Electrodes, their preparation methods, anodes for water electrolysis, electrolysis units, and methods for producing hydrogen.
By forming a LaNixMyO3-z layer on the electrode substrate, the problem of high oxygen overvoltage after long-term energization of the anode was solved, realizing a low-cost and efficient water electrolysis process.
Patent Information
- Application Number
- CN202280013696.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2021-09-29
- Filing Date
- 2022-03-25
- Publication Date
- 2026-11-10
- Estimated Expiration
- 2042-03-25
AI Technical Summary
The existing anodes used in water electrolysis have insufficient oxygen overvoltage after long-term energization, making it difficult to meet the needs of efficient hydrogen production.
An electrode is used to form a LaNixMyO3-z layer on a substrate, wherein x+y is 0.8 to 1.2, y is 0.001 to 0.6, z is -0.5 to 0.5, and M contains at least one of Nb, Ta, Sb, Ti, Mn, and Zr. The initial bilayer capacitance is greater than 0.6 F/cm2, and the layer is prepared by a specific process.
Even after prolonged energization, the electrodes still exhibit low oxygen overvoltage, improving the energy efficiency of water electrolysis and reducing costs.
Smart Images

Figure BDA0004379877490000241 
Figure BDA0004379877490000291 
Figure BDA0004379877490000301
Abstract
Description
Technical Field
[0001] This invention relates to electrodes, methods for their preparation, anodes for water electrolysis, electrolysis units using the anodes for water electrolysis, and methods for producing hydrogen using the anodes for water electrolysis. Background Technology
[0002] In recent years, hydrogen produced using renewable energy sources has garnered attention as a clean energy source for addressing global warming caused by CO2 and the depletion of fossil fuel reserves. Hydrogen production using renewable energy sources demands low costs comparable to existing fossil fuel-based modified hydrogen production methods. Therefore, the production of hydrogen using renewable energy sources requires high levels of energy efficiency and low-cost equipment that cannot be achieved with current technologies.
[0003] As a method for producing hydrogen that can meet the above requirements, water electrolysis (water electrolysis) can be cited as an example. For example, several ideas have also been proposed to produce hydrogen and store or transport it by using water electrolysis through power generation based on natural energy sources such as wind or sunlight.
[0004] In the electrolysis of water, oxygen is produced at the anode and hydrogen at the cathode by flowing an electric current through the water. Overvoltage at both the anode and cathode is a major cause of energy loss during electrolysis. By reducing this overvoltage, hydrogen can be produced efficiently. In particular, the overvoltage at the anode is higher than that at the cathode, and extensive research and development have been conducted to reduce the overvoltage at the anode.
[0005] Among oxides with a perovskite structure, materials with high oxygen evolution capacity are known, and they have attracted attention as anode materials for water electrolysis (Non-Patent Document 1). To use oxides with a perovskite structure as anodes for alkaline water electrolysis, there are methods for forming an oxide layer on the surface of a conductive substrate. For example, Patent Document 1 discloses a water electrolysis anode with low oxygen evolution overvoltage (oxygen overvoltage) and high durability, formed on the surface of a nickel porous substrate by forming a layer of metal oxide with a high content of perovskite oxide in the crystalline composition, and a water electrolysis apparatus using this anode.
[0006] Existing technical documents
[0007] Patent documents
[0008] Patent Document 1: International Publication No. 2018 / 155503
[0009] Non-patent literature
[0010] Non-patent literature 1: Science, 2011, 334, 1383 Summary of the Invention
[0011] The problem that the invention aims to solve
[0012] However, it is known that the anode described in Patent Document 1 has the problem that the oxygen overvoltage is not low enough after long-term energization.
[0013] The present invention was made in view of the following problems, and its object is to provide an electrode that exhibits low oxygen overvoltage even after long-term energization, a method for preparing the electrode, an anode for water electrolysis, an electrolysis unit using the anode for water electrolysis, and a method for producing hydrogen using the anode for water electrolysis.
[0014] Methods for solving problems
[0015] To address the aforementioned issues, the inventors conducted in-depth research and repeated experiments. The results revealed that LaNi0.05 on the substrate... x M y O 3-z The initial double-layer capacitor had a low oxygen overvoltage even after long-term energization, thus completing the present invention.
[0016] That is, the present invention is as follows.
[0017] [1] An electrode characterized in that it has LaNi on a substrate. x M y O 3-z (x+y is 0.8 to 1.2, y is 0.001 to 0.6, z is -0.5 to 0.5, and M must contain at least one of Nb, Ta, Sb, Ti, Mn, or Zr), and the initial double-layer capacitance is greater than 0.6 F / cm. 2 .
[0018] [2] The electrode as described in [1], wherein every 1 cm 2 The molar amount of La is between 0.06 mmol and 1.1 mmol.
[0019] [3] The electrode as described in [1] or [2], wherein the electrostatic capacitance per 1 mmol of La is 10 F or more and 25 F or less.
[0020] [4] The electrode as described in any one of [1] to [3], wherein the above-mentioned LaNi x M y O 3-z The adhesion amount is greater than 145g / m 2 And it is 3500g / m 2 the following.
[0021] [5] The electrode as described in any one of [1] to [4], wherein the above-mentioned LaNi x M y O3-z The position of the main peak in the XRD pattern is between 32.6° and 33.2°.
[0022] [6] The electrode as described in any one of [1] to [5], wherein the above-mentioned LaNi x M y O 3-z The y is greater than 0.002 and less than 0.2.
[0023] [7] The electrode as described in any one of [1] to [6], wherein the above-mentioned LaNi x M y O 3-z The position of the main peak in the XRD pattern is between 32.7° and 33.2°.
[0024] [8] The electrode as described in any one of [1] to [7], wherein the above-mentioned LaNi x M y O 3-z M is Nb.
[0025] [9] The electrode as described in any one of [1] to [8], wherein, in the above-described LaNi x M y O 3-z A 20μm square region in the layer, larger than 0.785μm. 2 And it is 20μm 2 The total area of the following pores is 10 μm. 2 Above 200μm 2 the following.
[0026]
[10] The electrode as described in any one of [1] to [9], wherein, in the above-described LaNi x M y O 3-z In a 20μm square region within the layer, the average pore area is greater than 0.785μm. 2 And it is 10μm 2 the following.
[0027]
[11] The electrode as described in any one of [1] to
[10] , wherein, in the above-described LaNi x M y O 3-z The average number of pores in a 20μm square region of the layer is between 20 and 150.
[0028]
[12] An electrolysis unit, characterized in that it is formed by using any one of the electrodes [1] to
[11] in the anode.
[0029]
[13] A method for producing hydrogen, characterized in that a variable power source is input into the electrolysis unit described in
[12] .
