A transition metal-based ceramic coating and preparation method thereof

By using materials such as fused corundum, graphene, zirconia and titanium boride, combined with the hydrolyzed solution of methyl silicone leveling agent, a high-performance transition metal-based ceramic coating is prepared, which solves the problem of insufficient strength of metal-based ceramic coatings. problems, significantly improving its application scope.

CN116874286BActive Publication Date: 2024-10-18SU ZHOU LANG MOU ER KE JI YOU XIAN GONG SI
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202310785381.8
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-06-29
Publication Date
2024-10-18
Estimated Expiration
2043-06-29

AI Technical Summary

Technical Problem

The strength of existing metal-based ceramic coatings is low, which limits their application scope.

Method used

Using fused corundum, graphene, zirconia and titanium boride as basic materials, and adding methyl silicone oil leveling agent to the hydrolysis solution to prepare a transition metal-based ceramic coating, the composite ceramic powder is obtained by calcination and then applied on Sintering is performed on the substrate at a sintering temperature of 1400-1600°C.

Benefits of technology

The hardness, thermal conductivity, electrical conductivity, oxidation resistance and chemical stability of the metal-based ceramic coating are improved, and the wear resistance and resistance to liquid metal erosion are enhanced, thereby improving the overall performance and strength of the coating.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The present invention provides a transition metal-based ceramic coating, including the following raw material components by weight: 10-25 parts of fused corundum, 5-10 parts of graphene, 5-10 parts of zirconium oxide, 5-15 parts of titanium boride and 25-40 parts of water, and also including a hydrolysis solution prepared by 30-50 parts of anhydrous ethanol, 30-50 parts of distilled water and 20-40 parts of a leveling agent. The present invention adopts fused corundum, graphene, zirconium oxide and titanium boride as the basic materials for preparing metal-based ceramic coatings, and titanium boride has high hardness, high thermal conductivity and electrical conductivity, good antioxidant performance and chemical stability, excellent wear resistance and resistance to liquid metal erosion, thereby improving the strength and overall performance of the metal-based ceramic coating. Secondly, in the process of preparing the metal-based ceramic coating, a methyl silicone oil leveling agent is added to the hydrolysis solution, so that the metal-based ceramic coating is quickly and naturally leveled on the surface of the substrate, and the efficiency of coating preparation is improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of ceramic coatings, in particular to a transition metal-based ceramic coating and a preparation method thereof. Background Art

[0002] Cermet is a structural material composed of a ceramic hard phase and a metal or alloy bonding phase. The coating formed by thermal spraying or laser cladding, high temperature melting method, vapor deposition, wet deposition and other coating technologies is a cermet coating. The high temperature melting and sintering method is to make the coating raw material into a slurry at room temperature, and then evenly apply it on the metal surface, and prepare the coating material by high temperature melting and sintering. This method has the characteristics of simple equipment and convenient operation. It is one of the important methods for preparing ceramic coatings. In addition, this method can also repair the damaged coating, which can not only achieve self-compensation through high temperature treatment, but also through filling slurry and appropriate high temperature treatment.

[0003] At present, when metal-based ceramic coatings are prepared by high-temperature melting method, aluminum oxide, titanium oxide, zirconium oxide, chromium oxide and their composite compounds are generally used as the main materials. The performance of the metal-based coating is improved by adding other auxiliary materials to the above materials. However, compared with carbide ceramic coatings, the strength of metal-based ceramic coatings is relatively low, which limits the application range of metal-based ceramic coatings. Summary of the invention

[0004] 1. Technical issues to be resolved

[0005] In view of the deficiencies in the prior art, the present invention provides a transition metal-based ceramic coating and a preparation method thereof, which solves the problem of insufficient strength of the current metal-based ceramic coating.

[0006] (II) Technical solution

[0007] To achieve the above objectives, the present invention is implemented by the following technical scheme: a transition metal-based ceramic coating, comprising the following raw material components in parts by weight: 10-25 parts of fused corundum, 5-10 parts of graphene, 5-10 parts of zirconium oxide, 5-15 parts of titanium boride and 25-40 parts of water;

[0008] The invention also comprises a hydrolysis solution prepared by 30-50 parts of anhydrous ethanol, 30-50 parts of distilled water and 20-40 parts of a leveling agent.

[0009] The transition metal-based ceramic coating is prepared according to the following raw materials in parts by weight: 10 parts of fused corundum, 5 parts of graphene, 5 parts of zirconium oxide, 5 parts of titanium boride and 25 parts of water, 30 parts of anhydrous ethanol, 30 parts of distilled water and 20 parts of a leveling agent.

[0010] The transition metal-based ceramic coating is prepared according to the following raw materials in parts by weight: 15 parts of fused corundum, 7 parts of graphene, 7 parts of zirconium oxide, 7 parts of titanium boride and 35 parts of water, 40 parts of anhydrous ethanol, 40 parts of distilled water and 25 parts of a leveling agent.

