A method for preparing aerogel-reinforced composite electrolyte film and solid-state lithium battery
By using an aerogel-reinforced composite electrolyte film in a lithium battery, combining polymer resin with lithium salt and silica aerogel, the problems of insufficient mechanical strength and low lithium ion conductivity of the polymer electrolyte are solved, and lithium ion batteries are realized. High energy density and improved safety of batteries.
Patent Information
- Application Number
- CN202310759524.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-06-26
- Publication Date
- 2024-10-15
- Estimated Expiration
- 2043-06-26
AI Technical Summary
Existing polymer solid electrolytes in lithium batteries have insufficient mechanical strength and cannot effectively inhibit the formation of lithium dendrites. At the same time, lithium ion conductivity is low, which affects battery performance.
Using an airgel-reinforced composite electrolyte film preparation method, polymer resin is mixed with lithium salt and then laminated with silica airgel to form an electrolyte membrane with high porosity and mechanical strength to ensure constant ionic conductivity. reduce.
It significantly improves the mechanical properties and ion transmission efficiency of the electrolyte membrane, inhibits the growth of lithium dendrites, and improves the energy density and safety of solid-state lithium batteries.
Smart Images

Figure CN116864785B_ABST
Abstract
Description
Technical Field
[0001] The present application relates to the technical field of lithium batteries, and in particular to a method for preparing an aerogel-reinforced composite electrolyte film and a solid-state lithium battery. Background Art
[0002] Lithium-ion batteries have many advantages such as high energy density, long cycle life, low self-discharge, no memory effect and environmental friendliness. Their application demand in the fields of electronics and electric vehicles is growing. Lithium-ion batteries are mainly composed of positive electrode, negative electrode, electrolyte and separator. The choice of negative electrode material directly affects the energy density of the battery. Metal lithium has the lowest standard electrode potential (-3.04V relative to hydrogen electrode) and a very high theoretical specific capacity (3860mA·h·g -1 ), is the first choice for negative electrode materials of lithium secondary batteries. However, the lithium negative electrode is prone to produce dendrites during the charge and discharge cycle. Lithium dendrites penetrate the diaphragm and cause a short circuit between the positive and negative electrodes of the battery, reducing battery efficiency and causing serious safety hazards. Solid-state lithium batteries use solid electrolytes to replace electrolytes and diaphragms, thereby solving the flammability and explosiveness of electrolytes and solving the safety problems of traditional liquid lithium batteries.
[0003] Solid electrolyte materials usually use polymers, oxides or sulfides. Among them, polymer solid electrolytes are low in price, have good material flexibility, are easy to process, have good battery stability, and can improve energy density. However, their mechanical strength is too low to effectively inhibit the formation of lithium dendrites. In addition, the lithium ion conductivity of polymer solid electrolytes is general, at least 2-3 orders of magnitude lower than that of liquids. In order to improve the electrical properties of polymer electrolytes, plasticizers can be introduced into lithium salt / polymer mixtures to significantly increase the ionic conductivity to the actual value, but this further reduces the mechanical properties. There is a contradiction between ionic conductivity and elastic modulus in polymer electrolytes. Therefore, in order to give full play to the excellent electrochemical properties of all-solid-state batteries, it is necessary to develop and apply electrolyte membranes and all-solid-state batteries with new structures of polymer-based composite solid electrolytes. Patent CN111916818A discloses a solid-state lithium battery silica aerogel framework electrolyte and a preparation method, wherein silica aerogel and lithium salt are mixed, and an adhesive is added to make lithium-loaded silica aerogel, which is then mixed with a modified polymer sol to obtain a polymer electrolyte material. In this scheme, the lithium salt and the high molecular polymer are not mixed sufficiently, which affects the ionic conductivity.
[0004] Based on the above analysis, it is very important to provide a method for preparing an electrolyte film that does not affect ionic conductivity after the introduction of aerogel. Summary of the invention
[0005] The embodiment of the present application provides a method for preparing an aerogel-reinforced composite electrolyte film to solve the problem in the related art that the ionic conductivity is affected after the introduction of silica aerogel.