[0030]
[14] A method for producing hydrogen, wherein hydrogen is produced by electrolyzing water containing alkali in an electrolytic cell, characterized in that the electrolytic cell has at least an anode and a cathode, wherein the anode has LaNi on a substrate. x M y O 3-z (x+y is 0.8 to 1.2, y is 0.001 to 0.6, z is -0.5 to 0.5, and M must contain at least one of Nb, Ta, Sb, Ti, Mn, or Zr), and the initial double-layer capacitance is greater than 0.6 F / cm. 2 .
[0031]
[15] A method for preparing an electrode according to any one of [1] to
[11] , characterized in that it includes a step of calcining a mixture of La(NO3)3, Ni(NO3)2, and a compound having a carboxyl group and an amino group and having C, H, N and O as constituent elements, wherein the combustion by-product gases (CO2, H2O and N2) generated in the calcination are relative to the LaNi x M y O 3-z molar ratio (combustion byproducts / LaNi) x M y O 3-z The value is 5 or higher and less than 12.6.
[0032]
[16] A method for preparing an electrode according to any one of [1] to
[11] , characterized in that it includes a step of calcining a mixture of La(NO3)3, Ni(NO3)2 and glycine, wherein the glycine / NO3 ratio in the mixture is... - The molar ratio is between 0.1 and 0.3.
[0033] The effects of the invention
[0034] According to the present invention, an electrode that exhibits a low oxygen overvoltage even after long-term energization, an anode for water electrolysis, and a water electrolysis unit having the anode for water electrolysis can be obtained. Attached Figure Description
[0035] Figure 1 This is an overall side view showing an example of an electrolytic cell, which includes an electrolysis unit having the electrodes of this embodiment as anodes.
[0036] Figure 2 This is an example of an electrolytic cell. Figure 1The diagram shows a cross-section of the electrolytic cell within the dashed square portion, which includes an electrolytic cell having the electrode of this embodiment as the anode.
[0037] Figure 3 This is a diagram showing an outline of the electrolysis apparatus used in the embodiments and comparative examples.
[0038] Figure 4 This is a diagram showing the outline of the bipolar electrolyzer used in the electrolysis experiment.
[0039] Figure 5 This is a diagram showing the equivalent circuit fitting model used in the calculation of double-layer capacitors.
[0040] Figure 6 This is an example of a cross-sectional photograph of the electrode and the setting of the 20μm square area that was cut out.
[0041] Figure 7 From Figure 6 An example of an image of a 20μm square region cut from the middle.
[0042] Figure 8 From Figure 7 An example of an image obtained by binarizing and extracting fine holes. Detailed Implementation
[0043] The specific embodiments of the present invention (hereinafter referred to as "this embodiment") will be described in detail below. It should be noted that the following embodiments are illustrative of the present invention and are not intended to limit the present invention. In addition, various modifications can be made to the present invention without departing from its essential points.
[0044] (electrode)
[0045] In this embodiment, the first feature of the electrode is that it has at least a substrate.
[0046] The substrate is preferably conductive. Examples of conductive substrate materials include nickel, materials with nickel as the main component, titanium, GC (glassy carbon), tantalum, zirconium, gold, platinum, palladium, etc. Examples of materials with nickel as the main component include nickel-based alloys such as Monel, Inconel, and Hastelloy.
[0047] From the perspective of heat resistance during the firing process in electrode preparation, the substrate material is more preferably metal. Furthermore, from the perspective of durability, conductivity, and economy, nickel or a material with nickel as the main component is more preferably nickel, as it is a metal that does not dissolve even at the oxygen evolution potential in alkaline aqueous solution and can be obtained at a lower cost compared to precious metals.
[0048] The conductive substrate used as the electrode can be flat or a porous plate with numerous pores. Specific shapes of the porous body include metal mesh, perforated metal, woven mesh, foamed metal, or similar shapes. Among these, metal mesh is preferred. While there are no particular limitations on size, to increase the electrolytic surface area for increasing gas generation, effectively remove gas generated through electrolysis from the electrode surface, and from a mechanical strength perspective, it is preferable that the center-to-center distance (SW) in the short grid direction of the mesh is 2 mm to 5 mm, the center-to-center distance (LW) in the long grid direction is 3 mm to 10 mm, the thickness is 0.2 mm to 2 mm, and the opening ratio is 20% to 80%. More preferably, SW is 3 mm to 4 mm, LW is 4 mm to 6 mm, the thickness is 0.8 mm to 1.5 mm, and the opening ratio is 40% to 60%.
[0049] The second feature of this embodiment is that it has LaNi x M y O 3-z (x+y is 0.8 to 1.2, y is 0.001 to 0.6, z is -0.5 to 0.5, and M contains at least one of Nb, Ta, Sb, Ti, Mn, or Zr). LaNi x M y O 3-z LaNi can be directly deposited on a substrate to form LaNi x M y O 3-z Layer, can also be formed between the substrate and LaNi x M y O 3-z Interfaces are formed between layers. M can contain two or more of Nb, Ta, Sb, Ti, Mn, and Zr.
[0050] In this embodiment, as a perovskite-type metal oxide, high oxygen evolution capacity can be achieved by configuring Ni at at least a portion of the B-site. Furthermore, if M (M includes at least one of Nb, Ta, Sb, Ti, Mn, and Zr) is configured together with Ni at the B-site, a low oxygen overvoltage can be imparted even after long-term energization, and high-temperature alkali resistance can be provided, which is therefore preferred. In particular, when Nb and Ni are configured together at the B-site, a low oxygen evolution overvoltage can be imparted when using an electrolyte with a high alkali concentration, which is also preferred. As for M, Nb, Ta, Sb, Ti, and Zr are preferred from the perspective of imparting high-temperature alkali resistance with a small amount; Ta, Sb, and Ti are further preferred from the perspective of excellent high-temperature alkali resistance; and Nb is most preferred from the perspective of balancing high-temperature alkali resistance and overvoltage with a further small amount.
[0051] Regarding x+y, from the perspectives of imparting a low oxygen overvoltage even after long-term energization, high-temperature alkali resistance, and low oxygen evolution overvoltage when using electrolytes with high alkali concentrations, the value is 0.8 or more and 1.2 or less. Preferably, it is 0.8 or more and 1.1 or less. From the perspectives of balancing high-temperature alkali resistance and overvoltage, it is more preferably 0.8 or more and 1.05 or less, further preferably 0.9 or more and 1.05 or less, and most preferably 1.0 or more and 1.05 or less.
[0052] Regarding y, from the perspective of high-temperature alkali resistance, it is 0.001 or more and 0.6 or less. From the perspective of balancing high-temperature alkali resistance and overvoltage, it is preferably 0.002 or more and less than 0.2, more preferably 0.005 or more and 0.15 or less, and even more preferably 0.01 or more and 0.1 or less.
