A method for comprehensive purification of copper electrolytic liquid using high-temperature and high-pressure oxidation process
By using a high-temperature and high-pressure oxidation process to separate impurities from the copper electrolytic solution, the problem of impurity separation in the copper electrolytic refining process has been solved, achieving efficient purification with no wastewater or waste gas emissions and improving the quality and yield of copper products.
Patent Information
- Application Number
- CN202310635366.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-05-31
- Publication Date
- 2026-11-17
- Estimated Expiration
- 2043-05-31
AI Technical Summary
In existing copper electrolytic refining processes, impurities such as nickel, iron, arsenic, antimony, and bismuth in the copper electrolytic solution are difficult to separate effectively, resulting in substandard cathode copper quality and the generation of black copper slag and arsine gas that pollutes the environment.
A high-temperature and high-pressure oxidation process is adopted. The copper electrolytic solution is neutralized with lime, and then oxygen is introduced into the pressure vessel to carry out the oxidation reaction, forming arsenic, antimony and bismuth impurity precipitates. The precipitates are then separated by filtration, evaporation crystallization and electrowinning to remove copper, thus achieving the separation of copper from impurities.
This method effectively separates copper from impurities, avoids the generation of black copper slag, reduces waste gas and wastewater emissions, improves the direct copper recovery rate of the copper production system, and yields qualified electrowinning copper and electrowinning copper powder products.
Smart Images

Figure CN116856014B_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of copper electrolytic refining hydrometallurgical technology, and in particular to a method for comprehensively purifying copper electrolytic liquid using a high-temperature and pressure oxidation process. Background Technology
[0002] During copper electrolytic refining, as the crude copper anode dissolves continuously, the composition of the electrolyte changes constantly. The concentration of copper ions increases, while impurities such as nickel, iron, arsenic, antimony, and bismuth accumulate. To maintain the concentrations of copper, acid, and impurities within the specified ranges, the electrolyte must be adjusted, and a portion of the electrolyte must undergo open-circuit purification to remove impurities such as copper, nickel, arsenic, antimony, and bismuth, ensuring the normal operation of the electrolysis process. The purified electrolyte is typically referred to as the copper post-electrolysis solution. Purification of the copper post-electrolysis solution is an essential and crucial step in copper electrolytic refining, directly affecting the quality of the cathode copper.
[0003] Induced electrodeposition for the removal of copper, arsenic, antimony, and bismuth is a widely used industrial method for purifying copper electrolytic electrolyte. This involves periodically circulating the extracted electrolyte through multiple stages of copper electrolytic cells, causing impurities such as arsenic, antimony, and bismuth to be deposited along with copper at the cathode. During the electrodeposition process, the first few cells produce plate-shaped cathode copper, the middle cells produce black copper plates, and the later cells produce black copper slag. The last one or two cells may produce arsine gas. The subsequent processing of the cathode copper, black copper plates, and black copper slag produced by this method is cumbersome and inconvenient for utilization. Copper and arsenic, antimony, and bismuth ions are not separated and cannot form separate open circuits; simultaneously, the produced arsine gas pollutes the environment and is difficult to treat. Summary of the Invention
[0004] To address the aforementioned technical problems, this invention provides a method for comprehensively purifying copper electrolytic wastewater using a high-temperature and pressure oxidation process.
