid heat insulation material is significantly improved due to the coarseness and high strength of the quartz yarn, and at the same time, the length processing of the quartz yarn is simpler than that of the quartz fiber, which significantly reduces the cost;
[0008] When quartz yarn is used as the raw material, the quartz yarn is thick, resulting in a problem that the pore size between the overlapping skeletons in the thermal insulation material is significantly reduced compared to the ceramic fiber wool as the raw material, and the porosity of the rigid thermal insulation material is easily reduced, resulting in reduced thermal insulation performance; however, by adding boron nitride fiber, the strength of the staggered connection points of the quartz yarn is increased, and at the same time, the problem of reduced porosity caused by increased strength of the staggered connection points of the quartz yarns by using powder to prepare slurry for impregnation is avoided; that is, the reduction in thermal insulation performance of the rigid thermal insulation material is avoided;
[0009] The aspect ratio of the quartz yarn is (100-500):1, and the aspect ratio of the boron nitride fiber is (10-50):1; the quartz yarn is long and the boron nitride fiber is short, so that a large-aperture fiber grid formed by the interlacing of the quartz yarns is realized, and the boron nitride fibers are interlaced and dispersed in the large-aperture fiber grid formed by the interlacing of the quartz yarns and overlapped with the quartz yarns; therefore, the strength of the thermal insulation material matrix is further improved due to the long quartz yarn, and at the same time, the porosity in the thermal insulation material matrix is large and the pores are uniform, so that the thermal insulation material has good thermal insulation performance.
[0010] Furthermore, the reinforcing fibers also include alumina-based fibers, and the aspect ratio of the alumina-based fibers is (10-50):1; preferably, the alumina-based fibers are polycrystalline alumina fibers.
[0011] The beneficial effect of adopting the previous step is that dispersion and overlap are achieved within the large-aperture fiber grid formed by the interlacing of the quartz yarns, further increasing the strength of the rigid thermal insulation material.
[0012] Furthermore, the step of surface treating the quartz yarn comprises:
[0013] The quartz yarn is impregnated in silica sol, and after impregnation, it is dried and solidified to obtain a modified quartz yarn, wherein the mass ratio of the quartz yarn to the silica sol is (30-70):1; preferably, before the quartz sand yarn is impregnated with silica sol, the quartz yarn is roughened.
[0014] The beneficial effect of adopting the previous step is that after the quartz yarn is surface treated, silica is attached to the fiber surface, and the silicon nitride fiber and the quartz yarn are overlapped and sintered. The silicon nitride fiber reacts with the silica attached to the surface of the quartz yarn to achieve high strength at the fiber overlap, which significantly improves the strength of the rigid thermal insulation material; by roughening the surface of the quartz yarn, the problem of small angles when the quartz yarn and alumina-based fibers are parallel or staggered in the thermal insulation material matrix is avoided, and it is also beneficial to achieve the attachment of more silica to the pits on the fiber surface, and it is easy for the pits to become the overlapping points of the fibers, which is ultimately beneficial to the high strength of the silicon nitride fiber overlap.
[0015] Further, the alumina-based fiber is surface treated to obtain a modified alumina-based fiber, the steps of which include: impregnating the alumina-based fiber in silica sol, drying and curing after the impregnation to obtain the modified alumina-based fiber, wherein the mass ratio of the alumina-based fiber to the silica sol is (5-50):1;
[0016] Preferably, the alumina-based fibers are roughened before being impregnated with silica sol to increase the surface roughness of the alumina-based fibers.
[0017] The beneficial effect of adopting the previous step is that the alumina-based fiber is surface treated, and the steps include: after the alumina-based fiber is surface treated, silica is attached to the fiber surface to achieve overlap of the silicon nitride fiber and the alumina-based fiber, and after sintering, the silicon nitride fiber reacts with the silica attached to the surface of the alumina-based fiber to achieve high strength at the fiber overlap, which significantly improves the strength of the rigid thermal insulation material; by roughening the surface of the alumina-based fiber, the problem of small angles when the alumina-based fiber is parallel or staggered in the thermal insulation material matrix is avoided, and it is also beneficial to achieve the attachment of more silica to the pits on the fiber surface, and it is easy for the pits to become overlap points of the fibers, which is ultimately beneficial to the high strength of the silicon nitride fiber overlap.