[0053] z is between -0.5 and 0.5. In this invention, La is assumed to be trivalent, Ni is assumed to be trivalent, Nb (as M) is assumed to be pentavalent, Ta is assumed to be pentavalent, Sb is assumed to be pentavalent, Ti is assumed to be quadratic, Mn is assumed to be trivalent, Zr is assumed to be quadratic, and O is assumed to be -2 valence. z is calculated based on the composition ratio of O, which is 3-z. This composition ratio of O is calculated by balancing the valences of the matching composition formula. For example, in the composition formula LaNi... x Nb y O 3-z If x = 0.8 and y = 0.2, then according to the relationship 3 - z = (3 + 3 × 0.8 + 5 × 0.2) / 2, we can find z = -0.2.
[0054] LaNi on the substrate x M y O 3-z(where x+y is 0.8 to 1.2, y is 0.001 to 0.6, z is -0.5 to 0.5, and M contains at least one of Nb, Ta, Sb, Ti, Mn, or Zr) can be confirmed, for example, by the following known method: peeling off LaNi from the substrate. x M y O 3-z The layer, dissolved in acids such as aqua regia, was subjected to compositional analysis using ICP-AES (inductively coupled plasma optical emission spectrometry); the LaNi on the exfoliated substrate was analyzed. x M y O 3-z Layer, compositional analysis using a fluorescence X-ray analysis device; LaNi layer of electrode cross-section. x M y O 3-z Perform SEM-EDX analysis on the layers; and so on.
[0055] The third feature of this embodiment is that the initial double-layer capacitance is greater than 0.6 F / cm. 2 .
[0056] In this specification, double-layer capacitance refers to the double-layer capacitance calculated as follows: AC impedance is measured using a three-electrode electrochemical cell with a Luggin tube, and a Cole-Cole curve is obtained by plotting the real and imaginary parts. The double-layer capacitance is then calculated by analyzing the equivalent circuit fitting.
[0057] The specific method for calculating double-layer capacitance is described in the embodiments below. It should be noted that in this embodiment, the area (cm²) used in the double-layer capacitance calculation... 2 The area is the geometric area of the electrode. For example, if an electrode with a metal mesh substrate is cut into a square that is 2cm long and 2cm wide when viewed from the thickness direction, its area is 2×2=4cm². 2 .
[0058] The inventors have discovered that for substrates containing LaNi x M y O 3-z (x+y is 0.8 to 1.2, y is 0.001 to 0.6, z is -0.5 to 0.5, and M must contain at least one of Nb, Ta, Sb, Ti, Mn, or Zr), and the initial double-layer capacitance is greater than 0.6 F / cm. 2 The electrode exhibits a surprisingly low oxygen overvoltage even after prolonged energization. The reason for this is not yet clear, but it can be attributed to the increased chemical stability and large double-layer capacitance resulting from the addition of element M, which allows the LaNi electrode to withstand higher oxygen overvoltages. x M y O3-z The current density of the catalyst, based on surface area, is suppressed to a very low level, which reduces the stress on the catalyst surface even during long-term energization, thereby reducing the oxygen overvoltage even after long-term energization.
[0059] From the perspective of imparting a low oxygen overvoltage even after prolonged energization, the initial double-layer capacitance is greater than 0.6 F / cm. 2 The preferred value is 1.0 F / cm. 2 The above, and more preferably 1.5F / cm 2 The above, and more preferably, is 1.9F / cm 2 The above, and the optimal value, is 2.5F / cm. 2 That's all. The initial double-layer capacitance was greater than 0.6 F / cm. 2 Under these conditions, even after prolonged energization, the oxygen overvoltage will decrease.
[0060] In addition, the initial double-layer capacitor is preferably 7.0 F / cm. 2 The following, and more preferably, is 6.8F / cm. 2 The following, and more preferably, is 6.4F / cm. 2 The following, and even more preferably, is 6.3F / cm. 2 The following, the optimal value is 6.0F / cm 2 Below. If the initial double-layer capacitance is 7.0 F / cm. 2 As the amount of catalyst attached increases, the double-layer capacitance increases, and even after long-term energization, the oxygen overvoltage tends to decrease.
[0061] In the electrodes of this embodiment, every 1cm 2 The molar amount of La is preferably 0.06 mmol or more and 1.1 mmol or less, more preferably 0.13 mmol or more and 0.91 mmol or less, and even more preferably 0.15 mmol or more and 0.68 mmol or less. Per 1 cm 2 When the number of moles of La is within the above range, it tends to be easier to achieve an initial double-layer capacitance greater than 0.6 F / cm. 2 .
[0062] per 1cm 2 The number of moles of La is calculated as follows: LaNi on electrodes with a specified area x M y O 3-z The catalyst was dissolved in acid, and the concentration of La in the solution was determined by ICP-AES. The mass of La contained on the electrode was calculated, and this mass was divided by the atomic weight of La, 138.9, to calculate the molar number. This molar number was then divided by the area of the electrode to determine the molar number per 1 cm². 2The number of moles of La. It should be noted that the area (cm²) used in the calculation... 2 The area is the geometric area of the electrode. For example, if an electrode with a metal mesh substrate is cut into a square that is 2cm long and 2cm wide when viewed from the thickness direction, its area is 4cm². 2 The specific calculation method is explained in the examples.
[0063] In the electrode of this embodiment, the electrostatic capacitance per 1 mmol of La is preferably 10 F to 25 F, more preferably 12 F to 23 F, and even more preferably 14 F to 21 F. When the electrostatic capacitance per 1 mmol of La is within the above range, there is a tendency to achieve a lower oxygen overvoltage with a smaller amount of catalyst. When the electrostatic capacitance per 1 mmol of La is 10 F or more, there is a tendency for the oxygen overvoltage per unit amount of catalyst to decrease. When the electrostatic capacitance per 1 mmol of La is 25 F or less, the double-layer capacitance does not decrease even after long-term energization, and there is a tendency for the oxygen overvoltage to decrease.
[0064] The electrostatic capacitance per 1 mmol of La is obtained by dividing the double-layer capacitance by the capacitance per 1 cm. 2 The molar number (mmol) of La is used to determine this.
[0065] In this embodiment, LaNi x M y O 3-z The adhesion amount relative to the substrate is preferably greater than 145 g / m². 2 And it is 3500g / m 2 The following, or more preferably, is 200g / m 2 Above 3000g / m 2 The following, and more preferably, is 350g / m 2 Above 2500g / m 2 Below. If LaNi x M y O 3-z The adhesion amount is greater than 145g / m 2 This indicates a tendency for the oxygen overvoltage to decrease further after prolonged energization. Additionally, if LaNi... x M y O 3-z The adhesion amount is 3500g / m 2 Therefore, as the amount of catalyst attached increases, the double-layer capacitance increases, and the oxygen overvoltage tends to decrease even after long-term energization. The area (m²) used in the attachment amount calculation... 2) represents the geometric area of the electrode. For example, for an electrode using a metal mesh as its substrate, if the substrate is cut into a square measuring 10cm (0.1m) long and 10cm (0.1m) wide when viewed from the thickness direction, its area is 0.01m². 2 In making 1g of LaNi x M y O 3-z When adhered to this substrate, the adhesion amount is 100g / m². 2 .