[0005] To achieve the above objectives, the technical solution of the present invention is as follows: A method for comprehensively purifying copper electrolytic wastewater using a high-temperature and pressure oxidation process, the method comprising the following steps: S1. Neutralization: Solid lime is added to the copper electrolysis solution to neutralize the solution to a pH of 1.5-2.5, resulting in a neutralized slurry. S2, Pressurized purification: The neutralized slurry obtained in step S1 is pumped into a pressurized kettle, heated to above 130°C, oxygen is introduced, oxygen partial pressure is above 0.4 MPa, and reaction time is above 1.0 h. S3. Filtration: After the pressure purification reaction is completed, the filter is filtered. The filtrate obtained is the purified liquid, and the filter residue is arsenic, antimony, bismuth, iron and calcium slag. S4. Evaporation and crystallization: The purified liquid obtained in step S3 is evaporated and crystallized with a volume evaporation rate of 60-70%, a crystallization temperature of 60℃ or above, and a crystallization time of 8 hours or above. The liquid is then filtered by centrifuge to obtain crude copper sulfate and crystallization mother liquor. S5. First-stage electrowinning copper removal: Electrowinning copper removal is performed on the crystallization mother liquor obtained in step S4 to obtain electrowinning copper. The conditions for first-stage electrowinning copper removal are a temperature above 50℃ and a current density of 200A / m. 2 The concentration of copper ions in the solution after copper removal is controlled to be above 8 g / L. S6. Two-stage electrodeposition copper removal: The copper removal solution obtained in step S5 is subjected to two-stage electrodeposition copper removal to obtain electrodeposited copper powder. The conditions for two-stage electrodeposition copper removal are a temperature above 50℃ and a current density of 500A / m. 2 The copper ion concentration in the electrowinning solution is above 1 g / L, resulting in a copper removal final solution. This copper removal final solution is then connected to the existing production process.
[0006] In step S2, the neutralized slurry obtained in step S1 is pumped into a pressure vessel, heated to 130-140°C, oxygen is introduced, the oxygen partial pressure is 0.4-0.5 MPa, and the reaction time is 1.0-2.0 h.
[0007] In step S4, the purified liquid obtained in step S3 is evaporated and crystallized at a temperature of 60-70°C for 8-10 hours, and then filtered by centrifuge to obtain crude copper sulfate and crystallization mother liquor.
[0008] In step S5, the mother liquor obtained in step S4 is subjected to electrowinning to remove copper, resulting in electrowinning copper. The conditions for the first stage of electrowinning are a temperature of 50-60℃ and a current density of 200-250 A / m. 2 The concentration of copper ions in the solution after copper removal is controlled to be 8-13 g / L.
[0009] In step S6, the copper-free solution obtained in step S5 undergoes a two-stage electrowinning process to remove copper, yielding electrowinning copper powder. The conditions for the two-stage electrowinning are a temperature of 50-60℃ and a current density of 500-1000 A / m. 2 After electrowinning, the copper ion concentration in the solution is 1-3 g / L, yielding the final copper-removed solution, which is then connected to the existing production process.
[0010] The beneficial effects of this invention are: (1) This invention employs a method of neutralizing the acid in the electrolyte with lime and precipitating arsenic, antimony, and bismuth impurities under pressure to create an open circuit. This method comprehensively removes iron, arsenic, antimony, and bismuth impurities, achieving separation of copper from impurities and complete opening of the iron, arsenic, antimony, and bismuth circuit. After purification, the solution can be directly followed by a copper electrowinning process to obtain qualified electrowinning copper and electrowinning copper powder products. This method is simple, produces no waste gas or wastewater discharge, does not pollute the environment, and does not introduce impurity elements into the system. It is a novel method for purifying copper electrolytic solution. (2) This invention achieves the separation of copper from iron, arsenic, antimony and bismuth impurity elements, fundamentally solves the problem of black copper slag production, has a simple process, no wastewater or waste gas emissions, does not consume copper ions in the electrolyte, and does not introduce impurity elements into the system.
[0011] (3) The present invention can remove impurities in the copper electrolysis solution in one step. After purification, the solution is followed by the subsequent electrowinning copper removal process, and qualified electrowinning copper and electrowinning copper powder can be obtained directly.
[0012] (4) The present invention uses a portion of the copper electrolytic liquid that needs to be purified extracted from the copper electrolytic cell, neutralizes and consumes part of the acid, and then uses a high temperature and pressure oxidation process to oxidize the iron, arsenic, antimony and bismuth impurity ions that are inherent in the copper electrolytic liquid. The impurities ions precipitate under high temperature conditions and enter the slag. After the reaction is complete, liquid-solid separation is carried out, and the purified slag is iron, arsenic, antimony and bismuth calcium slag, thus achieving the purpose of removing iron, arsenic, antimony and bismuth impurity ions in one step.