[0006] In a first aspect, the present application provides a method for preparing an aerogel-reinforced composite electrolyte film, comprising the following steps:
[0007] Mixing a polymer resin and a lithium salt, adding a solvent and stirring at 40 to 60° C. to obtain a 5 wt % to 15 wt % polymer solution;
[0008] coating the polymer solution onto a release film at room temperature, air-drying, and removing the release film to obtain an electrolyte film;
[0009] The aerogel is placed on the electrolyte film to make a laminate, and the laminate is pressed to obtain a composite electrolyte film.
[0010] In some embodiments, the polymer resin is a mixture of one or more of polyethylene oxide (PEO), polymethyl methacrylate (PMMA), polycarbonate, polyvinylidene fluoride (PVDF), polysiloxane (PDMS), trimerphosphazene epoxy resin, and phenoxy polyphosphazene resin.
[0011] In some embodiments, the weight average molecular weight (Mw) of the polymer resin is 1,000 to 1,000,000.
[0012] In some preferred embodiments, the weight average molecular weight (Mw) of the polymer resin is 5000 to 500000. The smaller the molecular weight, the higher the fluidity of the polymer resin, which is beneficial to the subsequent pressing of the electrolyte film.
[0013] In some embodiments, the solvent is acetonitrile.
[0014] In some embodiments, the anion of the lithium salt is F - , Cl - Br - ,I - 、NO3 - 、N(CN)2 - 、BF4 - 、ClO4 - PF6 - 、(CF3)2PF4 - 、(CF3)3PF3 - 、(CF3)4PF2 - 、(CF3)5PF - 、(CF3)6P - CF3SO3 - CF3CF2SO3 -、(CF3SO2)2N - 、(FSO2)2N - CF3CF2(CF3)2CO - 、(CF3SO2)2CH - 、(SF5)3C - 、(CF3SO2)3C - CF3(CF2)7SO3 - CF3CO2 - 、CH3CO2 - 、SCN - 、(CF3CF2SO2)2N - Any of .
[0015] In some embodiments, the mass ratio of the polymer resin to the lithium salt is 8-10:3-5, and the amount of the solvent used accounts for 85wt% to 95wt% of the total mass of the polymer resin and the lithium salt.
[0016] In some embodiments, the mass ratio of aerogel to electrolyte film is 40:60 to 95:5.
[0017] In some embodiments, the obtained polymer solution is subjected to plasma treatment and then coated, and the etching and polymerization of the plasma are used to increase the specific surface area of the material without changing the properties of the material itself, thereby improving the hydrophilicity of the electrolyte film. The plasma treatment process is as follows: the polymer solution is placed in the electrode device, the carbon dioxide and compressed air gas passages are opened, the carbon dioxide: air intake volume ratio is controlled to 9:1, and the flow rate is controlled to 4L / min; the high-voltage power supply is started, the voltage is controlled to 8kV, and a stable atmospheric pressure plasma is generated in the polymer solution, and the plasma treatment is performed for 5-15min.
[0018] In some embodiments, the pressure of the roller press during the pressing of the laminate is 80-120 MPa and the temperature is 60-120°C.
[0019] In some embodiments, the ionic conductivity of the polymer solution is not less than 1×10 -4 ms / cm.
[0020] In some preferred embodiments, the ionic conductivity of the polymer solution is 1×10 -2 ms / cm.
[0021] In some embodiments, the polymer solution also includes a plasticizer, and the amount of the plasticizer added is 0.1% to 10% of the total mass of the polymer resin and the lithium salt. The plasticizer enhances the flexibility and fluidity of the electrolyte film and allows the electrolyte film to be easily pushed into the aerogel during the aerogel sheeting process. In the manufacturing process of the solid electrolyte membrane, the higher the content of the plasticizer, the better, but since the higher the plasticizer content, the lower the strength of the solid electrolyte material, the amount of the plasticizer added is limited to 0.1% to 10% of the total mass of the polymer resin and the lithium salt.
[0022] In some embodiments, the plasticizer is selected from a mixture of one or more of ethylene carbonate (EC), propylene carbonate (PC), vinylene carbonate (VC), dioctyl phthalate (DOP), diisodecyl phthalate (DIDP), diisononyl phthalate (DINP), trioctyl phthalate (TOTM), and triisononyl trimellitate (TINTM).
