Methods for preparing C2 to C4 hydrocarbons and methods for preparing the resulting mixed catalysts
By preparing a hybrid catalyst combining metal oxides and microporous catalysts, the problems of low conversion rate and stability of existing catalysts in the conversion of C2 to C4 hydrocarbons were solved, and efficient conversion and stable production of C2 to C4 hydrocarbons were achieved.
Patent Information
- Application Number
- CN202280015809.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2021-02-26
- Filing Date
- 2022-02-18
- Publication Date
- 2026-11-10
- Estimated Expiration
- 2042-02-18
AI Technical Summary
Existing catalysts suffer from low conversion rates and stability issues in the process of converting feed carbon into C2 to C4 hydrocarbons. In particular, rapid catalyst deactivation leads to increased methane production and insufficient olefin yield and stability.
A hybrid catalyst is prepared by combining a metal oxide component (such as gallium oxide and zirconium oxide) with a microporous catalyst component and forming a single catalyst body by means of a binder, for converting carbon-containing gas into C2 to C4 hydrocarbons, including a molecular sieve with 8-MR pore openings and a binder such as alumina or zirconium oxide.
It achieves high conversion rate and stability for the efficient conversion of carbon-containing gases into C2 to C4 hydrocarbons, improves olefin yield, and reduces catalyst deactivation rate.
Smart Images

Figure BDA0004401571950000191
Abstract
Description
[0001] Cross-references to related applications
[0002] This application claims priority to U.S. Provisional Patent Application No. 63 / 154,138, filed February 26, 2021, the entire disclosure of which is incorporated herein by reference. Background Technology Technical Field
[0004] This disclosure relates to methods for efficiently converting various carbon-containing feed streams into C2 to C4 hydrocarbons. Specifically, this disclosure relates to the preparation of a mixed catalyst and the application of a process method to achieve high conversion rates of the syngas feed, thereby producing good carbon conversion and high yields of desired products. Technical Background
[0006] For many industrial applications, hydrocarbons are used or serve as starting materials to produce plastics, fuels, and a variety of downstream chemicals. These hydrocarbons include C2 to C4 materials such as ethylene, propylene, and butylene (often also referred to as ethylene, propylene, and butene, respectively). Numerous methods have been developed for producing these lower hydrocarbons, including petroleum cracking and various synthetic methods.
[0007] Synthetic methods for converting feed carbon into desired products, such as hydrocarbons, are known. Different types of catalysts, as well as different types of feed streams and the proportions of feed stream components, have been studied.
[0008] However, these catalysts themselves need to be loaded into the reactor in a molded form to reduce the pressure drop across the reactor. Furthermore, many of these synthetic methods have low carbon conversion rates, and much of the feed carbon (1) is not converted and leaves the method in the same form as the feed carbon; (2) is converted to CO2; or (3) these synthetic methods exhibit low stability over time, and the catalyst rapidly loses its activity in converting carbon into the desired product. For example, many synthetic methods tend to have increasing methane yields over time—and therefore decreasing C2 to C4 hydrocarbon yields.
[0009] Therefore, there is a need for methods and catalytic systems that comprise a single catalyst body containing both microporous catalyst components and metal oxide catalyst components, rather than forming the components separately, and that exhibit high conversion rates of feed carbon to desired products (e.g., C2 to C4 hydrocarbons) and high on-stream stability of the catalyst. Summary of the Invention
[0010] The embodiments of this disclosure address these and other needs through the preparation of a hybrid catalyst and methods for using such a catalyst. The hybrid catalyst comprises a combination of a metal oxide component, a microporous catalyst component, and a binder. The binder is used to combine the metal oxide component and the microporous catalyst component into a single catalyst body. This hybrid catalyst can then be used to directly convert feed streams containing hydrogen and carbon-containing gases, such as syngas, into C2 to C4 hydrocarbons. The metal oxide component and the microporous catalyst component operate in series, enabling the hybrid catalyst to directly and selectively convert feed streams containing hydrogen and carbon-containing gases, such as syngas, into C2 to C4 hydrocarbons with a high olefin / alkane ratio.
[0011] According to one or more aspects of this disclosure, a method for preparing C2 to C4 hydrocarbons includes introducing a feed stream comprising hydrogen and a carbon-containing gas selected from the group consisting of carbon monoxide, carbon dioxide, and mixtures thereof into a reaction zone of a reactor, and converting the feed stream into a product stream comprising C2 to C4 hydrocarbons in the reaction zone in the presence of a formed mixed catalyst. The formed mixed catalyst comprises: a metal oxide catalyst component comprising gallium oxide and zirconium oxide; a microporous catalyst component as a molecular sieve having an 8-membered ring (MR) pore opening; and a binder comprising alumina, zirconium oxide, or both.
[0012] According to one or more other aspects of this disclosure, a method for preparing a hybrid catalyst includes: mixing a metal oxide catalyst component and a microporous catalyst component, wherein the metal oxide catalyst component comprises gallium oxide and zirconium oxide, and the microporous catalyst component comprises a molecular sieve having 8-MR pore openings; adding a binder to the mixture of the metal oxide catalyst component and the microporous catalyst component to form a paste, wherein the binder is a colloidal solution, suspension, or gel containing a binder precursor comprising an oxide or hydroxide of aluminum, an oxide or hydroxide of zirconium, or a mixture thereof; and extruding the paste after drying and subsequent calcination to produce the hybrid catalyst.
[0013] Further features and advantages will be set forth in the following detailed description, and in part will be apparent to those skilled in the art from those description or will be recognized by practice of the embodiments described herein (including the following detailed description and claims).
[0014] It should be understood that both the foregoing general description and the following detailed description describe various implementation schemes and are intended to provide an overview or framework for understanding the nature and characteristics of the claimed subject matter. Detailed Implementation
[0015] Reference will now be made in detail to embodiments of methods for preparing the formed mixed catalyst and methods for forming C2 to C4 hydrocarbons from a feed stream containing hydrogen and a carbon-containing gas. As used herein, "carbon-containing gas" refers to a gas selected from carbon monoxide, carbon dioxide, and mixtures thereof. In one embodiment, a method for preparing C2 to C4 hydrocarbons includes introducing a feed stream containing hydrogen and a carbon-containing gas selected from the group consisting of carbon monoxide, carbon dioxide, and mixtures thereof into a reaction zone of a reactor; and converting the feed stream into a product stream containing C2 to C4 hydrocarbons in the reaction zone in the presence of the formed mixed catalyst. The formed mixed catalyst comprises: a metal oxide catalyst component including gallium oxide and zirconium oxide, a microporous catalyst component as a molecular sieve having 8-MR pore openings, and a binder including alumina, zirconium oxide, or both.
[0016] As used herein, “gallium oxide” refers to gallium in various oxidation states. In one embodiment, gallium oxide may include Ga₂O₃. In other embodiments, gallium oxide may include gallium in more than one oxidation state. For example, individual gallium particles may be in different oxidation states. Gallium oxide is not limited to gallium comprising a uniform oxidation state.
[0017] The use of such hybrid catalysts is known in the field of hydrocarbon products such as diesel or aromatic compounds. However, many known hybrid catalysts are inefficient for forming C2 to C4 hydrocarbons, and especially C2 to C4 olefins, from feed streams containing hydrogen and carbon-containing gases because they exhibit low feed carbon conversion and / or rapid deactivation during use, for example by increasing methane yield. This results in low olefin yields and low stability over a given time period under a given set of operating conditions. In contrast, the hybrid catalysts disclosed and described herein exhibit high and stable yields, particularly of C2 to C4 olefins, even with increased catalyst run times, when compared to hybrid catalysts in which metal oxide catalyst components and microporous catalyst components are physically mixed (e.g., not together to form a hybrid catalyst of one form). The preparation and composition of such hybrid catalysts used in embodiments are discussed below.