[0018] Furthermore, the steps of preparing the thermal insulation material matrix include:
[0019] Prepare a quartz yarn solution, disperse the modified quartz yarn in a dispersion medium to obtain the quartz yarn solution; wherein the mass ratio of the modified quartz yarn to the dispersant in the quartz yarn solution is (30-70):1;
[0020] Prepare a reinforcing fiber solution: disperse the boron nitride fiber in a dispersion medium to obtain the reinforcing fiber solution; or disperse the boron nitride fiber and alumina-based fiber in a dispersion medium to obtain the reinforcing fiber solution; the mass ratio of reinforcing fiber to dispersant in the reinforcing fiber solution is (40-100):1;
[0021] The dispersant is water.
[0022] Furthermore, the step of preparing the heat insulation material matrix also includes: pouring the quartz yarn solution into a porous mold with a screen on the bottom, and then filtering out the solvent in the quartz yarn solution;
[0023] When the solvent in the quartz yarn solution is completely or partially filtered out, the reinforcing fiber solution is poured into the porous mold, and the solvent is removed by suction filtration or pressure filtration to obtain a thermal insulation material matrix; preferably, when the reinforcing fiber includes boron nitride fiber, the mass ratio of quartz yarn to boron nitride fiber in the thermal insulation material matrix is (3-5): (2-5);
[0024] When the reinforcing fibers include boron nitride fibers and alumina-based fibers, the mass ratio of quartz yarn to boron nitride fibers and alumina-based fibers in the thermal insulation material matrix is (3-5): (2-5): (0-5).
[0025] The beneficial effect of adopting the previous step is to realize a large-aperture fiber mesh formed by interlacing quartz yarns, and the reinforcing fibers are interlaced and dispersed in the large-aperture fiber mesh formed by interlacing quartz yarns and overlapped with the quartz yarns.
[0026] Furthermore, the modified quartz yarn is subjected to secondary treatment before being used to prepare the quartz yarn solution. The specific process is: attaching paraffin wax to the surface of the modified quartz yarn or attaching an organic modified solution to the surface of the modified quartz yarn to complete the secondary treatment;
[0027] and / or
[0028] When the reinforcing fiber includes boron nitride fiber and alumina-based fiber, the modified alumina-based fiber is subjected to secondary treatment before being used to prepare the reinforcing fiber solution. The specific process is: paraffin is attached to the surface of the modified alumina-based fiber or an organic modified solution is attached to the surface of the modified alumina-based fiber to complete the secondary treatment.
[0029] Furthermore, the organic modification solution includes a reaction monomer and an initiator, and the reaction monomer is a mixture of triethylene glycol and monomer ethylene oxide, acrylate, and methacrylate.
[0030] Preferably, the mass ratio of the paraffin wax or organic modified solution to the quartz yarn is (0.1-0.8):1;
[0031] Preferably, the mass ratio of the paraffin or organic modified solution to the alumina-based fiber is (0.1-0.8):1;
[0032] Preferably, the quartz yarn and / or alumina-based fiber surface is subjected to heat treatment after the organic modification solution is attached thereto, and the heat treatment temperature is 50-150°C;
[0033] Preferably, the initiator is a peroxide; preferably, paraffin wax or an organic modified solution is sprayed or coated on the surface of the quartz yarn and / or alumina-based fiber;
[0034] The beneficial effect of adopting the previous step is that water-blocking or hydrophobic materials can be reattached to the surface of the boron nitride fiber and alumina-based fiber with silica attached to the surface, thereby avoiding the problem of partial shedding of silica attached to the boron nitride fiber and alumina-based fiber during the preparation of the solution.
[0035] Further, the heat insulation material matrix is dried at room temperature for 10-30 hours;
[0036] The sintering is carried out in stages, wherein the sintering temperature of the first stage is 65-75°C and the time is 8-24h; the sintering temperature of the second stage is 135-145°C and the time is 4-24h; and the sintering temperature of the third stage is 1100°C-1500°C and the time is 1-4h.
[0037] The beneficial effect of adopting the previous step is that the sintering of the insulation material matrix is achieved, and at the same time, the silicon and boron on the surface of the quartz yarn react to generate boron silicon compounds to achieve high strength at the joint between the boron nitride and the quartz yarn, thereby achieving high strength of the rigid insulation material.