[0011] The transition metal-based ceramic coating is prepared according to the following raw materials in parts by weight: 25 parts of fused corundum, 10 parts of graphene, 10 parts of zirconium oxide, 15 parts of titanium boride and 40 parts of water, 50 parts of anhydrous ethanol, 50 parts of distilled water and 40 parts of a leveling agent.

[0012] A method for preparing a transition metal-based ceramic coating comprises the following specific steps:

[0013] Step 1: Prepare the fused corundum, graphene, zirconium oxide and titanium boride according to the mixing ratio;

[0014] Step 2: Add the mixed materials prepared in step 1 into a mixing tank, then add a corresponding proportion of water into the mixing tank, and fully mix and stir the above materials in the mixing tank to obtain a mixed solution, and the stirring time is 30-60 minutes;

[0015] Step 3: Prepare the materials of anhydrous ethanol, distilled water and leveling agent according to the mixing ratio;

[0016] Step 4: Add the solution prepared in step 3 into a mixing tank, and fully mix anhydrous ethanol, distilled water and leveling agent in the mixing tank to obtain a hydrolysis solution, with a stirring time of 15-20 minutes;

[0017] Step 5: adding the mixed solution obtained in step 2 to the hydrolysis solution obtained in step 4, and stirring the mixed solution and the hydrolysis solution in a mixing tank for 30 minutes. After the mixing is completed, the mixture is allowed to stand at room temperature for more than 60 minutes.

[0018] Step 6: Add the solution after standing in step 5 into a drying oven, and calcine to obtain a composite ceramic powder, the calcination temperature is greater than 1200° C., calcination for 2 hours, and heat preservation for 1 hour;

[0019] Step 7: Add distilled water to the composite ceramic powder in step 6 to obtain a ceramic coating slurry, then apply the ceramic coating slurry on the substrate, and then sinter the substrate at a sintering temperature of 1400-1600°C.

[0020] Preferably, the stirring speed of the mixing tank is controlled at 200-300 r / min.

[0021] Preferably, the particle size of the fused corundum, graphene, zirconium oxide and titanium boride powder is 1-5 μm. Controlling the particle size of the fused corundum, graphene, zirconium oxide and titanium boride powder allows the prepared ceramic coating slurry to be finely applied to the surface of the substrate.

[0022] (III) Beneficial effects

[0023] The present invention provides a transition metal-based ceramic coating and a preparation method thereof. The coating has the following beneficial effects:

[0024] The present invention uses fused corundum, graphene, zirconium oxide and titanium boride as basic materials for preparing metal-based ceramic coatings. Titanium boride in the metal-based ceramic coating has high hardness, high thermal conductivity and electrical conductivity, good oxidation resistance and chemical stability, excellent wear resistance and liquid metal corrosion resistance, thereby improving the strength and overall performance of the metal-based ceramic coating. Secondly, in the process of preparing the metal-based ceramic coating, a methyl silicone oil leveling agent is added to the hydrolysis solution, so that the metal-based ceramic coating can be quickly and naturally leveled on the surface of the substrate, thereby improving the efficiency of coating preparation. DETAILED DESCRIPTION

[0025] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present invention.

[0026] Embodiment 1:

[0027] The embodiment of the present invention provides a transition metal-based ceramic coating, comprising the following raw material components in parts by weight: 10-25 parts of fused corundum, 5-10 parts of graphene, 5-10 parts of zirconium oxide, 5-15 parts of titanium boride and 25-40 parts of water;

[0028] It also includes a hydrolysis solution prepared from 30-50 parts of anhydrous ethanol, 30-50 parts of distilled water and 20-40 parts of a leveling agent. In this embodiment, the leveling agent is a methyl silicone oil leveling agent, which can make the prepared ceramic coating slurry quickly and naturally level on the surface of the substrate.

[0029] The transition metal-based ceramic coating is prepared according to the following raw materials in parts by weight: 10 parts of fused corundum, 5 parts of graphene, 5 parts of zirconium oxide, 5 parts of titanium boride and 25 parts of water, 30 parts of anhydrous ethanol, 30 parts of distilled water and 20 parts of a leveling agent.

[0030] The preparation method of the transition metal-based ceramic coating comprises the following specific steps:

[0031] Step 1: Prepare the fused corundum, graphene, zirconium oxide and titanium boride according to the mixing ratio; use an electronic scale to weigh the various raw materials to achieve a strict ratio of each material.

[0032] Step 2: Add the mixed materials prepared in step 1 into a mixing tank, then add a corresponding proportion of water into the mixing tank, and fully mix and stir the above materials in the mixing tank to obtain a mixed solution. The stirring time is 30-60 minutes. Before use, the mixing tank needs to be cleaned and dried inside, and then the mixed raw materials are added to the mixing tank. When adding water, it is necessary to stir while adding water.