[0018] In summary, the resulting hybrid catalyst tightly couples the independent reactions on each of the two independent catalysts. In the first step, a feed stream containing hydrogen (H2) and a carbon-containing gas selected from the group consisting of carbon monoxide (CO), carbon dioxide (CO2), or a mixture of CO and CO2, such as syngas, is converted into intermediates, such as oxygenated hydrocarbons. In subsequent steps, these intermediates are converted into a product stream containing hydrocarbons (primarily short-chain hydrocarbons, such as C2 to C4 hydrocarbons). The continuous formation and consumption of intermediate oxygenated compounds formed in the first step by the reaction in the second step ensures that there are no thermodynamic limitations on the conversion.
[0019] In one embodiment, the particle size of the formed mixed catalyst is from 0.5 mm to 6.0 mm, such as 0.5 mm to 5.5 mm, 0.5 mm to 5.0 mm, 0.5 mm to 4.5 mm, 0.5 mm to 4.0 mm, 0.5 mm to 3.5 mm, 0.5 mm to 3.0 mm, 0.5 mm to 2.5 mm, 0.5 mm to 2.0 mm, or 0.5 mm to 1.5 mm. In another embodiment, the particle size of the formed mixed catalyst is from 1.0 mm to 6.0 mm, such as 1.0 mm to 5.5 mm, 1.0 mm to 5.0 mm, 1.0 mm to 4.5 mm, 1.0 mm to 4.0 mm, 1.0 mm to 3.5 mm, 1.0 mm to 3.0 mm, 1.0 mm to 2.5 mm, 1.0 mm to 2.0 mm, or 1.0 mm to 1.5 mm. In the embodiments, the particle size of the formed mixed catalyst is 1.5 mm to 3.0 mm, for example 1.8 mm to 3.0 mm, 2.0 mm to 3.0 mm, 2.2 mm to 3.0 mm, 2.5 mm to 3.0 mm, 2.8 mm to 3.0 mm, 1.5 mm to 2.8 mm, 1.8 mm to 2.8 mm, 2.0 mm to 2.8 mm, 2.2 mm to 2.8 mm, 2.5 mm to 2.8 mm, 1.5 mm to 2.5 mm, 1.8 mm to 2.5 mm, 2.0 mm to 2.5 mm, 2.2 mm to 2.5 mm, 1.5 mm to 2.2 mm, 1.8 mm to 2.2 mm, 2.0 mm to 2.2 mm, 1.5 mm to 2.0 mm, 1.8 mm to 2.0 mm, or 1.5 mm to 1.8 mm. The particle size can be substantially the shortest size of the catalyst particles. For example, when the formed mixed catalyst has a hollow cylindrical or annular shape, the particle size is the thickness of the hollow cylinder wall. When the formed mixed catalyst has a spherical shape, the particle size is the diameter of the sphere. The particle size of the formed mixed catalyst can be controlled by selecting the extrusion die diameter and measured using dynamic image analysis methods.
[0020] The resulting hybrid catalyst comprises a metal oxide catalyst component that converts the feed stream into oxygen-containing hydrocarbons and a microporous catalyst component that converts the oxygen-containing hydrocarbons into hydrocarbons. The metal oxide catalyst component is combined with the microporous catalyst component. Therefore, it is necessary to produce a metal oxide catalyst component with high initial yield and high stability when combined with a microporous catalyst component in the resulting hybrid catalyst process. It should be understood that, as used herein, "metal oxide catalyst component" includes metals in various oxidation states. In some embodiments, the metal oxide catalyst component may include more than one metal oxide, and the individual metal oxides within the metal oxide catalyst component may have different oxidation states. Therefore, the metal oxide catalyst component is not limited to containing metal oxides having a uniform oxidation state.
[0021] In some embodiments, the metal oxide catalyst component has a particle size of less than 150 μm, less than 120 μm, or less than 100 μm. In some embodiments, the metal oxide catalyst component has a particle size of 0.1 μm to 150 μm, 0.1 μm to 120 μm, 0.1 μm to 100 μm, 1 μm to 150 μm, 1 μm to 120 μm, 1 μm to 100 μm, 1 μm to 50 μm, 5 μm to 150 μm, 5 μm to 120 μm, 5 μm to 100 μm, 5 μm to 50 μm, 10 μm to 150 μm, 10 μm to 120 μm, 10 μm to 100 μm, or 10 μm to 50 μm. Particle size may refer to the maximum particle size. The particle size of the metal oxide catalyst component may refer to the physical size of the metal oxide catalyst component, rather than the crystal size of the metal oxide catalyst component. The particle size of the metal oxide catalyst component can be measured by laser diffraction or by passing the material through an analytical sieve.
[0022] In the embodiments, the metal oxide catalyst component has a particle size D of 1 μm to 100 μm, 1 μm to 90 μm, 1 μm to 80 μm, or 1 μm to 50 μm. 50 , which is the median diameter or median of the volumetric particle size distribution.
[0023] The metal oxide catalyst component comprises gallium oxide and zirconium oxide (ZrO2). As used herein, the zirconium oxide used in the embodiments disclosed and described herein in the metal oxide catalyst component of the formed mixed catalyst is "phase-pure zirconium oxide," which is defined herein as zirconium oxide in which no other materials were intentionally added during formation. Thus, "phase-pure zirconium oxide" comprises zirconium oxide having a small amount of components other than zirconium (including oxides other than zirconium oxide) that are unintentionally present in zirconium oxide as a natural part of the zirconium oxide formation process, such as hafnium (Hf). Therefore, unless otherwise specifically stated, "zirconium oxide" and "phase-pure zirconium oxide" are used interchangeably herein.
[0024] Unbound by any specific theory, it is believed that the high surface area of zirconium oxide allows gallium oxide catalysts, acting as part of the resulting mixed catalyst, to convert carbonaceous components into C2 to C4 hydrocarbons. Gallium oxide and zirconium oxide are believed to facilitate mutual activation, thereby increasing the yield of C2 to C4 hydrocarbons.
[0025] In the embodiments disclosed herein, the composition of the metal oxide catalyst component is expressed as a weight percentage of gallium oxide metal relative to pure zirconium oxide (considering the stoichiometry of ZrO2). In one or more embodiments, the composition of the metal oxide catalyst component is expressed as the weight of gallium oxide per 100 grams (g) of zirconium oxide. According to embodiments, the metal oxide catalyst component comprises 0.1 g to 30.0 g of gallium oxide per 100 g of zirconium oxide, such as 5.0 g to 30.0 g of gallium oxide per 100 g of zirconium oxide, 10.0 g to 30.0 g of gallium oxide per 100 g of zirconium oxide, 15.0 g to 30.0 g of gallium oxide per 100 g of zirconium oxide, 20.0 g to 30.0 g of gallium oxide per 100 g of zirconium oxide, or 25.0 g to 30.0 g of gallium oxide per 100 g of zirconium oxide. In some embodiments, the metal oxide catalyst component comprises 0.1 g gallium oxide to 25.0 g gallium oxide per 100 g zirconium oxide, such as 0.1 g gallium oxide to 20.0 g gallium oxide per 100 g zirconium oxide, 0.1 g gallium oxide to 15.0 g gallium oxide per 100 g zirconium oxide, 0.1 g gallium oxide to 10.0 g gallium oxide per 100 g zirconium oxide, or 0.1 g gallium oxide to 5.0 g gallium oxide per 100 g zirconium oxide. In some embodiments, the metal oxide catalyst component comprises 5.0 g gallium oxide to 25.0 g gallium oxide per 100 g zirconium oxide, such as 10.0 g gallium oxide to 20.0 g gallium oxide per 100 g zirconium oxide. In some embodiments, the metal oxide catalyst component includes 0.1g to 5.00g to 100g gallium oxide per 100g zirconium oxide, such as 0.50g to 5.00g to 100g gallium oxide per 100g zirconium oxide, 1.00g to 5.00g to 100g gallium oxide per 100g zirconium oxide, 1.50g to 5.00g to 100g gallium oxide per 100g zirconium oxide, or 2.00g to 5.00g gallium oxide per 100g zirconium oxide. Gallium oxide to 100g zirconium oxide, 2.50g gallium oxide to 5.00g gallium oxide to 100g zirconium oxide per 100g zirconium oxide, 3.00g gallium oxide to 5.00g gallium oxide to 100g zirconium oxide per 100g zirconium oxide, 3.50g gallium oxide to 5.00g gallium oxide to 100g zirconium oxide per 100g zirconium oxide, 4.00g gallium oxide to 5.00g gallium oxide to 100g zirconium oxide per 100g zirconium oxide, or 4.50g gallium oxide to 5.00g gallium oxide to 100g zirconium oxide per 100g zirconium oxide.