[0066] It should be noted that the adhesion amount can be calculated as follows: The LaNi is completely peeled off from an electrode of a certain area. x M y O 3-z After catalyst removal, metallic powders such as Ni from the substrate are removed from the powder obtained through exfoliation using a magnet, resulting in the attached LaNi. x M y O 3-z The mass of the catalyst powder is weighed using an electronic balance and calculated. This mass is then divided by the value of a certain area of the electrode to determine the amount of adhesion.
[0067] LaNi stripping from the electrode x M y O 3-z Catalyst removal methods can employ various techniques that allow for the removal of foreign matter that cannot be removed with a magnet without introducing it. These techniques include filing with precision files or ultra-fine files; scraping with micro-scrapers or scrapers; and brushing with wire brushes.
[0068] In this embodiment, LaNi x M y O 3-z The preferred position of the main peak in XRD, 2θ, is above 32.6° and below 33.2°.
[0069] In this embodiment, LaNi x M y O 3-z The position of the main XRD peak shifts with the electrode. When using the Kα1 line of Cu as the XRD source to measure the XRD (X-ray diffraction) of the electrode, the position of the main peak of the (104) plane of LaNiO3 on the PDF01-070-5757 card (card) is taken as a reference, and the peaks near 2θ = 32.5° to 33.2° are taken as the main peaks of LaNiO3. x M y O 3-z The main peak location.
[0070] About LaNi x My O 3-z The main peak position was calculated by shifting the XRD spectrum using the "X-axis offset" tool, based on the main peak position of NiO near 2θ=43.276°, where 2θ is the 2θ=43.276° of the (200) plane of NiO in the PDF00-047-1049 card data.
[0071] From the perspective of high-temperature alkali resistance, LaNi x M y O 3-z The preferred position of the main peak in XRD, 2θ, is above 32.6° and below 33.2°.
[0072] The inventors have discovered that for LaNiO3, a specified amount of Ni is replaced with element M, or a specified amount of element M is added to LaNiO3 to form LaNiO3, the method is more efficient. x M y O 3-z LaNi was prepared by controlling the position of its main XRD peak 2θ to be above 32.6° and below 33.2°. x M y O 3-z Surprisingly, it exhibits a tendency to show high durability against high-temperature alkalis. The reason for this is not yet clear, but it can be attributed to the fact that by making LaNi... x M y O 3-z The XRD main peak position 2θ is above 32.6° to 33.2°, indicating that it is a high-temperature alkali reacting with LaNi. x M y O 3-z The concentration of oxygen vacancies at the reaction site decreases, and by adding element M, LaNi in a high-temperature alkali environment... x M y O 3-z The generation of oxygen defects in the oxygen was suppressed.
[0073] From the perspective of excellent durability against high-temperature alkali, it is more preferable to have a temperature of 32.7°C or higher and 33.2°C or lower. From the perspective of balancing durability against high-temperature alkali and overvoltage, it is even more preferable to have a temperature of 32.75°C or higher and 33.2°C or lower. Most preferably, it is preferable to have a temperature of 32.8°C or higher and 33.2°C or lower.
[0074] In this embodiment, from the perspective of durability against high-temperature alkali, LaNi x M y O 3-z The preferred half-width of the XRD main peak is between 0.6° and 0.85°. The half-width of the main peak refers to the half-width calculated by taking the range of 2θ between 31° and 35° as the peak.
[0075] LaNi x M y O 3-z The half-peak width of the XRD main peak is more preferably 0.6° or more and 0.8° or less. From the perspective of balancing durability against high-temperature alkali and overvoltage, it is further preferred to be 0.6° or more and 0.75° or less.
[0076] In this embodiment, from the perspective of durability against high-temperature alkali, LaNi x M y O 3-z The XRD peak intensity is preferably between 6,000 and 100,000. Peak intensity refers to the intensity obtained by subtracting the baseline intensity from the measured intensity (Counts) of the peak position of the peak measured using the D8 ADVANCE XRD apparatus (sold by Bruker Japan Co., Ltd.). The measurement conditions are described in the examples below.
[0077] LaNi x M y O 3-z The XRD main peak intensity is more preferably 6,500 to 50,000, further preferably 7,000 to 20,000, and most preferably 7,000 to 17,000, taking into account both durability against high-temperature alkali and overvoltage.
[0078] In this embodiment, in LaNi x M y O 3-z A 20μm square region in the layer, larger than 0.785μm. 2 And it is 20μm 2 The sum of the following pore areas is preferably 10 μm. 2 Above 200μm 2 the following.
[0079] When the pore is perfectly circular, the area of a perfectly circular pore with a diameter of 1 μm is 0.5 × 0.5 × π ≒ 0.785 (μm). 2 Furthermore, the area of a perfectly circular pore with a diameter of 5 μm is 2.5 × 2.5 × π ≒ 20 (μm). 2 Area greater than 0.785μm 2 And it is 20μm 2 The total area of the following pores is 10 μm. 2 Above 200μm 2 The following range indicates that, when the pores are perfectly circular, pores with a diameter greater than 1 μm and less than 5 μm exist within a certain area range in the cross-section of the catalyst layer.
[0080] In this embodiment, greater than 0.785μm 2 And it is 20μm 2 The total area of the pores was calculated as follows: A small electrode piece was embedded in epoxy resin. A cross-section of the sample was then prepared by cutting and grinding. The sample was observed using an electron microscope at 500x magnification. From the obtained reflected electron image, image processing software was used to binarize and extract the pores, setting the area to a 20μm square region and cutting it out. Image processing was performed on the cut-out image to binarize and extract the pores, calculating the area of each pore. The area of pores larger than 0.785μm was then calculated. 2 And it is 20μm 2 The sum of the following pore areas is calculated accordingly. A 20 μm square region extracted from the cross-sectional photograph by binarizing the pores is defined such that it does not contain any cracks on the outer surface or leading to the outer surface. When processing the image, appropriate filtering is preferably performed to remove noise. Specific methods for image processing are described in the examples below.