[0038] Another aspect of the present invention provides a rigid thermal insulation material, which is prepared according to the preparation method of the rigid thermal insulation material; the thermal conductivity at room temperature is ≤0.055W / (m·K), the thermal conductivity at 1100°C is ≤0.08W / (m·K); the compressive strength is ≥1.5MPa, preferably, the compressive strength is ≥2MPa; the strain performance is 3500-5000με; the tensile strength is ≥1.3MPa, preferably, the tensile strength is ≥1.5MPa, preferably, the rigid thermal insulation material density is 0.3-0.5g / cm 3 .
[0039] By adopting the beneficial effect of the previous step, the strength of the rigid thermal insulation material prepared in this application is significantly higher than that of the traditional rigid thermal insulation material, the density of which is 0.3-0.5g / cm 3 , the tensile strength is 0.6-0.7MPa; and the thermal insulation performance is not reduced. BRIEF DESCRIPTION OF THE DRAWINGS
[0040] Figure 1 The 200um microstructure diagram of the rigid thermal insulation material prepared by the present invention;
[0041] Figure 2 This is a 50um microstructure diagram of the rigid thermal insulation material prepared by the present invention;
[0042] Figure 3 This is a 200um microstructure diagram of a rigid insulation material prepared using quartz fiber using the traditional method. DETAILED DESCRIPTION
[0043] To make the purpose, technical solution and advantages of the embodiments of the present invention clearer, the technical solution in the embodiments of the present invention will be clearly and completely described below in combination with the embodiments of the present invention. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0044] Embodiment 1:
[0045] The first embodiment of the present invention provides a method for preparing a rigid thermal insulation material, comprising the following steps: surface treating quartz yarn to obtain modified quartz yarn;
[0046] The step of surface treating the quartz yarn comprises: dipping the quartz yarn in silica sol, drying and curing the quartz yarn after dipping to obtain a modified quartz yarn, wherein the mass ratio of the quartz yarn to the silica sol is 50:1;
[0047] A thermal insulation material matrix is prepared based on modified quartz yarn and reinforcing fibers; the reinforcing fibers include boron nitride fibers and alumina-based fibers, the aspect ratio of the alumina-based fibers is 30:1; and the alumina-based fibers are polycrystalline alumina fibers.
[0048] The modified alumina-based fiber is obtained by surface treating the alumina-based fiber. The step of surface treating the alumina-based fiber includes: impregnating the alumina-based fiber in silica sol, and drying and curing the fiber after impregnation to obtain the modified alumina-based fiber. The mass ratio of the alumina-based fiber to the silica sol is 25:1.
[0049] The aspect ratio of the quartz yarn is 300:1; the aspect ratio of the boron nitride fiber is 30:1.
[0050] The steps of preparing the heat insulation material matrix include: preparing a quartz yarn solution, and the specific process is: dispersing the modified quartz yarn into a dispersion medium to obtain the quartz yarn solution; the mass ratio of the modified quartz yarn to the dispersant in the quartz yarn solution is 50:1;
[0051] The reinforcing fiber solution is prepared by dispersing the boron nitride fiber and the alumina-based fiber in a medium to obtain the reinforcing fiber solution; the mass ratio of the reinforcing fiber to the dispersant in the reinforcing fiber solution is 70:1; and the dispersant is water.
[0052] pouring the quartz yarn solution into a porous mold with a screen at the bottom, and then filtering out the solvent in the quartz yarn solution;
[0053] When the solvent in the quartz yarn solution is completely or partially filtered out, the reinforcing fiber solution is poured into a porous mold with a screen at the bottom, and the solvent is removed by suction filtration and pressure filtration to obtain a thermal insulation material matrix; the mass ratio of quartz yarn to boron nitride fiber and alumina-based fiber in the thermal insulation material matrix is 4:3:2.
[0054] The insulation material matrix is dried at room temperature for 20 hours; the insulation material matrix is sintered in stages, with the first stage sintering temperature at 70°C for 16 hours; the second stage sintering temperature at 140°C for 14 hours; and the third stage sintering temperature at 1300°C for 2.5 hours.
[0055] Thermal conductivity at room temperature is 0.050W / (m·K), thermal conductivity at 1100℃ is 0.07W / (m·K); compressive strength is 1.6MPa; strain performance is 4300με; tensile strength is 1.4MPa; the density of the rigid insulation material is 0.35g / cm 3 .