[0023] In some embodiments, the release film is a terephthalate release film, which plays a supporting role in the process of preparing the electrolyte film.
[0024] In some embodiments, the aerogel is a mixture of one or more of silica aerogel, silica@MOF composite aerogel, aluminum oxide aerogel, zirconium dioxide aerogel, iron oxide aerogel and tin oxide aerogel.
[0025] In some embodiments, the pore size of the aerogel is 10-50 nm, and the porosity is not less than 90%. The porosity is not less than 90% to maintain appropriate ionic conductivity and mechanical strength without hindering depression, that is, the higher the porosity, the better the ionic conductivity.
[0026] In some embodiments, the silica@MOF composite aerogel is prepared by the following process: zinc oxide, silica aerogel, 2-methylimidazole and methanol are mixed and ball-milled, the solid mixture is washed with methanol, and dried at 75°C-90°C, and then heat-treated at 650°C-750°C at a heating rate of 5-10°C / min in a nitrogen atmosphere, cooled to room temperature, and finally freeze-dried at -40°C to -55°C to obtain the silica@MOF composite aerogel. In some embodiments, the thickness of the composite electrolyte film is 1μm to 100μm.
[0027] In some preferred embodiments, the thickness of the composite electrolyte film is 10 μm to 100 μm. For ionic conductivity and energy density, the smaller the thickness, the higher the ionic conductivity and energy density, and the thickness needs to be less than 100 μm; for physical strength, the higher the thickness, the greater the strength, and the thickness needs to be greater than 10 μm.
[0028] In some embodiments, the surface of the obtained composite electrolyte film is modified by ultraviolet irradiation, plasma, acid treatment or ozone treatment.
[0029] In a second aspect, the present application also provides a solid-state lithium battery comprising the above-mentioned composite electrolyte film.
[0030] In some embodiments, the solid-state lithium battery further includes a positive electrode and a negative electrode.
[0031] In some embodiments, the positive electrode includes a positive electrode active material, a current collector, a conductive material, and a binder resin.
[0032] In some embodiments, the positive electrode active material is selected from any one of LiCoO2, LiNiO2, LiFePO4, LiMnO3, LiMn2O3, LiMnO2, Li2CuO2, LiV3O8, LiV3O4, or a material of the chemical formula LiNi 1-x M x Lithium nickel oxide (M = Co, Mn, Al, Cu, Fe, Mg, B or Ga, x = 0.01-0.3) of the chemical formula LiMn 2-x M x O2 represents a lithium manganese composite oxide, disulfide, or the like (M=Co, Ni, Fe, Cr, Zn, or Ta, x=0.01 to 0.1) or Li2Mn3MO8 (M=Fe, Co, Ni, Cu, or Zn).
[0033] In some embodiments, the amount of conductive material added is 1% to 30% of the mass of the positive electrode active material, and the conductive material is a mixture of one or more of natural graphite, artificial graphite, acetylene black, Ketjen black, channel black, furnace black, lamp black, thermal black, carbon fiber, metal fiber, carbon fluoride, aluminum, nickel powder, zinc oxide, and potassium titanate.
[0034] In some embodiments, the binder resin is a mixture of one or more of polyvinylidene fluoride, polyvinyl alcohol, polyacrylic acid, carboxymethyl cellulose (CMC), starch, hydroxypropyl cellulose, regenerated cellulose, polyvinyl pyrrolidone, tetrafluoroethylene, polyethylene, polypropylene, ethylene propylene diene monomer (EPDM), sulfonated ethylene propylene diene monomer, styrene butadiene rubber, and fluororubber.
[0035] In some embodiments, the negative electrode active material of the negative electrode is selected from a mixture of one or more of non-graphitized carbon, graphite-based carbon, lithium metal, lithium alloy, silicon-based alloy, tin-based alloy, SnO, SnO2, PbO, PbO2, Pb2O3, Pb3O4, Sb2O3, Sb2O4, Sb2O5, GeO, GeO2, Bi2O3, Bi2O4, Bi2O5, polyacetylene, Li-Co-Ni material, titanium oxide, and lithium titanium oxide.