[0081] The inventors have discovered that the following electrode, when used with an electrolyte of high alkalinity, surprisingly exhibits a tendency for low overvoltage; this electrode has a LaNi substrate. x M y O 3-z (x+y is 0.8 to 1.2, y is 0.001 to 0.6, z is -0.5 to 0.5, and M contains at least one of Nb, Ta, Sb, Ti, Mn, or Zr), in LaNi x M y O 3-z A 20μm square region within the layer is larger than 0.785μm. 2 And it is 20μm 2 The total area of the following pores is 10 μm. 2 Above 200μm 2 The reason is not yet clear, but it can be considered that it is due to the area being greater than 0.785μm. 2 And it is 20μm 2 The total area of the following pores is 10 μm. 2 Above 200μm 2 Under the following conditions, even when using electrolytes with high alkalinity, the decrease in diffusion rate within the electrode caused by the viscosity of the electrolyte can be suppressed, and sufficient stability can be maintained with electrolytes with high alkalinity.
[0082] From the perspective of imparting a lower oxygen evolution overvoltage when using an electrolyte with a high alkalinity concentration, greater than 0.785 μm 2 And it is 20μm 2The sum of the following pore areas is more preferably 20 μm. 2 Above 160μm 2 The following, and more preferably 30μm 2 Above 130μm 2 the following.
[0083] In this embodiment, from the perspective of imparting a low oxygen evolution overvoltage when using an electrolyte with a high alkali concentration, the above-mentioned LaNi is preferred. x M y O 3-z The average pore area in a 20μm square region of the layer is greater than 0.785μm. 2 And it is 10μm 2 the following.
[0084] The average pore area is the average of the areas of each pore obtained by image processing software to perform image processing on the cut-out image and extracting the pores through binarization. The specific calculation method is described in the examples below.
[0085] From the perspective that a lower oxygen evolution overvoltage can be imparted when using an electrolyte with a high alkalinity concentration, LaNi x M y O 3-z The average pore area of the layer is more preferably 1.2 μm. 2 Above 6.8μm 2 The following, and more preferably, is 3.2μm 2 Above 4.5μm 2 the following.
[0086] In this embodiment, from the perspective of imparting a lower oxygen evolution overvoltage when using an electrolyte with a high alkali concentration, the above-mentioned LaNi is preferred. x M y O 3-z The average number of pores in a 20μm square region of the layer is more than 20 and less than 150.
[0087] The specific method for calculating the average number of pores is described in the examples below.
[0088] From the perspective of imparting a lower oxygen evolution overvoltage when using an electrolyte with a high alkalinity concentration, the average number of pores is more preferably 22 or more and 140 or less, further preferably 29 or more and 140 or less, and most preferably 29 or more and 51 or less.
[0089] In this embodiment, from the perspective of imparting a low oxygen evolution overvoltage when using an electrolyte with a high alkali concentration, the above-mentioned LaNi is preferred. x M y O 3-zThe porosity in a 20μm square region of the layer is greater than 29% and less than 55%.
[0090] The specific method for calculating porosity is described in the examples below.
[0091] The porosity is more preferably 41% or more and 55% or less, further preferably 42% or more and 55% or less, and most preferably 45% or more and 55% or less.
[0092] The electrode of this embodiment can be used as an anode for water electrolysis, and an electrolysis unit for water electrolysis using the electrode of this embodiment as an anode, as well as a method for producing hydrogen using the anode for water electrolysis, can be provided. Water containing alkali can be used in water electrolysis.
[0093] (Electrode preparation method)
[0094] The electrode of this embodiment can be prepared as follows: an aqueous solution (coating solution) containing metal salts of La, Ni, and M (M at least includes any one of Nb, Ta, Sb, Ti, Mn, and Zr) is coated onto a substrate, dried, and pre-fired to form a LaNi electrode of a specified mass on the substrate. x M y O 3-z The precursor is then subjected to a primary calcination process to prepare the electrode.
[0095] As metal salts, water-soluble salts such as nitrates, hydroxynitrates, chlorides, oxalates, tartrates, acetates, and sulfates can be used. Metal salts can be anhydrous or hydrated.
[0096] For La, Ni, and M, aqueous sols of oxides or hydroxides can also be used instead of metal salts.
[0097] When using Nb as M, niobium oxalate or ammonium niobium oxalate is preferred from a solubility perspective. Conversely, when using Sb as M, antimony tartrate is preferred.
[0098] LaNi exhibits low oxygen overvoltage and is easily prepared. x M y O 3-z In terms of ease of preparation and high durability against high-temperature alkalis, LaNi is readily available. x M y O 3-z In terms of its properties, and the ease of preparation of LaNi, which exhibits lower oxygen evolution overvoltage even when using electrolytes with high alkalinity concentrations. x M y O 3-z From this perspective, it is preferable to add organic ligands such as glycine and other amino acids, oxalic acid, tartaric acid and other carboxylic acids to the coating solution.
[0099] In particular, if a coating solution containing glycine and metal nitrates is used, it is easy to prepare an electrode that exhibits a lower oxygen overvoltage, an electrode that can balance durability and overvoltage against high-temperature alkali, and an electrode that exhibits a lower oxygen evolution overvoltage when using an electrolyte with a high alkali concentration. Therefore, glycine is a preferred organic ligand.
[0100] The electrode preparation in this embodiment includes the preparation of glycine / NO3. - A firing process involving a mixture of La(NO3)3, Ni(NO3)2, and glycine in a molar ratio of 0.1 to 0.3 easily produces an initial double-layer capacitance greater than 0.6 F / cm. 2 The electrode is preferred. For glycine / NO3 - The process of calcining a mixture of La(NO3)3, Ni(NO3)2, and glycine with a molar ratio of 0.1 to 0.3 is as follows: La(NO3)3·6H2O, Ni(NO3)2·6H2O, and glycine are prepared according to the ratio of glycine to NO3... - The mixture is prepared in a molar ratio of 0.1 to 0.3, and the resulting aqueous solution is coated onto a substrate, dried, and then fired. This process is performed. If glycine / NO3 - If the molar ratio is less than 0.1, secondary crystals composed of La and Ni, outside the perovskite crystalline phase, will be obtained, and the oxygen overvoltage may not decrease. When the molar ratio is below 0.3, it can reduce the bilayer capacitance during the initial preparation stage by more than 0.6 F / cm. 2 The tendency of the electrode to be coated a certain number of times is preferred.
[0101] In the preparation of the electrode in this embodiment, from the perspective of increasing the electrostatic capacitance per 1 mmol of La, it is more preferable to include the preparation of the electrode with respect to glycine / NO3. - The process involves firing a mixture of La(NO3)3, Ni(NO3)2, and glycine in a molar ratio of 0.1 to 0.25.
[0102] In the electrode fabrication of this embodiment, the amount of gas generated due to glycine decomposition during firing is reduced, and the initial double-layer capacitance of greater than 0.6 F / cm can be prepared with fewer coating passes. 2 From the perspective of the electrode, further optimization includes the addition of a component for glycine / NO3. - The process involves firing a mixture of La(NO3)3, Ni(NO3)2, and glycine in a molar ratio of 0.1 to 0.2.