[0056] Embodiment 2:
[0057] The features of this embodiment that are the same as those of the first embodiment are not described in detail. The features of this embodiment that are different from those of the first embodiment are: a method for preparing a rigid thermal insulation material, further comprising:
[0058] The step of surface treating the quartz yarn further includes: roughening the quartz yarn before impregnating the quartz yarn with silica sol to increase the surface roughness of the quartz fiber;
[0059] Before the alumina-based fiber is impregnated with silica sol, the alumina-based fiber is subjected to a coarsening treatment to increase the surface roughness of the alumina-based fiber.
[0060] The mass ratio of the quartz yarn to the silica sol is 40:1; the aspect ratio of the alumina-based fiber is 20:1; the mass ratio of the alumina-based fiber to the silica sol is 20:1; the aspect ratio of the quartz yarn is 450:1; and the aspect ratio of the boron nitride fiber is 45:1.
[0061] The mass ratio of the modified quartz yarn to the dispersant in the quartz yarn solution is 65:1; the mass ratio of the reinforcing fiber to the dispersant in the reinforcing fiber solution is 80:1;
[0062] The mass ratio of quartz yarn to boron nitride fiber and alumina-based fiber in the thermal insulation material matrix is 4.5:4:4;
[0063] The insulation material matrix is dried at room temperature for 25 hours; the insulation material matrix is sintered in stages, with the first stage sintering temperature at 72°C for 22 hours; the second stage sintering temperature at 143°C for 22 hours; and the third stage sintering temperature at 1400°C for 3.5 hours.
[0064] Thermal conductivity at room temperature is 0.045W / (m·K), thermal conductivity at 1100℃ is 0.06W / (m·K); compressive strength is 2.1MPa; strain performance is 4500με; tensile strength is 1.6MPa, and the density of the rigid insulation material is 0.4g / cm 3 .
[0065] Embodiment 3
[0066] The features of this embodiment that are the same as those of the second embodiment are not repeated here. The features of this embodiment that are different from those of the second embodiment are: a method for preparing a rigid thermal insulation material, further comprising: the modified quartz yarn is subjected to secondary treatment before being used to prepare a quartz yarn solution, and the specific process is: an organic modified solution is attached to the surface of the modified quartz yarn to complete the secondary treatment;
[0067] The modified alumina-based fiber is subjected to secondary treatment before being used to prepare a reinforcing fiber solution, and the specific process is: attaching an organic modification solution to the surface of the modified quartz yarn to complete the secondary treatment;
[0068] The organic modification solution includes a reaction monomer and an initiator, wherein the reaction monomer is a mixture of triethylene glycol and monomer ethylene oxide; the initiator is a peroxide, specifically hydrogen peroxide;
[0069] The mass ratio of the organic modified solution to the quartz yarn is 0.9:1; the mass ratio of the organic modified solution to the alumina-based fiber is 0.9:1;
[0070] The quartz yarn and alumina-based fiber surfaces are subjected to heat treatment after the organic modification solution is attached thereto, and the heat treatment temperature is 120° C.;
[0071] Specifically, the organic modified solution is sprayed on the surface of quartz yarn and alumina-based fiber.
[0072] The mass ratio of the quartz yarn to the silica sol is 40:1; the aspect ratio of the alumina-based fiber is 15:1; the mass ratio of the alumina-based fiber to the silica sol is 15:1; the aspect ratio of the quartz yarn is 200:1; and the aspect ratio of the boron nitride fiber is 15:1.
[0073] The mass ratio of the modified quartz yarn to the dispersant in the quartz yarn solution is 40:1; the mass ratio of the reinforcing fiber to the dispersant in the reinforcing fiber solution is (40-100):1;
[0074] The mass ratio of quartz yarn to boron nitride fiber and alumina-based fiber in the thermal insulation material matrix is 3.5:2.5:1.5;
[0075] The insulation material matrix is dried at room temperature for 15 hours; the insulation material matrix is sintered in stages, with the first stage sintering temperature at 68°C for 12 hours; the second stage sintering temperature at 138°C for 10 hours; and the third stage sintering temperature at 1200°C for 2 hours.
[0076] Thermal conductivity at room temperature is 0.045W / (m·K), thermal conductivity at 1100℃ is 0.065W / (m·K); compressive strength is 2.2MPa; strain performance is 4500με; tensile strength is 1.7MPa, and the density of the rigid insulation material is 0.45g / cm3 .