[0026] In the embodiments disclosed herein, the composition of the metal oxide catalyst component is expressed as a weight percentage of lanthanum oxide metal relative to pure zirconium oxide (considering the stoichiometry of ZrO2). In one or more embodiments, the composition of the metal oxide catalyst component is expressed as the weight of lanthanum oxide per 100 grams (g) of zirconium oxide. According to embodiments, the metal oxide catalyst component comprises 0.1 g to 10.0 g of lanthanum oxide per 100 g of zirconium oxide, such as 5.0 g to 10.0 g of lanthanum oxide per 100 g of zirconium oxide, 10.0 g to 30.0 g of lanthanum oxide per 100 g of zirconium oxide, 15.0 g to 30.0 g of lanthanum oxide per 100 g of zirconium oxide, 20.0 g to 30.0 g of lanthanum oxide per 100 g of zirconium oxide, or 25.0 g to 30.0 g of lanthanum oxide per 100 g of zirconium oxide. In some embodiments, the metal oxide catalyst component comprises 0.1 g of lanthanum oxide to 25.0 g of lanthanum oxide per 100 g of zirconium oxide, such as 0.1 g of lanthanum oxide to 20.0 g of lanthanum oxide per 100 g of zirconium oxide, 0.1 g of lanthanum oxide to 15.0 g of lanthanum oxide per 100 g of zirconium oxide, 0.1 g of lanthanum oxide to 10.0 g of lanthanum oxide per 100 g of zirconium oxide, or 0.1 g of lanthanum oxide to 5.0 g of lanthanum oxide per 100 g of zirconium oxide. In some embodiments, the metal oxide catalyst component comprises 5.0 g of lanthanum oxide to 25.0 g of lanthanum oxide per 100 g of zirconium oxide, such as 10.0 g of lanthanum oxide to 20.0 g of lanthanum oxide per 100 g of zirconium oxide. In some embodiments, the metal oxide catalyst component comprises 0.1 g of lanthanum oxide to 5.00 g of lanthanum oxide to 100 g of zirconium oxide per 100 g of zirconium oxide, such as 0.50 g of lanthanum oxide to 5.00 g of lanthanum oxide to 100 g of zirconium oxide per 100 g of zirconium oxide, 1.00 g of lanthanum oxide to 5.00 g of lanthanum oxide to 100 g of zirconium oxide per 100 g of zirconium oxide, 1.50 g of lanthanum oxide to 5.00 g of lanthanum oxide to 100 g of zirconium oxide per 100 g of zirconium oxide, or 2.00 g of lanthanum oxide to 5.00 g of lanthanum oxide per 100 g of zirconium oxide. Lanthanum oxide to 100g zirconium oxide, 2.50g lanthanum oxide to 5.00g lanthanum oxide to 100g zirconium oxide per 100g zirconium oxide, 3.00g lanthanum oxide to 5.00g lanthanum oxide to 100g zirconium oxide per 100g zirconium oxide, 3.50g lanthanum oxide to 5.00g lanthanum oxide to 100g zirconium oxide per 100g zirconium oxide, 4.00g lanthanum oxide to 5.00g lanthanum oxide to 100g zirconium oxide per 100g zirconium oxide, or 4.50g lanthanum oxide to 5.00g lanthanum oxide to 100g zirconium oxide per 100g zirconium oxide.
[0027] In view of the above, a method for preparing the gallium oxide and zirconium oxide metal oxide components of the formed mixed catalyst is carried out by initial wet impregnation. In this method, while stirring and mixing zirconium oxide particles, an aqueous mixture of gallium precursor material (in an embodiment, this may be gallium nitrate (Ga(NO3)3)) is added to the zirconium oxide powder in a dosage (such as dropwise). In other embodiments, gallium oxide may be deposited or distributed on the zirconium oxide by chemical vapor deposition (CVD). However, the method for preparing the gallium oxide and zirconium oxide metal oxide components of the formed mixed catalyst is not particularly limited, and any method that can apply a fine layer of gallium oxide to the zirconium oxide surface can be used according to the embodiments. It should be understood that the total amount of gallium precursor mixed with the zirconium oxide particles will be determined based on the desired target amount of gallium in the metal oxide catalyst component.
[0028] As previously discussed, according to some embodiments, the zirconia particles comprise zirconia particles having a crystalline structure. In some embodiments, the zirconia particles comprise zirconia particles having a monoclinic crystal structure. In one or more embodiments, the zirconia particles are substantially composed of or consist of crystalline zirconia particles, and in some embodiments, the zirconia particles are substantially composed of or consist of monoclinic zirconia particles. According to some embodiments, the BET surface area of the zirconia particles is greater than or equal to 5 square meters per gram (m²). 2 / g), such as greater than 10m 2 / g, greater than 20m 2 / g, greater than 30m 2 / g, greater than 40m 2 / g, greater than 50m 2 / g, greater than 60m 2 / g, greater than 70m 2 / g, greater than 80m 2 / g, greater than 90m 2 / g, greater than 100m 2 / g, greater than 110m 2 / g, greater than 120m 2 / g, greater than 130m 2 / g or greater than 140m 2 / g. According to some implementation schemes, the maximum BET surface area of the zirconium oxide particles is 150m². 2 / g. Therefore, in some embodiments, the BET surface area of the zirconium oxide particles is 5m². 2 / g to 150m 2 / g, 10m 2 / g to 150m 2 / g、20m 2 / g to 150m 2 / g, such as 30m 2 / g to 150m 2 / g、40m 2 / g to 150m 2 / g, 50m 2 / g to 150m 2 / g、60m 2 / g to 150m 2 / g、70m 2 / g to 150m 2 / g、80m 2 / g to 150m 2 / g、90m 2 / g to 150m 2 / g, 100m 2 / g to 150m 2 / g、110m 2 / g to 150m 2 / g, 120m 2 / g to 150m 2 / g, 130m 2 / g to 150m 2 / g or 140m 2 / g to 150m 2 / g. In some embodiments, the BET surface area of the zirconium oxide particles is 5m². 2 / g to 140m 2 / g, such as 5m 2 / g to 130m 2 / g、5m 2 / g to 120m 2 / g、5m 2 / g to 110m 2 / g、5m 2 / g to 100m 2 / g、5m 2 / g to 90m 2 / g、5m 2 / g to 80m 2 / g、5m 2 / g to 70m 2 / g、5m 2 / g to 60m 2 / g、5m 2 / g to 50m 2 / g、5m 2 / g to 40m 2 / g、5m 2 / g to 30m 2 / g、5m 2 / g to 20m 2 / g or 5m 2 / g to 10m 2 / g. In some embodiments, the BET surface area of the zirconium oxide particles is 10m². 2 / g to 140m 2 / g、20m 2 / g to 130m 2 / g、30m 2 / g to 120m 2 / g、40m 2 / g to 110m 2 / g, 50m 2 / g to 100m 2 / g、60m 2 / g to 90m 2 / g or 70m 2 / g to 80m 2 / g.