[0013] (5) The solution purified by the present invention is used in the subsequent copper electrowinning process. No black copper plate or black copper powder is generated during the electrowinning process, and the generation of harmful arsine gas is avoided. Qualified electrowinning copper and electrowinning copper powder can be obtained, realizing the complete open circuit of copper and improving the direct copper recovery rate in the copper production system.
[0014] (6) Solid lime, i.e. calcium oxide, is used for neutralization. Excess calcium will form gypsum slag. The process will not cause sulfate and calcium ions to accumulate in the system. No wastewater or waste gas is generated, and the environment is not polluted. Attached Figure Description
[0015] Figure 1 This is a process flow diagram of the present invention. Detailed Implementation
[0016] To make the objectives, technical solutions, and advantages of this invention clearer, the invention will be further described in detail below with reference to specific embodiments. It should be understood that these descriptions are merely exemplary and not intended to limit the scope of the invention. Furthermore, descriptions of well-known structures and technologies are omitted in the following description to avoid unnecessarily obscuring the concepts of the invention.
[0017] Example 1 Table 1 shows the composition (g / L) of the copper electrolysis solution after Example 1.
[0018] Take the copper electrolysis solution with the composition shown in Table 1, add lime to neutralize the solution to a pH of 1.5, add the neutralized slurry to a pressure vessel, heat to 130℃, introduce oxygen, control the oxygen partial pressure at 0.4 MPa, react for 2.0 h, cool and open the vessel, filter to obtain purified residue; the purified solution enters the evaporation crystallization process, evaporation temperature 60℃, evaporation time 8 h, volume evaporation rate 70%, to obtain crude copper sulfate and crystallization mother liquor; the crystallization mother liquor enters a copper removal process, temperature 55℃, current density 200 A / m 2 The copper ion concentration in the solution after the first copper removal stage is 13 g / L; the solution after the first copper removal stage enters the second copper removal stage at a temperature of 50℃ and a current density of 500 A / m. 2 After electrowinning, the copper ion concentration in the solution is 3 g / L. The solution after the second stage of copper removal is connected to the existing production process.
[0019] The Cu+Ag content in the produced electrolytic copper and copper powder reached over 99.90%. The composition and removal rate of impurities in the purified liquid after high-temperature and high-pressure oxidation are shown in Table 2.
[0020] .
[0021] Example 2 Table 3 shows the composition (g / L) of the copper electrolysis solution after Example 2.
[0022] Take the copper electrolysis solution with the components listed in Table 3, add lime to neutralize the solution to a pH of 2.0, add the neutralized slurry to a pressure vessel, heat to 140℃, introduce oxygen, control the oxygen partial pressure at 0.4 MPa, react for 1.5 hours, cool and open the vessel, filter to obtain purified residue, the purified liquid enters the evaporation crystallization process, evaporation temperature 70℃, evaporation time 9 hours, volume evaporation rate 60%, to obtain crude copper sulfate and crystallization mother liquor; the crystallization mother liquor enters a copper removal process, temperature 60℃, current density 250 A / m 2 The copper ion concentration in the solution after the first copper removal stage is 8.48 g / L; the solution after the first copper removal stage enters the second copper removal stage at a temperature of 55℃ and a current density of 1000 A / m. 2 After electrowinning, the copper ion concentration in the solution is 2.05 g / L. The solution after the second stage of copper removal is connected to the existing production process.
[0023] The Cu+Ag content in the produced electrolytic copper and copper powder reached over 99.90%. The composition and removal rate of impurities in the purified liquid after high-temperature and high-pressure oxidation are shown in Table 4.
[0024] .
[0025] Example 3 Table 5 shows the composition (g / L) of the copper electrolysis solution after the examples.
[0026]
[0027] Take the copper electrolytic solution from Table 5, add lime to neutralize it to a pH of 2.5, add the neutralized slurry to a pressure vessel, heat to 135℃, introduce oxygen, control the oxygen partial pressure at 0.5 MPa, react for 1.0 hour, cool and open the vessel, filter to obtain purified residue, the purified liquid enters the evaporation crystallization process, evaporation temperature 65℃, evaporation time 10 hours, volume evaporation rate 68%, to obtain crude copper sulfate and crystallization mother liquor; the crystallization mother liquor enters the first copper removal process, temperature 58℃, current density 230 A / m 2 The copper ion concentration in the solution after the first copper removal stage is 10.20 g / L; the solution after the first copper removal stage enters the second copper removal stage at a temperature of 60℃ and a current density of 700 A / m. 2 After electrowinning, the copper ion concentration in the solution is 2.58 g / L. The solution after the second stage of copper removal is connected to the existing production process.