[0103] In this embodiment, the electrode preparation includes a process of calcining a mixture of La(NO3)3, Ni(NO3)2, and compounds containing carboxyl and amino groups and with C, H, N, and O as constituent elements, such as amino acids like glycine and aspartic acid, dipeptides like carnosine, and polypeptides like polylysine. The combustion byproducts (CO2, H2O, and N2) generated during calcination, relative to the LaNi... x M y O 3-z molar ratio (combustion byproducts / LaNi) x M y O 3-z Preferably, the ratio is 5 or higher and less than 12.6. If the combustion byproduct gas / LaNi x M y O 3-z When the molar ratio is 5 or higher, the electrode deposits are not easily dissolved or detached when the aqueous solution of the mixture is used as the coating solution for coating, drying, and firing. There is a tendency to increase the electrode deposits through repeated coating, drying, and firing processes. Additionally, if the combustion byproduct gas / LaNi x M y O 3-z If the molar ratio is less than 12.6, when the aqueous solution of the mixture is used as the coating liquid for coating, drying and firing, the amount of adhesion in one coating-drying-firing process may increase, and there is a tendency to easily prepare electrodes with high adhesion by fewer coating-drying-firing processes.
[0104] Combustion byproduct gas / LaNi x M y O 3-z The specific method for calculating the molar ratio is described in the examples below.
[0105] It should be noted that the amount of combustion byproduct gases (CO2, H2O, and N2) produced can be determined by thoroughly drying the coating solution at 100°C and then placing the resulting product in an organic elemental analyzer such as the Flash2000 manufactured by Thermo Fisher Scientific. Regarding LaNi... x M y O 3-z The amount produced can be calculated from the mass of the powder produced by thoroughly drying the coating solution at 100°C and firing the resulting product under specified firing conditions. Therefore, the amount of combustion byproduct gases (CO2, H2O, and N2) produced, as determined by measurement, and the LaNi... x M y O 3-z The combustion byproduct gas / LaNi was calculated based on the amount generated.x M y O 3-z Molar ratio.
[0106] The concentration of aqueous solutions containing metal salts of La, Ni, and M is expressed in terms of LaNi. x M y O 3-z The reference molality is preferably 0.1 mol / kg solvent or more and 4.0 mol / kg solvent or less. When the solvent concentration is 0.1 mol / kg or more, an electrode with a specified adhesion amount can be prepared with fewer coating and firing cycles, which is preferable from a productivity perspective. When the solvent concentration is 4.0 mol / kg or less, the dissolution of metal salts and organic ligands becomes easier, which is preferable from a coating solution productivity perspective. More preferably, it is 0.2 mol / kg solvent or more and 2.0 mol / kg solvent or less; even more preferably, it is 0.3 mol / kg solvent or more and 2.0 mol / kg solvent or less; even more preferably, it is 0.35 mol / kg solvent or more and 2.0 mol / kg solvent or less; and even more preferably, it is 0.4 mol / kg solvent or more and 1.0 mol / kg solvent or less.
[0107] In addition, especially in LaNi x M y O 3-z When M is Nb, the concentration of the aqueous solution containing metal salts of La, Ni, and Nb is expressed as LaNi x Nb y O 3-z The preferred gravimetric concentration for the reference is 0.3 mol / kg solvent or higher and 4.0 mol / kg solvent or lower. When the concentration is 0.3 mol / kg solvent or higher, it is easy to obtain a concentration greater than 0.785 μm. 2 And it is 20μm 2 The total area of the following pores is 10 μm. 2 Above 200μm 2 The following applies. When the solvent concentration is 4.0 mol / kg or less, the dissolution of metal salts and organic ligands becomes easier, which is preferred from the perspective of coating solution productivity. More preferably, the solvent concentration is 0.35 mol / kg or more to 2.0 mol / kg or less, and even more preferably, 0.4 mol / kg or more to 1.0 mol / kg or less.
[0108] The preferred drying temperature after applying the coating liquid to the substrate is 50°C to 200°C. At 50°C or higher, drying is completed within 3 minutes to 1 hour, which is preferable from a productivity perspective. At 200°C or lower, the cooling time of the substrate after drying is shortened, which is also preferable from a productivity perspective.
[0109] Spraying is the preferred coating method for applying a coating liquid to a substrate. In particular, when the atomized coating liquid is moderately dried and made more viscous before falling onto the substrate from the nozzle, the coating liquid film does not move on the substrate after landing, and a uniform film thickness can be formed on the substrate. This makes it easy to prepare electrodes that exhibit low oxygen overvoltage even after long-term energization.
[0110] Furthermore, as a coating method that involves applying the coating solution directly to the substrate, immersion coating, in which the substrate is completely immersed in the coating solution, is also a preferred method. When using immersion coating, it is easy to achieve a thickness greater than 0.785 μm by controlling the concentration of the coating solution. 2 And it is 20μm 2 The total area of the following pores is 10 μm. 2 Above 200μm 2 the following.
[0111] When the substrate is immersed in the coating solution, it can be completely immersed without adhering to air bubbles by slowly lowering it with the substrate facing at an angle. Furthermore, the voids within the metal oxide layer (pre-fired body layer) formed on the substrate surface can be completely replaced by the coating solution, thus enabling reproducible coating for substrates larger than 0.785 μm. 2 And it is 20μm 2 Controlling the total area of the pores below is preferred.
[0112] The preferred temperature for pre-firing the dried substrate is between 300°C and 500°C. If the temperature is above 300°C, pre-firing can be completed within 3 minutes to 1 hour, which is preferable from a productivity perspective. If the temperature is below 500°C, the cooling time of the dried substrate is shortened, which is also preferable from a productivity perspective.
[0113] In order to prepare the desired LaNi x M y O 3-z The electrode coating, drying, and pre-firing processes can be repeated. Each coating, drying, and pre-firing process results in an adhesion amount of 10 g / m². 2 Above 50g / m 2 The following approach reduces the number of coating passes, which is preferable from a productivity perspective. Furthermore, the adhesion weight per coating, drying, and pre-firing pass is 10 g / m². 2 Above 20g / m 2 Below this, it is easy to make it larger than 0.785μm. 2 And it is 20μm 2 The total area of the following pores is 10 μm. 2 Above 20μm 2 The following are preferred options.