[0029] Once the gallium precursor and zirconium oxide particles are thoroughly mixed, the metal oxide catalyst component can be dried at temperatures below 200 degrees Celsius (°C), such as below 175°C, below 150°C, below 100°C, or about 85°C. After drying, the metal oxide catalyst component is calcined at temperatures between 400°C and 800°C, such as 425°C to 775°C, 450°C to 750°C, 475°C to 725°C, 500°C to 700°C, 525°C to 675°C, 550°C to 650°C, 575°C to 625°C, about 550°C, or about 600°C. After calcination, the composition of the mixed metal oxide catalyst component is determined and reported as gallium oxide as a reference to Ga2O3, as previously disclosed above for the weight of 100g of phase-pure zirconium oxide (simplified to the stoichiometry of ZrO2).
[0030] In some embodiments, the metal oxide catalyst component can be prepared by mixing gallium precursors (such as gallium nitrate or gallium oxide) and zirconium oxide powder or slurry. According to some embodiments, the zirconium oxide particles comprise zirconium oxide particles having a crystalline structure. In some embodiments, the zirconium oxide particles comprise zirconium oxide particles having a monoclinic crystal structure. In one or more embodiments, the zirconium oxide particles consist substantially of or are composed of crystalline zirconium oxide particles, and in some embodiments, the zirconium oxide particles consist substantially of or are composed of monoclinic zirconium oxide particles. In some embodiments, the zirconium oxide particles have the BET surface area disclosed above. The powder or slurry can be vigorously mixed at high temperatures, such as room temperature (approximately 23°C) to 100°C. After the powder or slurry is thoroughly mixed, the metal oxide catalyst components can be dried and calcined at temperatures ranging from 400°C to 800°C, such as 425°C to 775°C, 450°C to 750°C, 475°C to 725°C, 500°C to 700°C, 525°C to 675°C, 550°C to 650°C, 575°C to 625°C, or approximately 600°C. After calcination, the composition of the mixed metal oxide catalyst components is determined and reported as gallium oxide as Ga2O3 relative to the stoichiometry of 100g of phase-pure zirconium oxide (simplified to ZrO2) as disclosed above.
[0031] It should be understood that, according to the embodiments, the metal oxide catalyst component can be prepared by other methods that ultimately produce a close contact between the gallium precursor and zirconium oxide. Some non-limiting examples involve the vapor deposition of a Ga-containing precursor (organic or inorganic in nature), followed by its controlled decomposition. Similarly, methods for dispersing liquid gallium metal can be modified by those skilled in the art to produce a close contact between the gallium precursor and zirconium oxide.
[0032] In some embodiments, elements other than gallium oxide and zirconium oxide may be present in the metal oxide catalyst component containing phase-pure zirconium oxide and gallium oxide. Such elements can be introduced into phase-pure zirconium oxide before, during, or after the introduction of the gallium precursor into the composition. Sometimes, such elements are added to guide and stabilize the crystallization of the zirconium oxide phase (e.g., Y-stabilized tetragonal ZrO2).
[0033] In some embodiments, the metal oxide catalyst component includes lanthanum. In others, additional elements from the group consisting of rare earth, alkali metals, and / or transition metals are co-deposited with the gallium precursor or introduced only when a mixed composition comprising gallium oxide and zirconium oxide has already been prepared first.
[0034] In one or more embodiments, after the metal oxide catalyst component has been prepared, for example by the methods disclosed above, the metal oxide catalyst component is mixed with a microporous catalyst component and a binder to form a single catalyst. In embodiments, the microporous catalyst component is selected from molecular sieves having 8-MR pore openings and having a framework type selected from the group consisting of: CHA, AEI, AFX, ERI, LTA, UFI, RTH, EDI, GIS, MER, RHO, and combinations thereof, which correspond to the nomenclature conventions of the International Zeolite Association. It should be understood that both aluminosilicate and aluminosilicate phosphate frameworks can be used in embodiments. Some embodiments may include tetrahedral aluminosilicates, ALPO (e.g., tetrahedral aluminosilicates), SAPO (e.g., tetrahedral aluminosilicates), and silica-only framework silicates. In some embodiments, the microporous catalyst component may be aluminosilicate phosphate having a chalcogenide (CHA) framework type. Examples of these may include, but are not limited to, the CHA embodiments selected from SAPO-34 and SSZ-13; and AEI embodiments, such as SAPO-18. Combinations of microporous catalyst components having any of the above framework types may also be used. It should be understood that, depending on the desired product, the microporous catalyst components may have different membered ring pore openings. For example, depending on the desired product, microporous catalyst components with 8-MR to 12-MR pore openings may be used. However, for the production of C2 to C4 hydrocarbons, microporous catalyst components with 8-MR pore openings are used in the embodiments.
[0035] The metal oxide catalyst component and the microporous catalyst component of the resulting mixed catalyst can be mixed together by any suitable method to achieve homogeneous mixing of all components prior to extrusion. The metal oxide catalyst component and the microporous catalyst component can initially be mixed in powder form to achieve homogeneity in a suitable dry mixer, such as a ribbon or plow mixer. A gelled binder precursor can be added to the mixture of the metal oxide catalyst component and the microporous catalyst component and mixed in a suitable heavy-duty industrial mixer capable of handling thick paste formulations. Alternatively, the dried premixed metal oxide catalyst component and the microporous catalyst component can be fed directly into the feed screw of a screw extruder along with the gelled binder precursor composition and mixed directly in the screw extruder. The resulting mixed catalyst can be extruded into the desired shape by any suitable extrusion method. Examples of shapes include pellets, spheres, or near-spherical shapes. In the embodiments, the metal oxide catalyst component may account for 1.0 wt% to 80.0 wt% of the formed mixed catalyst, such as 5.0 wt% to 80.0 wt%, 10.0 wt% to 80.0 wt%, 15.0 wt% to 80.0 wt%, 20.0 wt% to 80.0 wt%, 25.0 wt% to 80.0 wt%, 30.0 wt% to 80.0 wt%, 35.0 wt% to 80.0 wt%, 40.0 wt% to 80.0 wt%, 45.0 wt% to 80.0 wt%, 50.0 wt% to 80.0 wt%, 55.0 wt% to 80.0 wt%, 60.0 wt% to 80.0 wt%, 65.0 wt% to 80.0 wt%, 70.0 wt% to 80.0 wt%, or 75.0 wt% to 80.0 wt%. In some embodiments, the metal oxide catalyst component comprises 1.0 wt% to 80.0 wt%, 1.0 wt% to 75.0 wt%, 1.0 wt% to 70.0 wt%, 1.0 wt% to 65.0 wt%, 1.0 wt% to 60.0 wt%, 1.0 wt% to 55.0 wt%, 1.0 wt% to 50.0 wt%, 1.0 wt% to 45.0 wt%, 1.0 wt% to 40.0 wt%, 1.0 wt% to 35.0 wt%, 1.0 wt% to 30.0 wt%, 1.0 wt% to 25.0 wt%, 1.0 wt% to 20.0 wt%, 1.0 wt% to 15.0 wt%, 1.0 wt% to 10.0 wt%, or 1.0 wt% to 5.0 wt%.In some embodiments, the metal oxide catalyst component accounts for 5.0 wt% to 80.0 wt% of the formed mixed catalyst, such as 10.0 wt% to 80.0 wt%, 15.0 wt% to 80.0 wt%, 20.0 wt% to 80.0 wt%, 25.0 wt% to 75.0 wt%, 30.0 wt% to 70.0 wt%, 35.0 wt% to 65.0 wt%, 40.0 wt% to 60.0 wt%, or 45.0 wt% to 55.0 wt%. In some embodiments, the metal oxide catalyst component accounts for 50.0 wt% to 80.0 wt% of the formed mixed catalyst, such as 50.0 wt% to 75.0 wt%, 50.0 wt% to 70.0 wt%, 60.0 wt% to 80.0 wt%, 60.0 wt% to 75.0 wt%, or 60.0 wt% to 70.0 wt%.