[0028] The Cu+Ag content in the produced electrolytic copper and copper powder reached over 99.90%. The composition and removal rate of impurities in the purified liquid after high-temperature and high-pressure oxidation are shown in Table 6.
[0029] .
[0030] Example 4 A method for comprehensively purifying copper electrolytic wastewater using a high-temperature and pressure oxidation process, the method comprising the following steps: S1. Neutralization: Solid lime is added to the copper electrolysis solution to neutralize the solution to pH 1.5, resulting in a neutralized slurry. S2, Pressurized purification: The neutralized slurry obtained in step S1 is pumped into a pressurized kettle, heated to 130°C, oxygen is introduced, oxygen partial pressure is 0.4 MPa, and reaction time is 1.0 h. S3. Filtration: After the pressure purification reaction is completed, the filter is filtered. The filtrate obtained is the purified liquid, and the filter residue is arsenic, antimony, bismuth, iron and calcium slag. S4. Evaporation and crystallization: The purified liquid obtained in step S3 is evaporated and crystallized with a volume evaporation rate of 60%, a crystallization temperature of 60℃, and a crystallization time of 8 hours. The liquid is then filtered by centrifuge to obtain crude copper sulfate and crystallization mother liquor. S5. First-stage electrowinning copper removal: Electrowinning copper removal is performed on the crystallization mother liquor obtained in step S4 to obtain electrowinning copper. The conditions for first-stage electrowinning copper removal are a temperature of 50℃ and a current density of 200A / m. 2 The concentration of copper ions in the solution after copper removal is controlled to be 8 g / L. S6. Two-stage electrodeposition copper removal: The copper removal solution obtained in step S5 is subjected to two-stage electrodeposition copper removal to obtain electrodeposited copper powder. The conditions for two-stage electrodeposition copper removal are a temperature of 50℃ and a current density of 500A / m. 2 After electrowinning, the copper ion concentration in the solution is 1 g / L, resulting in the copper removal final solution, which is then connected to the existing production process.
[0031] Example 5 A method for comprehensively purifying copper electrolytic wastewater using a high-temperature and pressure oxidation process, the method comprising the following steps: S1. Neutralization: Solid lime is added to the copper electrolysis solution to neutralize the solution to pH 2.5, resulting in a neutralized slurry. S2, Pressurized purification: The neutralized slurry obtained in step S1 is pumped into a pressurized kettle, heated to 140°C, oxygen is introduced, oxygen partial pressure is 0.5 MPa, and reaction time is 2.0 h. S3. Filtration: After the pressure purification reaction is completed, the filter is filtered. The filtrate obtained is the purified liquid, and the filter residue is arsenic, antimony, bismuth, iron and calcium slag. S4. Evaporation and crystallization: The purified liquid obtained in step S3 is subjected to evaporation and crystallization with a volume evaporation rate of 70%, a crystallization temperature of 70℃, and a crystallization time of 10 hours. The liquid is then filtered by centrifuge to obtain crude copper sulfate and crystallization mother liquor. S5. First-stage electrowinning copper removal: Electrowinning copper removal is performed on the crystallization mother liquor obtained in step S4 to obtain electrowinning copper. The conditions for first-stage electrowinning copper removal are a temperature of 60℃ and a current density of 250A / m. 2 The concentration of copper ions in the solution after copper removal was controlled to be 13 g / L. S6. Two-stage electrodeposition copper removal: The copper removal solution obtained in step S5 is subjected to two-stage electrodeposition copper removal to obtain electrodeposited copper powder. The conditions for two-stage electrodeposition copper removal are a temperature of 60℃ and a current density of 1000A / m. 2 After electrowinning, the copper ion concentration in the solution is 3 g / L, resulting in a copper removal final solution. This copper removal final solution is then connected to the existing production process.