[0036] In the preparation method of the present application, the aerogel has an amorphous oxide as the basic skeleton, has a high elastic modulus and an ultra-high porosity (up to 80-99.8%), and especially has a high specific surface area. By adding a rigid aerogel skeleton, the mechanical properties of the electrolyte can be significantly improved, thereby inhibiting the growth of lithium dendrites. At the same time, the high porosity can make the transmission of lithium ions in the composite solid electrolyte more efficient.
[0037] The beneficial effects of the technical solution provided by this application include:
[0038] 1. The preparation method provided by the present application firstly mixes the polymer resin and the lithium salt thoroughly and evenly, so that the lithium salt and the polymer form a stable complex, then forms an electrolyte film by solvent drying, and finally combines the aerogel and the electrolyte film in a solid-solid form. This dry film form can prevent the formation of pores that can act as resistance;
[0039] 2. The method provided in this application can reduce the thickness of the solid electrolyte film to less than 100 μm, thereby improving the ionic conductivity and the energy density of the battery, with almost no damage during the manufacturing process and battery use. BRIEF DESCRIPTION OF THE DRAWINGS
[0040] In order to more clearly illustrate the technical solutions in the embodiments of the present application, the drawings required for use in the description of the embodiments will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present application. For ordinary technicians in this field, other drawings can be obtained based on these drawings without creative work.
[0041] Figure 1 A schematic flow chart of a method for preparing an aerogel-reinforced composite electrolyte film provided in an embodiment of the present application. DETAILED DESCRIPTION
[0042] In order to make the purpose, technical solution and advantages of the embodiments of the present application clearer, the technical solution in the embodiments of the present application will be clearly and completely described below in conjunction with the drawings in the embodiments of the present application. Obviously, the described embodiments are part of the embodiments of the present application, not all of the embodiments. Based on the embodiments in the present application, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of this application.
[0043] The embodiment of the present application provides a method for preparing an aerogel-reinforced composite electrolyte film, which can solve the problem in the prior art that the ionic conductivity is affected after the introduction of silica aerogel.
[0044] Example 1
[0045] Example 1 provides a method for preparing an aerogel-reinforced composite electrolyte film, comprising the following steps:
[0046] Step S101, polyethylene oxide with a weight average molecular weight of 600,000 and LiTFSI are mixed at a molar ratio of 1:833, acetonitrile is added at 85 wt % of the total mass of polyethylene oxide and LiTFSI, and the mixture is stirred at 60° C. overnight to prepare a polymer solution of about 10 wt %;
[0047] Step S102, using a scraper to apply the polymer solution onto a terephthalate release film at room temperature, and air-drying at room temperature to remove the terephthalate release film to obtain an electrolyte film with a thickness of about 20 μm;
[0048] Step S103, placing silica aerogel with a porosity of 99% on the electrolyte film in a mass ratio of 5:9, stacking the silica aerogel and the electrolyte film in sequence from top to bottom to form a laminate, placing the laminate in a roller press and pressing four times while gradually reducing the distance between the rollers, so that the electrolyte film is pushed into the silica aerogel substrate, and obtaining an aerogel-reinforced composite electrolyte film with a thickness of about 80 μm.
[0049] In Example 1, the pressure of the roller press was set to 90 MPa and the temperature was set to 80°C.
[0050] Example 2
[0051] Example 2 provides a method for preparing an aerogel-reinforced composite electrolyte film, comprising the following steps:
[0052] Step S101, polymethyl methacrylate with a weight average molecular weight of 300,000 and LiTFSI are mixed at a molar ratio of 1:519, acetonitrile is added at 90 wt % of the total mass of polymethyl methacrylate and LiTFSI, and the mixture is stirred at 60° C. overnight to prepare a polymer solution of about 5 wt %;
[0053] Step S102, using a scraper to apply the polymer solution onto a terephthalate release film at room temperature, and air-drying at room temperature to remove the terephthalate release film to obtain an electrolyte film with a thickness of about 20 μm;
[0054] Step S103, placing a silica@MOF composite aerogel with a porosity of 99% on the electrolyte film in a mass ratio of 3:2, and stacking the silica aerogel and the electrolyte film in sequence from top to bottom to form a laminate, placing the laminate in a roller press and pressing four times while gradually reducing the distance between the rollers, so that the electrolyte film is pushed into the silica aerogel substrate, to obtain a composite electrolyte film with a thickness of about 80 μm.