[0036] The metal oxide catalyst component and the microporous catalyst component can be mixed in a mass ratio of 1:10 to 10:1, 1:10 to 9:1, 1:10 to 8:1, 1:10 to 5:1, 1:10 to 4:1, 1:10 to 3:1, 1:8 to 8:1, 1:8 to 7:1, 1:8 to 6:1, 1:8 to 5:1, 1:8 to 4:1, 1:5 to 8:1, 1:5 to 7:1, 1:5 to 6:1 or 1:5 to 5:1.
[0037] After the prepared metal oxide catalyst component is mixed with the microporous catalyst component, a binder is added to prepare a paste. The binder enables the metal oxide catalyst component and the microporous catalyst component to be held together. The paste can be extruded to produce the resulting mixed catalyst. The resulting mixed catalyst can be formed by any suitable extrusion method.
[0038] Various binders are considered suitable. For example, binders may include alumina, zirconium oxide, or both. In some embodiments, the binder may include pure alumina. In some embodiments, the binder may include pure zirconium oxide. When the binder includes alumina, the alumina binder may be hydrated alumina. Hydrated alumina compositions may be prepared from bohemitic precursors with water and a colloidal solvent. The binder may be mixed with both the metal oxide catalyst component and the microporous catalyst component. After mixing the binder with the metal oxide catalyst component and the microporous catalyst component, the mixture may be extruded, dried, and calcined. Upon calcination, the binder may form alumina and bind the metal oxide catalyst component and the microporous catalyst component together to provide mechanical strength for the extruded mixed catalyst. Without being bound by any particular theory, other commonly used binders, such as SiO2 and TiO2, may lead to catalyst activity poisoning or a significant loss of olefin selectivity. Mixing two catalyst components into a single catalyst body is not straightforward. Although a physical mixture of metal oxide catalyst components and microporous catalyst components (i.e., without forming a single catalyst body) can reduce the pressure drop on the reactor, catalytic performance such as olefin selectivity and carbon conversion is significantly reduced.
[0039] Binders, including alumina, zirconium oxide, or both, can blend metal oxide catalyst components and microporous catalyst components into a single catalyst body to improve C2 to C4 olefin yields and carbon conversion. Forming either the metal oxide catalyst or the microporous catalyst separately and combining them into a physical mixture does not yield the C2 to C4 yields and carbon conversions that are achieved using mixed catalysts formed as disclosed and described herein.
[0040] In some embodiments, the binder is a colloidal solution, suspension, or gel of a binder precursor. The binder precursor may include oxides or hydroxides of aluminum, oxides or hydroxides of zirconium, or mixtures thereof. In one embodiment, the binder precursor may include pure alumina, (pseudo)boehmite, or gibbsite, or mixtures thereof. In other embodiments, the binder precursor may include pure zirconium oxide, hydrated zirconium oxide, or mixtures thereof.
[0041] In embodiments, when the binder comprises alumina, the binder may have a [H] content of 0.005 to 0.1, 0.01 to 0.1, or about 0.05. + ] / [Al] ratio.
[0042] In the implementation scheme, the adhesive may have a thickness of 100m. 2 / g to 400m 2 / g、125m 2 / g to 400m 2 / g, 150m 2 / g to 400m 2 / g, 100m2 / g to 200m 2 / g、125m 2 / g to 200m 2 / g, 150m 2 / g to 200m 2 / g, 100m 2 / g to 175m 2 / g、125m 2 / g to 175m 2 / g, 150m 2 / g to 175m 2 / g, 100m 2 / g to 150m 2 / g、125m 2 / g to 150m 2 / g or 100m 2 / g to 125m 2 / g of surface area.
[0043] Unbound by any particular theory, it has been found that using templated molecular sieves (e.g., uncalcined) in formulations has a positive impact on catalyst performance and structural properties, especially when strong acidic conditions, such as [H+] greater than 0.05 or greater than 0.025, are used during the formulation process of the resulting mixed catalysts. + When ] / [Al] is compared.
[0044] In some embodiments, the mixed metal oxide catalyst component and / or binder are substantially free of silica. The term "substantially free" means that the component is less than 0.5 wt.% of the composition. For example, a substantially silica-free mixed metal oxide catalyst component and binder may have less than 0.5 wt.% silica based on the combined weight of the mixed metal oxide and binder.
[0045] The resulting mixed catalyst can be used in methods for converting carbon in a carbon-containing feed stream into C2 to C4 hydrocarbons. Such methods will be described in more detail below.
[0046] According to the embodiments, a feed stream comprising hydrogen (H2) and a carbonaceous gas selected from carbon monoxide (CO), carbon dioxide (CO2), and combinations thereof is fed into the reaction zone. In some embodiments, H2 gas is present in the feed stream at an amount from 10 volume percent (vol%) to 90 vol%, based on the combined volume of the H2 gas and the gas selected from CO, CO2, and combinations thereof. The feed stream is contacted in the reaction zone with a mixed catalyst formed as disclosed and described herein. The formed mixed catalyst comprises a metal oxide catalyst component comprising gallium oxide and zirconium oxide; a microporous catalyst component; and a binder.
[0047] It should be understood that the activity of the resulting mixed catalyst will be higher for a feed stream containing CO as a carbon-containing gas, and the activity of the resulting mixed catalyst will decrease when the majority of the carbon-containing gas in the feed stream is CO2. However, this does not mean that the mixed catalysts disclosed and described herein cannot be used in methods in which the feed stream includes CO2 as all or most of the carbon-containing gas.
[0048] Under reaction conditions sufficient to form a product stream comprising C2 to C4 hydrocarbons, the feed stream is contacted with the formed mixed catalyst in the reaction zone. According to one or more embodiments, the reaction conditions include a temperature range within the reaction zone of 350°C to 480°C, such as 375°C to 450°C, 400°C to 450°C, 350°C to 425°C, 375°C to 425°C, 400°C to 425°C, 350°C to 400°C, or 375°C to 400°C.
[0049] In the implementation scheme, the reaction conditions include a pressure within the reaction zone of at least 1 bar (100 kPa), such as at least 5 bar (500 kPa), at least 10 bar (1,000 kPa), at least 15 bar (1,500 kPa), at least 20 bar (2,000 kPa), at least 25 bar (2,500 kPa), at least 30 bar (3,000 kPa), at least 35 bar (3,500 kPa), at least 40 bar (4,000 kPa), and at least 45 bar (4,500 kPa). Pa), at least 50 bar (5,000 kPa), at least 55 bar (5,500 kPa), at least 60 bar (6,000 kPa), at least 65 bar (6,500 kPa), at least 70 bar (7,000 kPa), at least 75 bar (7,500 kPa), at least 80 bar (8,000 kPa), at least 85 bar (8,500 kPa), at least 90 bar (9,000 kPa), at least 95 bar (9,500 kPa) or at least 100 bar (10,000 kPa). In other embodiments, the reaction conditions include pressures within the reaction zone ranging from 5 bar (500 kPa) to 100 bar (10,000 kPa), such as 10 bar (1,000 kPa) to 95 bar (9,500 kPa), 15 bar (1,500 kPa) to 90 bar (9,000 kPa), 20 bar (2,000 kPa) to 85 bar (8,500 kPa), 25 bar (2,500 kPa) to 80 bar (8,000 kPa), and 30 bar (3,000 kPa). The pressure ranges from 0 kPa to 75 bar (7,500 kPa), 35 bar (3,500 kPa) to 70 bar (7,000 kPa), 40 bar (4,000 kPa) to 65 bar (6,500 kPa), 45 bar (4,500 kPa) to 60 bar (6,000 kPa), or 50 bar (5,000 kPa) to 55 bar (5,500 kPa). In some embodiments, the pressure inside the reaction zone is from 20 bar (2,000 kPa) to 60 bar (6,000 kPa).