[0114] Regarding the main firing temperature, firing can be performed between 500°C and 1000°C, preferably above 650°C. Firing at 650°C or above allows for the fabrication of electrodes exhibiting low oxygen overvoltage within a firing time of 10 minutes to 24 hours, which is preferable from a productivity standpoint. Furthermore, firing at 800°C or above allows for the fabrication of electrodes conforming to the LaNi alloy within a firing time of 10 minutes to 24 hours. x M y O 3-z The XRD peak position 2θ is controlled to be 32.6° to 33.2°, and the electrode exhibits high durability against high-temperature alkalis. From a productivity perspective, firing at 800°C or higher is more preferable. Furthermore, firing at 750°C or higher allows for the preparation of electrodes exhibiting lower oxygen evolution overvoltages when using electrolytes with high alkali concentrations, within a firing time of 10 minutes to 24 hours. Therefore, from a productivity perspective, firing at 750°C or higher is more preferable.
[0115] M can be added by coating, drying, pre-firing, and main firing using the following key points: pre-coating a coating solution containing an aqueous dispersible sol, which is an aqueous dispersible sol of a metal salt or oxide or hydroxide of La or Ni; after drying and pre-firing, top-coating the electrode with a coating solution containing an aqueous dispersible sol, which is an aqueous dispersible sol of a metal salt or oxide or hydroxide of M.
[0116] Alternatively, M can be added by coating, drying, pre-firing, and main firing using the following key points: pre-coating a coating solution containing an aqueous dispersible sol, which is an aqueous dispersible sol of a metal salt, oxide, or hydroxide of La or Ni; after drying, pre-firing, and main firing, top-coating the electrode with a coating solution containing an aqueous dispersible sol, which is an aqueous dispersible sol of a metal salt, oxide, or hydroxide of M.
[0117] (Electrolytic cell)
[0118] Figure 1 The image shows an overall side view of an example of an electrolytic cell, which includes an electrolysis unit having the electrodes of this embodiment as anodes.
[0119] Figure 2 A cross-sectional view of an example zero-pole structure of an electrolytic cell is shown in the figure. Figure 1 (The cross-sectional view of the electrolysis unit inside the dashed square shown) The electrolysis cell includes an electrolysis unit having the electrode of this embodiment as the anode.
[0120] The bipolar electrolytic cell 50 of this embodiment (refer to...) Figure 3 In this structure, the diaphragm 4 contacts the anode 2a and the cathode 2c to form a zero-gap structure Z (refer to...). Figure 2 ).
[0121] It should be noted that, Figure 3 The diagram shows an outline of the electrolysis apparatus used in the embodiments and comparative examples. Figure 4 The diagram shows an outline of the bipolar electrolyzer used in the electrolysis test.
[0122] (element)
[0123] like Figure 1 As shown, in the bipolar electrolytic cell 50, the bipolar element 60 is disposed between the anode terminal element 51a and the cathode terminal element 51c, and the diaphragm 4 is disposed between the anode terminal element 51a and the bipolar element 60, between adjacent bipolar elements 60, and between the bipolar element 60 and the cathode terminal element 51c.
[0124] In this embodiment, the portion between the partition walls 1 of two adjacent bipolar elements 60 in the bipolar electrolytic cell 50, and the portion between the partition walls 1 of adjacent bipolar elements 60 and terminal elements are specifically referred to as electrolysis unit 65. Electrolysis unit 65 includes partition walls 1, anode chamber 5a, anode 2a and diaphragm 4 of one element, and cathode 2c, cathode chamber 5c and partition walls 1 of another element.
[0125] (Electrode chamber)
[0126] In the bipolar electrolytic cell 50 of this embodiment, such as Figure 2 As shown, the electrode chamber 5 through which the electrolyte passes is defined by the partition wall 1, the outer frame 3, and the diaphragm 4. Here, the electrode chamber 5 on the anode side sandwiched by the partition wall 1 is the anode chamber 5a, and the electrode chamber 5 on the cathode side is the cathode chamber 5c.
[0127] In this embodiment, the configuration of the main pipe for the bipolar electrolyzer can be either an internal main pipe type or an external main pipe type, and the space occupied by the anode and cathode themselves can also be located inside the electrode chamber. Furthermore, especially when a gas-liquid separator is provided, the space occupied by the gas-liquid separator can also be located inside the electrode chamber.
[0128] (rib material)
[0129] In the bipolar electrolysis unit 65 for alkaline water electrolysis of this embodiment, it is preferable to physically connect the rib 6 to the electrode 2. With this configuration, the rib 6 becomes a support for the electrode 2, easily maintaining the zero-gap structure Z. Furthermore, the rib 6 is preferably electrically connected to the partition wall 1. Additionally, by providing the rib 6, convection generated in the electrode chamber 5 due to turbulence of the gas-liquid flow can be reduced, suppressing localized increases in electrolyte temperature.
[0130] Here, the electrode can be placed on the rib, or the current collector, conductive elastomer, and electrode can be placed on the rib in sequence.
[0131] In the above example of a bipolar electrolysis unit for alkaline water electrolysis, the cathode chamber adopts a structure in which cathode ribs, cathode current collectors, conductive elastomers, and cathodes are stacked in sequence, and the anode chamber adopts a structure in which anode ribs and anodes are stacked in sequence.
[0132] It should be noted that in the above example of the bipolar electrolysis unit for alkaline water electrolysis, the above-mentioned "cathode rib - cathode current collector - conductive elastomer - cathode" structure is used in the cathode chamber, and the above-mentioned "anode rib - anode" structure is used in the anode chamber. However, this invention is not limited to this, and the "anode rib - anode current collector - conductive elastomer - anode" structure can also be used in the anode chamber.
[0133] In detail, in the bipolar electrolysis unit for alkaline water electrolysis of this embodiment, such as Figure 2 As shown, preferably, ribs 6 (anode ribs and cathode ribs) are installed in the partition wall 1.
[0134] In the ribs (anode ribs, cathode ribs), it is preferable that they not only have the function of supporting the anode or cathode, but also have the function of transferring current from the partition to the anode or cathode.
[0135] In the bipolar electrolysis unit for alkaline water electrolysis of this embodiment, it is preferable that at least a portion of the ribs is conductive, and more preferably that the entire rib is conductive. With this configuration, the rise in unit voltage caused by electrode deflection can be suppressed.
[0136] The material used for the ribs is typically a conductive metal. Examples include mild steel plated with nickel, stainless steel, and nickel. The material of the ribs is particularly preferred to be the same as that of the partition walls, and nickel is especially preferred.
[0137] The spacing between adjacent anode ribs or adjacent cathode ribs can be determined by considering factors such as electrolytic pressure and the pressure difference between the anode and cathode chambers.