[0055] In Example 2, the pressure of the roller press was set to 100 MPa and the temperature was set to 75°C.
[0056] In Example 2, the silica@MOF composite aerogel was prepared by the following process: 1 g zinc oxide, 0.5 g silica aerogel, 1.5 g 2-methylimidazole and 1 mL methanol were mixed and ball-milled, the solid mixture was washed with methanol, dried at 85°C, and then heat-treated at 750°C at a heating rate of 5°C / min in a nitrogen atmosphere, cooled to room temperature, and finally freeze-dried at -50°C to obtain the silica@MOF composite aerogel.
[0057] Example 3
[0058] Example 3 provides a method for preparing an aerogel-reinforced composite electrolyte film, comprising the following steps:
[0059] Step S101, polyethylene oxide with a weight average molecular weight of 100,000 and LiTFSI are mixed at a molar ratio of 1:174, acetonitrile is added according to 95 wt % of the total mass of polyethylene oxide and LiTFSI, and the mixture is stirred at 40° C. overnight to prepare a 15 wt % polymer solution;
[0060] Step S102, placing the polymer solution in the electrode device, opening the carbon dioxide and compressed air gas passages, controlling the carbon dioxide: air intake volume ratio to 9:1, and controlling the flow rate to 4L / min; starting the high-voltage power supply, controlling the voltage to 8kV, generating a stable atmospheric pressure plasma in the polymer solution, and plasma treatment for 10 minutes, then using a scraper to apply the plasma-treated polymer solution to a terephthalate release film at room temperature, and air-drying at room temperature, removing the terephthalate release film, and obtaining an electrolyte film with a thickness of about 20μm;
[0061] Step S103, placing alumina aerogel with a porosity of 99% on the electrolyte film in a mass ratio of 1:1, stacking the silica aerogel and the electrolyte film in sequence from top to bottom to form a laminate, placing the laminate in a roller press and pressing four times while gradually reducing the distance between the rollers, so that the electrolyte film is pushed into the alumina aerogel substrate, and obtaining a composite electrolyte film with a thickness of about 80 μm.
[0062] In Example 3, the pressure of the roller press was set to 110 MPa and the temperature was set to 90°C.
[0063] Comparative Example 1
[0064] Comparative Example 1 provides a method for preparing an electrolyte film, comprising the following steps:
[0065] Step S101, mixing polyethylene oxide with a weight average molecular weight of 600,000 and LiTFSI at a molar ratio of 1:833, adding acetonitrile and stirring at 60° C. overnight to prepare a polymer solution of about 10 wt %;
[0066] Step S102: Use a scraper to apply the polymer solution onto the terephthalate release film at room temperature, and air-dry at room temperature to remove the terephthalate release film to obtain an electrolyte film with a thickness of about 80 μm.
[0067] Comparative Example 2
[0068] Comparative Example 2 provides a method for preparing a composite electrolyte film, comprising the following steps:
[0069] Step S101, mixing polyethylene oxide with a weight average molecular weight of 600,000 and LiTFSI at a molar ratio of 1:833, adding acetonitrile and stirring at 60° C. overnight to prepare a polymer solution of about 10 wt %;
[0070] Step S102, immersing the silica aerogel in the polymer solution, taking it out, and placing it in a vacuum oven for heat treatment at 60° C. for 12 hours to complete curing and obtain a composite electrolyte film.
[0071] The ionic conductivity and elastic modulus of the composite electrolyte membranes prepared in the above-mentioned Examples 1 to 3 and the electrolyte membranes of Comparative Examples 1 and 2 are shown in Table 1.
[0072] Table 1: Ionic conductivity and elastic modulus data
[0073]
[0074] It can be seen from the data of Example 1 and Comparative Example 1 in Table 1 that the addition of silica aerogel can significantly improve the ionic conductivity and elastic modulus; it can be seen from the data of Example 1 and Comparative Example 2 that the present application combines aerogel and electrolyte in a solid-solid form, which can improve the ionic conductivity and elastic modulus.