[0050] According to the implementation plan, the gas hourly space velocity (GHSV) in the reaction zone is from 500 per hour to 12,000 per hour, such as 500 to 10,000 per hour, 1,200 to 12,000 per hour, 1,500 to 10,000 per hour, 2,000 to 9,500 per hour, 2,500 to 9,000 per hour, 3,000 to 8,500 per hour, 3,500 to 8,000 per hour, 4,000 to 7,500 per hour, 4,500 to 7,000 per hour, 5,000 to 6,500 per hour, or 5,500 to 6,000 per hour. In some implementations, the GHSV in the reaction zone is 1,800 to 3,600 rpm, such as 2,000 to 3,600 rpm, 2,200 to 3,600 rpm, 2,400 to 3,600 rpm, 2,600 to 3,600 rpm, 2,800 to 3,600 rpm, 3,000 to 3,600 rpm, 3,200 to 3,600 rpm, or 3,400 to 3,600 rpm. In some embodiments, the GHSV within the reaction zone is 1,800 to 3,400 rpm, such as 1,800 to 3,200 rpm, 1,800 to 3,000 rpm, 1,800 to 2,800 rpm, 1,800 to 2,600 rpm, 1,800 to 2,400 rpm, 1,800 to 2,200 rpm, or 1,800 to 2,000 rpm. In some embodiments, the GHSV within the reaction zone is 2,000 to 3,400 rpm, such as 2,200 to 3,200 rpm, 2,400 to 3,000 rpm, or 2,600 to 2,800 rpm.
[0051] Compared to the catalytic functions formed individually, improved C2 to C4 olefin yields and carbon conversion can be achieved by using the mixed catalysts formed herein and the process conditions disclosed and described herein. For example, in embodiments, the hydrogen-to-carbon monoxide (H2 / CO) ratio ranges from 2 to 5, such as greater than 2.2 and less than 3.8 or greater than 2.8 and less than 3.4; the temperature ranges from 360°C to 460°C, such as 380°C to 440°C, 400°C to 420°C, or 400°C to 410°C; the pressure ranges from 5 to 100 bar, such as 20 to 80 bar or 30 to 60 bar; and the weight hourly space velocity ranges from 1 hour. -1Up to 5 hours -1 such as 1 hour -1 Up to 3 hours -1 Under these conditions, the yields of C2 to C4 olefins are greater than or equal to 4.0 mol%, such as greater than or equal to 5.0 mol%, greater than or equal to 7.0 mol%, greater than or equal to 10.0 mol%, greater than or equal to 12.0 mol%, greater than or equal to 15.0 mol%, greater than or equal to 17.0 mol%, greater than or equal to 20.0 mol%, greater than or equal to 22.0 mol%, greater than or equal to 25.0 mol%, greater than or equal to 27.0 mol%, greater than or equal to 30.0 mol%, greater than or equal to 32.0 mol%, greater than or equal to 35.0 mol%, greater than or equal to 37.0 mol%, and greater than or equal to 40.0 mol%. ≥42.0 mol%, ≥45.0 mol%, ≥47.0 mol%, ≥50.0 mol%, ≥52.0 mol%, ≥55.0 mol%, ≥57.0 mol%, ≥60.0 mol%, ≥62.0 mol%, ≥65.0 mol%, ≥67.0 mol%, ≥70.0 mol%, ≥72.0 mol%, ≥75.0 mol%, ≥77.0 mol%, ≥80.0 mol%, ≥82.0 mol%. In some embodiments, the maximum C2 to C4 olefin yield is 85.0 mol%. Therefore, in some embodiments, the C2 to C4 olefin yield is greater than or equal to 4.0 mol% to 85.0 mol%, such as 5.0 mol% to 85.0 mol%, 7.0 mol% to 85.0 mol%, 10.0 mol% to 85.0 mol%, 12.0 mol% to 85.0 mol%, 15.0 mol% to 85.0 mol%, 17.0 mol% to 85.0 mol%, 20.0 mol% to 85.0 mol%, 22.0 mol% to 85.0 mol%, 25.0 mol% to 85.0 mol%, 27.0 mol% to 85.0 mol%, 30.0 mol% to 85.0 mol%, 32.0 mol% to 85.0 mol%, 35.0 mol% to 85.0 mol%, 37.0 mol% to 85.0 mol%, or 40.0 mol% to 85.0 mol%.
[0052] In the implementation scheme, the use of the mixed catalysts and process conditions disclosed and described herein can improve carbon conversion. Within the scope of the disclosed methods, the conversion of a feed containing carbon oxides and hydrogen can be carried out in a series of reactors, wherein water byproducts are knocked out intermediately by means of, for example, phase separation, membrane separation, or some type of water-selective absorption or adsorption method. Further continuously guiding the partial conversion and anhydrous effluent to subsequent reactors and repeating this technical operation will have the overall effect of improving olefin yield.
[0053] In the implementation scheme, using the mixed catalysts formed as disclosed and described herein and the process conditions disclosed and described herein, the C2-C3 olefin selectivity / alkane selectivity ratio of the method may be greater than or equal to 2, 2 to 20, 2 to 10, 2 to 8, 2 to 6, 3 to 11, 3 to 10, 3 to 8, 3 to 6 or about 4.
[0054] In addition to improved selectivity, yield, and conversion during long-term operation, the use of a mixed catalyst formed according to the embodiments also provides these benefits over a wider range of process conditions (temperature, pressure, flow rate, etc.) in the reactor's reaction zone. For example, the mixed catalyst formed according to the embodiments disclosed and described herein allows for the use of lower reaction temperatures while still providing high conversion, selectivity, yield, and low oxygen-containing compound selectivity over time.
[0055] Example
[0056] The following examples illustrate the features of this disclosure, but are not intended to limit the scope of this disclosure. For each of the following examples and comparative examples, the microporous catalyst component was prepared as follows: SAPO-34 was synthesized according to a literature procedure (Lok, BM; Messina, CA; Patton, RL; Gajek, RT; Cannan, TR; Flanigen, EMC Crystallinesilicoaluminophosphates. U.S. Patent 4,440,871A, 1984). When calcined SAPO-34 was used, the material was calcined in air using the following procedure: heating from 25°C to 600°C at a heating rate of 5°C / min, holding at 600°C for 4 hours (h), and cooling to 25°C over 4 hours. The material was sieved into a fraction smaller than 200 mesh (smaller than 75 μm).
[0057] Example 1
[0058] Gallium-containing metal oxide catalyst components on zirconium oxide supports were prepared by a wet impregnation method. Impregnation solutions of gallium(III) nitrate hydrate (Ga(NO3)3·xH2O) and lanthanum(III) nitrate hexahydrate (La(NO3)3·6H2O) were prepared in deionized water at concentrations of 1 mol / L and 0.3 mol / L, respectively. 5 g of a ZrO2 support (manufactured by NORPRO, product code SZ31164, BET surface area = 100 m²) with a mesh size less than 200 mesh (less than 75 μm) was weighed. 2 / g, XRD showed over 95% monoclinic phase (pore volume measured with deionized water = 0.4 mL / g), and it was placed in a glass vial. Then, 2 mL of Ga and La impregnation solution was added dropwise to the support while continuously agitated. After impregnation, the metal oxide catalyst component was dried overnight at 85 °C in a forced convection oven and calcined in a muffle furnace using the following procedure: heating from 25 °C to 550 °C at a heating rate of 3 °C / min, and holding at 550 °C for 4 hours. After calcination, the catalyst was re-sieved to a diameter of less than 200 mesh (less than 75 μm) to remove larger agglomerated particles.