[0077] Embodiment 4:
[0078] The features common to the third embodiment are not described in detail here. The features different from the third embodiment are as follows:
[0079] The modified quartz yarn is subjected to secondary treatment before being used to prepare the quartz yarn solution. The specific process is: paraffin is attached to the surface of the modified quartz yarn to complete the secondary treatment;
[0080] The modified alumina-based fiber is subjected to secondary treatment before being used to prepare the reinforcing fiber solution. The specific process is: paraffin is attached to the surface of the modified alumina-based fiber to complete the secondary treatment;
[0081] The mass ratio of paraffin wax to quartz yarn is 0.6:1; the mass ratio of paraffin wax to alumina-based fiber is 0.6:1;
[0082] The quartz yarn and the alumina-based fiber surfaces are attached with an organic modified solution and then heat treated at a temperature of 120° C. Specifically, the paraffin melt is sprayed on the quartz yarn and the alumina-based fiber surfaces.
[0083] Thermal conductivity at room temperature is 0.042W / (m·K), thermal conductivity at 1100℃ is 0.060W / (m·K); compressive strength is 2.1MPa; strain performance is 4600με; tensile strength is 1.65MPa, and the density of the rigid insulation material is 0.43g / cm 3 .
[0084] pass Figure 1 It can be shown that the rigid thermal insulation material prepared by the method of the present application using quartz yarn has uniformly interlaced fibers inside and uniformly distributed pores, contains relatively long fibers and the overall fibers are well-arranged, there are no particles attached to the fiber surface, and there is no phenomenon that some pores are blocked by particles; Figure 2 The thermal conductivity of the medium product at room temperature is 0.042W / (m·K), and the thermal conductivity at 1100℃ is 0.060W / (m·K); the compressive strength is 2.1MPa; the strain performance is 4600με; the tensile strength is 1.65MPa, and the density of the rigid insulation material is 0.43g / cm3.
[0085] pass Figure 2 It can be shown that the rigid thermal insulation material prepared by the method of the present application using quartz yarn has uniformly interlaced fibers inside and uniformly distributed pores, contains relatively long fibers and the overall fibers are well-arranged, there are no particles attached to the fiber surface, and there is no phenomenon that some pores are blocked by particles; Figure 2The thermal conductivity of the medium product at room temperature is 0.042W / (m·K), and the thermal conductivity at 1100℃ is 0.060W / (m·K); the compressive strength is 2.1MPa; the strain performance is 4600με; the tensile strength is 1.65MPa, and the density of the rigid insulation material is 0.43g / cm3.
[0086] pass Figure 3 It can be shown that the rigid thermal insulation material prepared by the traditional method using quartz fibers has very uneven fiber interlacing and uneven pore distribution. The overall fibers are relatively short, particles are attached to the fiber surface, and some pores are blocked by particles. Figure 1 The thermal conductivity of the product at room temperature is 0.05W / (m·K), the thermal conductivity at 1100℃ is 0.07W / (m·K); the compressive strength is 0.7MPa; the tensile strength is 0.6MPa, and the density of the rigid insulation material is 0.43g / cm 3 .
[0087] The above is only a specific embodiment of the present invention, but the protection scope of the present invention is not limited thereto. Any person skilled in the art can easily think of changes or substitutions within the technical scope disclosed by the present invention, which should be included in the protection scope of the present invention. Therefore, the protection scope of the present invention should be based on the protection scope of the claims.
Claims
1. A method for preparing a rigid thermal insulation material, characterized in that: The following steps are involved: Surface treatment is performed on the quartz yarn to obtain modified quartz yarn; Preparation of thermal insulation material matrix based on modified quartz yarn and reinforcing fibers; Wherein, the reinforcing fiber comprises boron nitride fiber, the aspect ratio of the quartz yarn is (100-500):1, and the aspect ratio of the boron nitride fiber is (10-50):1; The steps of preparing the thermal insulation material matrix include: Preparing a quartz yarn solution: dispersing the modified quartz yarn in a dispersant to obtain the quartz yarn solution; wherein the mass ratio of the modified quartz yarn to the dispersant in the quartz yarn solution is (30-70):1; Preparing a reinforcing fiber solution: dispersing the boron nitride fiber in a dispersant to obtain the reinforcing fiber solution; the mass ratio of reinforcing fiber to dispersant in the reinforcing fiber solution is (40-100):1; the dispersant is water; The step of preparing the thermal insulation material matrix also includes: pouring the quartz yarn solution into a porous mold with a screen on the bottom, and then filtering out the solvent in the quartz yarn solution; when the solvent in the quartz yarn solution is completely or partially filtered out, pouring the reinforcing fiber solution into the porous mold, and removing the solvent by suction filtration or pressure filtration to obtain the thermal insulation material matrix; Drying and sintering the heat insulation material matrix to obtain a rigid heat insulation material; The step of surface treating the quartz yarn comprises: dipping the quartz yarn in silica sol, drying and curing the quartz yarn after dipping to obtain modified quartz yarn, wherein the mass ratio of the quartz yarn to the silica sol is (30-70):1; Before the quartz yarn is impregnated with silica sol, the quartz yarn is firstly roughened.