[0033] Step 3: Prepare the materials of anhydrous ethanol, distilled water and leveling agent according to the mixing ratio;

[0034] Step 4: Add the solution prepared in step 3 into a mixing tank, and fully mix anhydrous ethanol, distilled water and a leveling agent in the mixing tank to obtain a hydrolysis solution. The stirring time is 15-20 minutes. When preparing the hydrolysis solution, add anhydrous ethanol and distilled water first, and then add the leveling agent.

[0035] Step 5: Add the mixed solution obtained in step 2 to the hydrolysis solution obtained in step 4, and stir the mixed solution and the hydrolysis solution in a mixing tank for 30 minutes. After mixing, let it stand at room temperature for more than 60 minutes. When stirring the mixed solution and the hydrolysis solution, add nitric acid catalyst to form a gel solution.

[0036] Step 6: Add the solution after standing in step 5 into a drying oven, and calcine to obtain a composite ceramic powder, the calcination temperature is greater than 1200° C., calcination for 2 hours, and heat preservation for 1 hour;

[0037] Step 7: Add distilled water to the composite ceramic powder in step 6 to obtain a ceramic coating slurry, then apply the ceramic coating slurry on the substrate, and then sinter the substrate at a sintering temperature of 1400-1600°C.

[0038] Embodiment 2:

[0039] This embodiment is based on the embodiment one: the transition metal-based ceramic coating is prepared according to the following raw materials in parts by weight: 15 parts of fused corundum, 7 parts of graphene, 7 parts of zirconium oxide, 7 parts of titanium boride and 35 parts of water, 40 parts of anhydrous ethanol, 40 parts of distilled water and 25 parts of leveling agent.

[0040] The preparation method of the transition metal-based ceramic coating comprises the following specific steps:

[0041] Step 1: Prepare the fused corundum, graphene, zirconium oxide and titanium boride according to the mixing ratio;

[0042] Step 2: Add the mixed materials prepared in step 1 into a mixing tank, then add a corresponding proportion of water into the mixing tank, and fully mix and stir the above materials in the mixing tank to obtain a mixed solution, and the stirring time is 30-60 minutes;

[0043] Step 3: Prepare the materials of anhydrous ethanol, distilled water and leveling agent according to the mixing ratio;

[0044] Step 4: Add the solution prepared in step 3 into a mixing tank, and fully mix anhydrous ethanol, distilled water and leveling agent in the mixing tank to obtain a hydrolysis solution, with a stirring time of 15-20 minutes;

[0045] Step 5: adding the mixed solution obtained in step 2 to the hydrolysis solution obtained in step 4, and stirring the mixed solution and the hydrolysis solution in a mixing tank for 30 minutes. After the mixing is completed, the mixture is allowed to stand at room temperature for more than 60 minutes.

[0046] Step 6: Add the solution after standing in step 5 into a drying oven, and calcine to obtain a composite ceramic powder, the calcination temperature is greater than 1200° C., calcination for 2 hours, and heat preservation for 1 hour;

[0047] Step 7: Add distilled water to the composite ceramic powder in step 6 to obtain a ceramic coating slurry, then apply the ceramic coating slurry on the substrate, and then sinter the substrate at a sintering temperature of 1400-1600°C.

[0048] Embodiment three:

[0049] This embodiment is based on the embodiment one: the transition metal-based ceramic coating is prepared according to the following raw materials in parts by weight: 25 parts of fused corundum, 10 parts of graphene, 10 parts of zirconium oxide, 15 parts of titanium boride and 40 parts of water, 50 parts of anhydrous ethanol, 50 parts of distilled water and 40 parts of leveling agent.

[0050] The preparation method of the transition metal-based ceramic coating comprises the following specific steps:

[0051] Step 1: Prepare the fused corundum, graphene, zirconium oxide and titanium boride according to the mixing ratio;

[0052] Step 2: Add the mixed materials prepared in step 1 into a mixing tank, then add a corresponding proportion of water into the mixing tank, and fully mix and stir the above materials in the mixing tank to obtain a mixed solution, and the stirring time is 30-60 minutes;

[0053] Step 3: Prepare the materials of anhydrous ethanol, distilled water and leveling agent according to the mixing ratio;

[0054] Step 4: Add the solution prepared in step 3 into a mixing tank, and fully mix anhydrous ethanol, distilled water and leveling agent in the mixing tank to obtain a hydrolysis solution, with a stirring time of 15-20 minutes;

[0055] Step 5: adding the mixed solution obtained in step 2 to the hydrolysis solution obtained in step 4, and stirring the mixed solution and the hydrolysis solution in a mixing tank for 30 minutes. After the mixing is completed, the mixture is allowed to stand at room temperature for more than 60 minutes.