[0059] Powder was prepared by mixing 3.75 g of the aforementioned metal oxide catalyst component with 1.25 g of calcined SAPO-34 (less than 200 mesh, less than 75 μm) for 10 min using a mortar and pestle. Separately, pseudoboehmite (AlOOH) (manufactured by Sasol Limited, trade name Catapal D) was dissolved in water using HNO3 (65 wt.% in H2O) at an HNO3 / Al ratio of 0.05 and a total solids content of 27 wt.%. The dissolved pseudoboehmite mixture was added to the dried powder to form a paste, aiming for a pseudoboehmite concentration of 20 wt.% based on total solids (Catapal D, SAPO-34, and MMO). The paste was then mixed using a mortar and pestle for at least 10 min until an extrudable paste was obtained. The paste was transferred to a ceramic pan and dried overnight at 85 °C to form a dried precursor. The dried precursor was heated from 25°C to 600°C in a static muffle furnace at a heating rate of 2°C / min and held at 600°C for 4 hours to form a mixed catalyst. After calcination, the mixed catalyst was crushed and sieved to 40 mesh (400 μm) to 80 mesh (177 μm) for testing.
[0060] Example 2
[0061] The mixed catalyst was prepared according to Example 1, but the size of the mixed catalyst was adjusted from 20 mesh (841 μm) to 30 mesh (575 μm) for testing.
[0062] Example 3
[0063] The metal oxide catalyst component was prepared according to Example 1. A mixed catalyst was prepared according to Example 1, but 3.35 g of the metal oxide catalyst component and 1.25 g of calcined SAPO-34 were mixed to prepare the mixed catalyst. The size of the resulting mixed catalyst was adjusted from 40 mesh (400 μm) to 80 mesh (177 μm) for testing.
[0064] Example 4
[0065] The metal oxide catalyst component was prepared according to Example 1. A mixed catalyst was prepared by mixing 5 g of the above-described metal oxide catalyst component with 2.5 g of calcined SAPO-34 (less than 200 mesh, less than 75 μm) for 10 min using a mortar and pestle. 5 mL of a colloidal ZrO2 solution of zirconium oxide sol (manufactured by Daiichi Kigenso Kagaku-Kogyo Co., Ltd., trade name ZSL-10A; based on 10 wt.% ZrO2) was added to this mixture to form a paste. The paste was then mixed with a mortar and pestle for at least 10 minutes until a kneadable paste was obtained. The paste was transferred to a ceramic pan and dried overnight at 85°C to form a dried precursor. The dried precursor was heated from 25°C to 600°C in a static muffle furnace at a heating rate of 2°C / min and held at 600°C for 4 hours to form a mixed catalyst. After calcination, the resulting mixed catalyst was crushed and sieved to 40 mesh (400 μm) to 80 mesh (177 μm) for testing.
[0066] Example 5
[0067] The metal oxide catalyst component was prepared according to Example 1. A mixed catalyst was prepared according to Example 1, but 8 g of the metal oxide catalyst component was mixed with 1.808 g of uncalcined SAPO-34 to prepare the mixed catalyst. Based on total solids, the target pseudoboehmite concentration was 24.6 wt.%. The size of the resulting mixed catalyst was adjusted from 20 mesh (841 μm) to 30 mesh (575 μm) for testing.
[0068] Comparative Example 1
[0069] The metal oxide catalyst component was prepared according to Example 1, but after calcination, the catalyst was sieved to a size of 40 mesh (400 μm) to 80 mesh (177 μm) to remove fine particles.
[0070] The mixed catalyst was prepared by mixing 1g of the above-mentioned metal oxide catalyst component with 0.33g of pre-calcined SAPO-34 (40 to 80 mesh) and shaking for 30 seconds until fully mixed.
[0071] Comparative Example 2
[0072] The mixed catalyst was prepared according to Comparative Example 1, but the particle size of the metal oxide catalyst and SAPO-34 was 20 mesh (841 μm) to 30 mesh (575 μm) respectively.
[0073] Comparative Example 3
[0074] Metal oxide catalyst components were prepared according to Comparative Example 1.
[0075] A mixed catalyst was prepared by mixing 5g of the above-mentioned metal oxide catalyst component with 2.5g of calcined SAPO-34 (less than 200 mesh, less than 75μm) for 10min using a mortar and pestle. 2.925mL of a 40wt.% aqueous dispersion of colloidal titanium dioxide (manufactured by Evonik Industries, trade name) was then added to this mixture. W-740X) and 2.075 mL of deionized H2O (target 18 wt.% TiO2 binder). The components were then mixed using a mortar and pestle for at least 10 minutes until a kneadable paste was obtained. The paste was transferred to a ceramic dish and dried overnight at 85 °C to form a dried precursor. The dried precursor was heated in a static muffle furnace from 25 °C to 600 °C at a heating rate of 2 °C / min and held at 600 °C for 4 hours to form a mixed catalyst. After calcination, the mixed catalyst was crushed and sieved from 40 mesh (400 μm) to 80 mesh (177 μm) for testing.
[0076] Comparative Example 4
[0077] Metal oxide catalyst components were prepared according to Comparative Example 1.
[0078] A mixed catalyst was prepared by mixing 3.2 g of the above-mentioned metal oxide catalyst component with 0.724 g of uncalcined SAPO-34 (less than 200 mesh, less than 75 μm) for 10 min using a mortar and pestle. 1.7 mL of a 40 wt.% alkaline aqueous dispersion of colloidal silica (manufactured by Grace, trade name) was added to this mixture. AS-40) and 0.93 mL of deionized H2O (target 18 wt.% SiO2 binder). The components were then mixed using a mortar and pestle for at least 10 minutes until a kneadable paste was obtained. The paste was transferred to a ceramic dish and dried overnight at 85 °C to form a dried precursor. The dried precursor was heated in a static muffle furnace from 25 °C to 600 °C at a heating rate of 2 °C / min and held at 600 °C for 4 hours to form a mixed catalyst. After calcination, the mixed catalyst was crushed and sieved from 40 mesh (400 μm) to 80 mesh (177 μm) for testing.
[0079] Comparative Example 5
[0080] Metal oxide catalyst components were prepared according to Comparative Example 1.
[0081] The mixed catalyst was prepared by mixing 0.8g of the above-mentioned metal oxide catalyst component with 0.2g of pre-calcined SAPO-34 (40 to 80 mesh) and shaking for 30 seconds until fully mixed.
[0082] Catalytic performance data
[0083] The mixed catalyst was tested in a stainless steel fixed-bed reactor system (7.7 mm inner diameter) under the conditions shown in Table 1. The equilibrium gas volume was 10%.
[0084] Table 1
[0085] Temperature (°C) <![CDATA[H2 / CO ratio]]> Stress (Barg) <![CDATA[Weight hourly space velocity (hour -1 )]]> Condition 1 420 3 50 1.54 Condition 2 400 3 40 1.54 Condition 3 400 3 40 1.37 Condition 4 420 3 40 1.87 Condition 5 420 3.3 40 2.79 Condition 6 400 3.3 40 2.79 Condition 7 430 2 40 3
[0086] In conditions 1 to 4, the WHSV remains constant based on the same active catalyst (WHSV). (MMO+SAPO-34) In conditions 5 through 7, the total WHSV (including binder, for example) remained constant. The catalyst was heated to the reaction temperature and pressure under nitrogen (N2) before contact with the synthesis gas. The reactor effluent composition was obtained by gas chromatography, and the conversion and carbon-based selectivity were calculated using the following equations:
[0087] WHSV (MMO+SAPO-34) =(F CO +F H2 ) / W MMO +W SAPO-34
[0088] WHSV=(FCO+FH2) / W 催化剂
[0089] Where F CO and F H2 Let W be defined as the mass flow rates of CO and H2, respectively.MMO W SAPO-34 and W 催化剂 These are defined as the mass of the MMO component, the mass of the SAPO-34 component, and the total catalyst mass (including binder), respectively.
[0090] X CO (%)=[(η CO,in –η CO,out ) / η CO,in ]·100; and (1)
[0091] S j (%) = [α] j ·η j,out / (η CO,in –η CO,out )]·100, (2)
[0092] Where X CO Defined as CO conversion rate (%), η CO,in The molar inlet flow rate of CO (μmol / s), η CO,out S is the molar outlet flow rate of CO (μmol / s). j α is defined as the carbon-based selectivity (%) for product j. j η is the number of carbon atoms in product j. j,out denoted as the molar outlet flow rate (μmol / s) of product j. All data were collected under steady-state conditions after a run of at least 40 hours.