2. The method for preparing a rigid thermal insulation material according to claim 1, characterized in that: The reinforcing fiber further comprises an alumina-based fiber, and the aspect ratio of the alumina-based fiber is (10-50):1; The step of preparing the reinforcing fiber solution further comprises: dispersing the boron nitride fiber and the alumina-based fiber in a dispersant to obtain the reinforcing fiber solution.
3. The method for preparing a rigid thermal insulation material according to claim 2, characterized in that: The modified alumina-based fiber is obtained by surface treating the alumina-based fiber, and the steps include: impregnating the alumina-based fiber in silica sol, drying and curing after the impregnation to obtain the modified alumina-based fiber, wherein the mass ratio of the alumina-based fiber to the silica sol is (5-50):
1.
4. The method for preparing a rigid thermal insulation material according to claim 3, characterized in that: Before the alumina-based fibers are impregnated with silica sol, the alumina-based fibers are firstly roughened.
5. The method for preparing the rigid thermal insulation material according to claim 3, characterized in that: When the reinforcing fibers include boron nitride fibers, the mass ratio of quartz yarn to boron nitride fibers in the thermal insulation material matrix is (3-5): (2-5); when the reinforcing fibers include boron nitride fibers and alumina-based fibers, the mass ratio of quartz yarn to boron nitride fibers and alumina-based fibers in the thermal insulation material matrix is (3-5): (2-5): (0-5).
6. The method for preparing a rigid thermal insulation material according to claim 1 or 2, characterized in that: The modified quartz yarn is subjected to secondary treatment before being used to prepare the quartz yarn solution. The specific process is: attaching paraffin wax to the surface of the modified quartz yarn or attaching an organic modified solution to the surface of the modified quartz yarn to complete the secondary treatment; and / or When the reinforcing fiber includes boron nitride fiber and alumina-based fiber, the modified alumina-based fiber is subjected to secondary treatment before being used to prepare the reinforcing fiber solution. The specific process is: paraffin is attached to the surface of the modified alumina-based fiber or an organic modified solution is attached to the surface of the modified alumina-based fiber to complete the secondary treatment.
7. The method for preparing a rigid thermal insulation material according to claim 6, characterized in that: The organic modification solution comprises a reaction monomer and an initiator, wherein the reaction monomer is a mixture of triethylene glycol and monomer ethylene oxide, acrylate, or methacrylate.
8. The method for preparing a rigid thermal insulation material according to claim 1, characterized in that: Dry the thermal insulation material matrix at room temperature for 10-30 hours; The sintering is carried out in stages, wherein the sintering temperature of the first stage is 65-75°C and the time is 8-24h; the sintering temperature of the second stage is 135-145°C and the time is 4-24h; and the sintering temperature of the third stage is 1100°C-1500°C and the time is 1-4h.
9. A rigid thermal insulation material, characterized in that: The rigid thermal insulation material is prepared according to the preparation method of the rigid thermal insulation material according to any one of claims 1 to 8; the thermal conductivity of the rigid thermal insulation material at room temperature is ≤0.035W / (m•K), and the thermal conductivity at 1100°C is ≤0.08W / (m•K); the compressive strength is ≥1.5MPa, the strain performance is 3500-5000με; and the tensile strength is ≥1.3MPa.
Citation Information
Patent Citations
Preparation method of lightweight rigid heat insulation material
CN104909729A
Method for improving strain performance of thermal insulation material used for high-temperature-resistant sandwich structure, and material prepared by using same
CN106626581A
Light efficient heat protection and insulation integrated thermal protection material and preparation method thereof
CN111908932A
Modification treatment method of chopped glass fibers
CN113773458A
Frequency selection, electromagnetic shielding, heat insulation, light weight and impact resistance integrated three-dimensional fabric composite material and preparation method thereof
CN114381841A