[0056] Step 6: Add the solution after standing in step 5 into a drying oven, and calcine to obtain a composite ceramic powder, the calcination temperature is greater than 1200° C., calcination for 2 hours, and heat preservation for 1 hour;

[0057] Step 7: Add distilled water to the composite ceramic powder in step 6 to obtain a ceramic coating slurry, then apply the ceramic coating slurry on the substrate, and then sinter the substrate at a sintering temperature of 1400-1600°C.

[0058] It should be noted that, in this article, relational terms such as first and second, etc. are only used to distinguish one entity or operation from another entity or operation, and do not necessarily require or imply any such actual relationship or order between these entities or operations. Moreover, the terms "include", "comprise" or any other variants thereof are intended to cover non-exclusive inclusion, so that a process, method, article or device including a series of elements includes not only those elements, but also other elements not explicitly listed, or also includes elements inherent to such process, method, article or device. In the absence of further restrictions, the elements defined by the statement "comprising a reference structure" do not exclude the existence of other identical elements in the process, method, article or device including the elements.

[0059] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.

Claims

1. A transition metal-based ceramic coating, characterized in that: The method comprises the following raw material components in parts by weight: 10-25 parts of fused corundum, 5-10 parts of graphene, 5-10 parts of zirconium oxide, 5-15 parts of titanium boride and 25-40 parts of water; The hydrolysis solution is prepared by 30-50 parts of anhydrous ethanol, 30-50 parts of distilled water and 20-40 parts of a leveling agent, wherein the leveling agent is a methyl silicone oil leveling agent; The preparation method of the transition metal-based ceramic coating comprises the following specific steps: Step 1: Prepare the fused corundum, graphene, zirconium oxide and titanium boride according to the mixing ratio; Step 2: Add the mixed materials prepared in step 1 into a mixing tank, then add a corresponding proportion of water into the mixing tank, and fully mix and stir the above materials in the mixing tank to obtain a mixed solution, and the stirring time is 30-60 minutes; Step 3: Prepare the materials of anhydrous ethanol, distilled water and leveling agent according to the mixing ratio; Step 4: Add the solution prepared in step 3 into a mixing tank, and fully mix anhydrous ethanol, distilled water and leveling agent in the mixing tank to obtain a hydrolysis solution, with a stirring time of 15-20 minutes; Step 5: adding the mixed solution obtained in step 2 to the hydrolysis solution obtained in step 4, and stirring the mixed solution and the hydrolysis solution in a mixing tank for 30 minutes. After the mixing is completed, the mixture is allowed to stand at room temperature for more than 60 minutes. Step 6: Add the solution after standing in step 5 into a drying oven, and calcine to obtain a composite ceramic powder, the calcination temperature is greater than 1200° C., calcination for 2 hours, and heat preservation for 1 hour; Step 7: Add distilled water to the composite ceramic powder in step 6 to obtain a ceramic coating slurry, then apply the ceramic coating slurry on the substrate, and then sinter the substrate at a sintering temperature of 1400-1600°C.

2. A transition metal-based ceramic coating according to claim 1, characterized in that: The transition metal-based ceramic coating is prepared according to the following raw materials in parts by weight: 10 parts of fused corundum, 5 parts of graphene, 5 parts of zirconium oxide, 5 parts of titanium boride and 25 parts of water, 30 parts of anhydrous ethanol, 30 parts of distilled water and 20 parts of a leveling agent.

3. A transition metal-based ceramic coating according to claim 1, characterized in that: The transition metal-based ceramic coating is prepared according to the following raw materials in parts by weight: 15 parts of fused corundum, 7 parts of graphene, 7 parts of zirconium oxide, 7 parts of titanium boride and 35 parts of water, 40 parts of anhydrous ethanol, 40 parts of distilled water and 25 parts of a leveling agent.

4. A transition metal-based ceramic coating according to claim 1, characterized in that: The transition metal-based ceramic coating is prepared according to the following raw materials in parts by weight: 25 parts of fused corundum, 10 parts of graphene, 10 parts of zirconium oxide, 15 parts of titanium boride and 40 parts of water, 50 parts of anhydrous ethanol, 50 parts of distilled water and 40 parts of a leveling agent.

5. The transition metal-based ceramic coating according to claim 1, characterized in that: The stirring speed of the mixing tank is controlled at 200-300r / min.

6. A transition metal-based ceramic coating according to claim 1, characterized in that: The particle size of the fused corundum, graphene, zirconium oxide and titanium boride powders is 1-5 μm.

Citation Information

Patent Citations

  • Aluminum oxide ceramic coating and preparation method thereof

    CN109440051A

  • Titanium diboride-based nanometer composite cutter material and preparation method thereof

    CN111170755A