[0093] The results of the catalytic test are shown in Table 2 below.
[0094] Table 2
[0095]
[0096] *The C2 / C3 ratio refers to the total C2 hydrocarbon (total C-mol selectivity of ethylene and ethane) / total C3 hydrocarbon (total C-mol selectivity of propylene and propane).
[0097] As shown in Table 2, the comparison of Examples 1 to 2 with Comparative Examples 1 to 2 demonstrates that the performance of the single-particle formulation is improved compared to the two-particle mixture when larger particles are loaded into the reactor. While the two-particle mixture is subject to transport limitations, the single-particle formulation maintains the same performance between large and small particles loaded into the reactor. Furthermore, the single-particle formulation achieves higher olefin selectivity and C2 / C3 ratio while maintaining low oxygen-containing compound selectivity, resulting in a higher absolute ethylene yield. The single-particle formulation also exhibits broader operability, particularly at lower operating temperatures. As shown in Comparative Example 2 under Condition 2, the two-particle formulation exhibits high oxygen-containing compound selectivity when operated at 400°C.
[0098] The comparison of Examples 3 to 4 with Comparative Examples 3 to 4 demonstrates the importance of the binder used. Al2O3 and ZrO2 binders provide comparable performance, while TiO2 and SiO2 binders lead to olefin hydrogenation or catalyst poisoning, respectively.
[0099] Example 5 shows the performance of the 4:1 single-grain formulation compared to the 4:1 dual-grain formulation in Comparative Example 5 under different reaction conditions. At the same total WHSV, the single-grain formulation exhibits comparable conversion to the dual-grain system, but with significantly higher hydrocarbon and olefin selectivity and a higher C2 / C3 ratio. Additionally, as shown in condition 6, the single-grain formulation allows for reaction at lower temperatures without oxygen-containing compound selectivity.
[0100] It should be noted that one or more of the following claims utilize the terms "where" or "in which" as transitional phrases. For the purpose of defining this technology, it should be noted that this term is introduced in the claims as an open-ended transitional phrase used to introduce a description of a series of characteristics of the structure, and should be interpreted in a manner similar to the more commonly used open-ended prepositional term "comprising." For the purpose of defining this invention, the transitional phrase "consisting of..." may be introduced in the claims as a closed prepositional term, limiting the scope of the claims to the listed components or steps and any naturally occurring impurities. For the purpose of defining this invention, the transitional phrase "consisting substantially of..." may be introduced in the claims to limit the scope of one or more claims to the stated elements, components, materials, or method steps and any non-stated elements, components, materials, or method steps that do not substantially affect the novelty of the claimed subject matter. The transitional phrases “composed of” and “substantially composed of” can be interpreted as open-ended transitional phrases, such as subsets of “comprising” and “including”, such that any use of an open-ended phrase to introduce a list of elements, components, materials, or steps should be interpreted as also disclosing a list of elements, components, materials, or steps that also use the closed terms “composed of” and “substantially composed of”. For example, a statement that a composition “comprising” components A, B, and C should be interpreted as also disclosing a composition “composed of” components A, B, and C, and a composition “substantially composed of” components A, B, and C. Any quantitative values expressed in this application can be considered to include open-ended embodiments conforming to the transitional phrases “comprising” or “including”, as well as closed or partially closed embodiments conforming to the transitional phrases “composed of” and “substantially composed of”.
[0101] As used in the specification and appended claims, unless the context clearly indicates otherwise, the singular forms “a,” “an,” and “the” include plural references. The verb “comprising” and its homologous forms should be interpreted as referring to an element, component, or step in a non-exclusive manner. The referenced element, component, or step may exist, be used, or be combined with other elements, components, or steps not expressly referenced.
[0102] It should be understood that any two quantitative values assigned to a characteristic can constitute a range for that characteristic, and all combinations of ranges formed by all said quantitative values of a given characteristic are considered in this disclosure. The subject matter of this disclosure has been described in detail and by reference to specific embodiments. It should be understood that any detailed description of a component or feature of one or more embodiments does not necessarily imply that the component or feature is necessary for a particular embodiment or any other embodiment. Furthermore, it will be apparent to those skilled in the art that various modifications and changes can be made to the described embodiments without departing from the spirit and scope of the claimed subject matter.
Claims
1. A method for preparing C2 to C4 hydrocarbons, the method comprising: A feed stream containing hydrogen and carbon-containing gases selected from the group consisting of carbon monoxide, carbon dioxide, and mixtures thereof is introduced into the reaction zone of the reactor. as well as In the presence of a formed mixed catalyst, the feed stream is converted into a product stream containing C2 to C4 hydrocarbons in the reaction zone, the formed mixed catalyst comprising: The metal oxide catalyst component includes gallium oxide and zirconium oxide; A microporous catalyst component, wherein the microporous catalyst component is a molecular sieve with 8-membered ring pore openings; and Adhesive, said adhesive comprising alumina, zirconium oxide, or both, The binder is used to combine the metal oxide component and the microporous catalyst component into a single catalyst body.
2. A method for preparing a mixed catalyst, the method comprising: Mixed metal oxide catalyst components and microporous catalyst components, wherein The metal oxide catalyst composition includes gallium oxide and zirconium oxide; and The microporous catalyst component includes a molecular sieve with an 8-membered ring pore opening; A binder is added to a mixture of the metal oxide catalyst component and the microporous catalyst component to form a paste, wherein the binder is a colloidal solution, suspension, or gel comprising a binder precursor including aluminum oxide or hydroxide, zirconium oxide or hydroxide, or mixtures thereof; and The paste is extruded to produce the resulting mixed catalyst.
3. The method according to claim 1 or 2, wherein the metal oxide catalyst component has a particle size of less than 150 µm.
4. The method according to any one of claims 1 to 3, wherein the metal oxide catalyst component further comprises lanthanum.
5. The method according to any one of claims 1 to 4, wherein the formed mixed catalyst has a particle size of 0.5 mm to 6 mm.
6. The method according to any one of claims 1 to 4, wherein the formed mixed catalyst has a particle size of 1.5 mm to 3.0 mm.
7. The method according to any one of claims 1 to 6, wherein the metal oxide catalyst component comprises from 0.1 g gallium oxide per 100 g zirconium oxide to 30.0 g gallium oxide per 100 g zirconium oxide.
8. The method according to any one of claims 1 to 7, wherein the microporous catalyst component comprises SAPO-34.
9. The method according to any one of claims 1 to 7, wherein the microporous catalyst component comprises uncalcined SAPO-34.
10. The method according to any one of claims 1 to 9, wherein the binder comprises pure alumina.
11. The method according to any one of claims 1 to 10, wherein the binder comprises pure zirconium oxide.
12. The method according to any one of claims 1 to 11, wherein the metal oxide catalyst component accounts for 40.0 wt.% to 80.0 wt.% of the formed mixed catalyst.
13. The method according to any one of claims 1 to 12, wherein the metal oxide catalyst component is formed by impregnation.
14. The method according to any one of claims 1 to 13, wherein the temperature within the reaction zone is 350°C to 480°C during the conversion.
15. The method according to any one of claims 1 to 3 to 14, wherein the method has a C2-C3 olefin selectivity / alkane selectivity ratio of 2 to 20.
16. The method according to any one of claims 1 and 15, wherein the metal oxide catalyst component, the binder, or both the metal oxide component and the binder are substantially free of silicon dioxide.
Citation Information
Patent Citations
Catalyst comprising an EUO zeolite, a 10 mr zeolite and a 12 mr zeolite, and its use in isomerizing aromatic c8 compounds
US20090093661A1
Catalysts comprising a zirconia and gallium oxide component for production of c 2 to c 4 olefins