[0032] It should be understood that the specific embodiments described above are merely illustrative or explanatory of the principles of the invention and do not constitute a limitation thereof. Therefore, any modifications, equivalent substitutions, improvements, etc., made without departing from the spirit and scope of the invention should be included within the protection scope of the invention. Furthermore, the appended claims are intended to cover all variations and modifications falling within the scope and boundaries of the appended claims, or equivalent forms of such scope and boundaries.
Claims
1. A method for comprehensively purifying copper electrolytic wastewater using a high-temperature and high-pressure oxidation process, characterized in that, The method includes the following steps: S1. Neutralization: Solid lime is added to the copper electrolysis solution to neutralize the solution to a pH of 1.5-2.5, resulting in a neutralized slurry. S2, Pressurized purification: The neutralized slurry obtained in step S1 is pumped into a pressurized kettle, heated to above 130°C, oxygen is introduced, oxygen partial pressure is above 0.4 MPa, and reaction time is above 1.0 h. S3. Filtration: After the pressure purification reaction is completed, the filter is filtered. The filtrate obtained is the purified liquid, and the filter residue is arsenic, antimony, bismuth, iron and calcium slag. S4. Evaporation and crystallization: The purified liquid obtained in step S3 is evaporated and crystallized with a volume evaporation rate of 60-70%, a crystallization temperature of 60℃ or above, and a crystallization time of 8 hours or above. The liquid is then filtered by centrifuge to obtain crude copper sulfate and crystallization mother liquor. S5. First-stage electrowinning copper removal: Electrowinning copper removal is performed on the crystallization mother liquor obtained in step S4 to obtain electrowinning copper. The conditions for first-stage electrowinning copper removal are a temperature above 50℃ and a current density of 200A / m. 2 The concentration of copper ions in the solution after copper removal is controlled to be above 8 g / L. S6. Two-stage electrodeposition copper removal: The copper removal solution obtained in step S5 is subjected to two-stage electrodeposition copper removal to obtain electrodeposited copper powder. The conditions for two-stage electrodeposition copper removal are a temperature above 50℃ and a current density of 500A / m. 2 The copper ion concentration in the electrowinning solution is above 1 g / L, resulting in a copper removal final solution. This copper removal final solution is then connected to the existing production process.
2. The method for comprehensively purifying copper electrolytic solution using a high-temperature and pressure oxidation process according to claim 1, characterized in that, In step S2, the neutralized slurry obtained in step S1 is pumped into a pressure vessel, heated to 130-140°C, oxygen is introduced, the oxygen partial pressure is 0.4-0.5 MPa, and the reaction time is 1.0-2.0 h.
3. The method for comprehensively purifying copper electrolytic solution using a high-temperature and pressure oxidation process according to claim 1, characterized in that, In step S4, the purified liquid obtained in step S3 is evaporated and crystallized at a temperature of 60-70°C for 8-10 hours. The liquid is then filtered by centrifugation to obtain crude copper sulfate and crystallization mother liquor.
4. The method for comprehensively purifying copper electrolytic solution using a high-temperature and pressure oxidation process according to claim 1, characterized in that, In step S5, the mother liquor obtained in step S4 is subjected to electrowinning to remove copper, resulting in electrowinning copper. The conditions for the first stage of electrowinning are a temperature of 50-60℃ and a current density of 200-250 A / m. 2 The concentration of copper ions in the solution after copper removal is controlled to be 8-13 g / L.
5. The method for comprehensively purifying copper electrolytic solution using a high-temperature and pressure oxidation process according to claim 1, characterized in that, In step S6, the copper-removing solution obtained in step S5 undergoes a two-stage electrowinning process to remove copper, yielding electrowinning copper powder. The conditions for the two-stage electrowinning are a temperature of 50-60℃ and a current density of 500-1000 A / m. 2 After electrowinning, the copper ion concentration in the solution is 1-3 g / L, yielding the final copper-removed solution, which is then connected to the existing production process.
Citation Information
Patent Citations
Waste electrolyte treatment method and device
CN104694978A
Method for recovering refined nickel sulfate from copper electrolyte
JP1987284025A