[0075] In the description of this specification, the description with reference to the terms "one embodiment / method", "some embodiments / methods", "example", "specific example" or "some examples" etc. means that the specific features, structures, materials or characteristics described in conjunction with the embodiment / method or example are included in at least one embodiment / method or example of the present application. In this specification, the schematic representations of the above terms do not necessarily refer to the same embodiment / method or example. Moreover, the specific features, structures, materials or characteristics described may be combined in a suitable manner in any one or more embodiments / methods or examples. In addition, those skilled in the art may combine and combine the different embodiments / methods or examples described in this specification and the features of the different embodiments / methods or examples, unless they are contradictory.
[0076] It should be noted that, in the present application, relational terms such as "first" and "second" are only used to distinguish one entity or operation from another entity or operation, and do not necessarily require or imply that there is any such actual relationship or order between these entities or operations. Moreover, the terms "include", "comprise" or any other variants thereof are intended to cover non-exclusive inclusion, so that the process, method, article or equipment including a series of elements includes not only those elements, but also includes other elements not explicitly listed, or also includes elements inherent to such process, method, article or equipment. In the absence of more restrictions, the elements defined by the sentence "comprise one..." do not exclude the existence of other identical elements in the process, method, article or equipment including the elements. In the present application, the meaning of "multiple" is at least two, such as two, three, etc., unless otherwise clearly and specifically stipulated.
[0077] The above description is only a specific implementation of the present application, so that those skilled in the art can understand or implement the present application. Various modifications to these embodiments will be apparent to those skilled in the art, and the general principles defined herein can be implemented in other embodiments without departing from the spirit or scope of the present application. Therefore, the present application will not be limited to the embodiments shown herein, but will conform to the widest range consistent with the principles and novel features applied for herein.
Claims
1. A method for preparing an aerogel-reinforced composite electrolyte film, It is characterized in that The following steps are involved: Mixing a polymer resin with a lithium salt, adding a solvent and stirring to obtain a polymer solution; The polymer solution is coated on a release film at room temperature, air-dried, and the release film is removed to obtain an electrolyte film, wherein the release film is a polyethylene terephthalate release film; The aerogel is placed on the electrolyte film to make a laminate, and the laminate is pressed to obtain a composite electrolyte film. The aerogel is a mixture of one or more of silica aerogel, silica@MOF composite aerogel, aluminum oxide aerogel, zirconium dioxide aerogel, iron oxide aerogel and tin oxide aerogel. The pressure during the pressing of the laminate is 80-120Mpa and the temperature is 60-120°C.
2. The method for preparing the aerogel-reinforced composite electrolyte film according to claim 1, It is characterized in that The polymer resin is a mixture of one or more of polyethylene oxide, polymethyl methacrylate, polycarbonate, polyvinylidene fluoride, polysiloxane, tripolyphosphazene epoxy resin, and phenoxy polyphosphazene resin, and the solvent is acetonitrile or acetone.
3. The method for preparing the aerogel-reinforced composite electrolyte film according to claim 1, It is characterized in that The average molecular weight of the polymer resin is 1,000 to 1,000,000.
4. The method for preparing the aerogel-reinforced composite electrolyte film according to claim 1, It is characterized in that The polymer solution also includes a plasticizer, and the amount of the plasticizer added accounts for 0.1% to 10% of the total mass of the polymer resin and the lithium salt; the plasticizer is selected from a mixture of one or more of ethylene carbonate, propylene carbonate, vinylene carbonate, dioctyl phthalate, diisodecyl phthalate, diisononyl phthalate, trioctyl phthalate, and triisononyl trimellitate.
5. The method for preparing the aerogel-reinforced composite electrolyte film according to claim 1, It is characterized in that The pore size of the aerogel is 10-50 nm, and the porosity is not less than 90%.
6. The method for preparing an aerogel-reinforced composite electrolyte film according to claim 1, It is characterized in that The thickness of the composite electrolyte film is 1 μm to 100 μm.
7. A solid-state lithium battery, It is characterized in that It comprises a composite electrolyte film prepared by the preparation method according to any one of claims 1 to 6.