[0138] If the spacing between the anode ribs or the spacing between adjacent cathode ribs is too narrow, it will not only hinder the flow of electrolyte and gas, but also increase costs. If the rib spacing is 10 mm or more, gas discharge from the back of the electrode is good. On the other hand, if the spacing is too wide, the electrodes (anode and cathode) held by the small pressure difference between the anode and cathode chambers will deform, or the number of anode or cathode ribs will decrease, resulting in increased resistance. If the rib spacing is 150 mm or less, the electrode is less prone to bending. The number of ribs, the length of the ribs, the angle between the ribs and the partition wall, the number of through holes, and the spacing of the through holes along the given direction of the partition wall can be suitably set as long as the effects of the present invention are achieved. The ribs are preferably arranged parallel to the direction given by the partition wall (for example, it can be a vertical direction; if the shape of the partition wall is approximately rectangular when viewed from above, it can be in the same direction as one of the two sets of opposite sides). The rib spacing of the anode ribs and the rib spacing of the cathode ribs can be the same or different. Preferably, the rib spacing of both the anode ribs and the cathode ribs meets the above-mentioned range.
[0139] For the installation of anode and cathode ribs in the partition, laser welding can be used.
[0140] In addition, regarding the thickness of the ribs, considering factors such as cost, manufacturability, and strength, ribs of 0.5mm to 5mm and 1mm to 2mm are easy to use, but there are no particular limitations.
[0141] Electrodes and current collectors are typically mounted on the ribs using spot welding, but other methods such as laser welding can also be used. Furthermore, methods involving the use of wire or rope-like components to create a tight seal can also be employed. The ribs, like the anode or cathode, are fixed to the partition wall using spot welding, laser welding, or similar methods.
[0142] (Methods for producing hydrogen)
[0143] Next, a method for producing hydrogen by alkaline water electrolysis using the bipolar electrolyzer of this embodiment will be described.
[0144] In this embodiment, water electrolysis is performed by applying an electric current to a bipolar electrolyzer equipped with an anode and cathode as described above, in which an electrolyte is circulated, thereby producing hydrogen at the cathode. At this time, a variable power source can be used, for example. A variable power source differs from a power source with a stable output, such as system power, and refers to a power source from a renewable energy power plant whose output varies in increments of seconds to minutes. The method of generating renewable energy is not particularly limited; examples include solar power generation and wind power generation.
[0145] For example, in the case of electrolysis using a bipolar electrolyzer, cationic electrolytes in the electrolyte move from the anode chamber of one element through a diaphragm to the cathode chamber of an adjacent element, while anionic electrolytes move from the cathode chamber of one element through a diaphragm to the anode chamber of an adjacent element. Thus, the current in the electrolysis flows along the direction of the series connection of the elements. That is, the current flows through the diaphragm from the anode chamber of one element to the cathode chamber of an adjacent element. During electrolysis, oxygen is generated in the anode chamber and hydrogen is generated in the cathode chamber.
[0146] The bipolar electrolysis unit 65 for alkaline water electrolysis of this embodiment can be used in bipolar electrolyzers 50, electrolysis apparatus 70 for alkaline water electrolysis, etc. Examples of the aforementioned electrolysis apparatus 70 for alkaline water electrolysis include the bipolar electrolyzer 50 of this embodiment, a liquid pump 71 for circulating the electrolyte, a gas-liquid separator 72 for separating the electrolyte from hydrogen and / or oxygen, and a water supply device for replenishing the water consumed during electrolysis.
[0147] The aforementioned electrolysis device for alkaline water electrolysis may further include a rectifier 74, an oxygen concentration meter 75, a hydrogen concentration meter 76, a flow meter 77, a pressure gauge 78, a heat exchanger 79, and a pressure control valve 80.
[0148] In the alkaline water electrolysis method using the above-mentioned alkaline water electrolysis apparatus, the preferred current density supplied to the electrolysis unit is 4 kA / m. 2 ~20kA / m 2 More preferably 6kA / m 2 ~15kA / m 2 .
[0149] Especially when using a variable power source, it is preferable to keep the upper limit of the current density within the aforementioned range.
[0150] The electrodes, electrolysis units, and hydrogen manufacturing methods of the present invention have been illustrated above with reference to the accompanying drawings. However, the electrodes, electrolysis units, and hydrogen manufacturing methods of the present invention are not limited to the above examples, and appropriate modifications can be made to the above embodiments.
[0151] Example
[0152] The present invention is illustrated in detail below by way of examples, but the present invention is not limited to these examples. Of course, various modifications can be made within the scope of the essential points of the present invention.
[0153] (Example A1)
[0154] As a porous nickel substrate, a nickel metal mesh with dimensions of SW3.0mm, LW4.5mm, thickness 1.2mm, aperture ratio 54%, length 10cm, width 10cm, and square 10cm was prepared. After sandblasting, the nickel metal mesh was acid-treated in hydrochloric acid at 50℃ and 6N for 6 hours, followed by washing and drying to serve as a coating substrate.
[0155] Dissolve 18.61g of Ni(NO3)2·6H2O, 34.64g of La(NO3)3·6H2O, and 8.29g of glycine in 200g of pure water, and transfer the solution to a square polyethylene container with a bottom edge of 6cm × 10cm and a height of 11cm, as solution A of Example A1.
[0156] Niobium oxalate ammonium was dissolved in pure water to prepare an aqueous solution of 200 g containing 80 mmol / kg Nb, which was used as solution B in Example A1. The concentration of Nb was confirmed using CP-AES (inductively coupled plasma optical emission spectrometry).
[0157] While stirring liquid A of Example A1 using a magnetic stirrer, liquid B of Example A1 was slowly mixed to form the coating liquid of Example A1.
[0158] While stirring the coating solution, the substrate is held vertically, with the lower half slowly immersed in the solution for 5 seconds. The substrate is then lifted, flipped over, and the upper half is also slowly immersed in the solution for 5 seconds. After the coating solution is applied to the entire surface of the substrate, it is placed horizontally and blown away excess solution using a blower-like air jet. It is then dried at 60°C for 10 minutes, followed by firing at 400°C for 10 minutes to form a metal oxide layer on the substrate surface.
[0159] The coating, drying, and firing cycle was repeated 60 times. A further firing at 750°C for 1 hour resulted in an adhesion of 502 g / m² on the coated substrate. 2 The metal oxide layer is used to obtain the electrode of Example A1.
[0160] (Example A2)
[0161] Prepare the coating substrate in the same manner as in Example A1.
[0162] Next, solution A (composition shown in Table 1) and solution B (composition shown in Table 2) were prepared. Solution B was prepared by adding pure water to Nb₂O₅ sol with a particle size of less than 5 nm. The concentration of Nb was confirmed by ICP-AES (inductively coupled plasma optical emission spectrometry).
[0163] Using a spraying device (rCoater sold by Asahi Sunac Co., Ltd.), liquid A is applied to both sides of the substrate, dried at 60°C for 10 minutes, and then fired at 400°C for 10 minutes to form a metal oxide layer on the substrate surface.
[0164] After repeating the coating, drying, and firing cycle of solution A six times, solution B was applied to both sides of the substrate using a spraying device, followed by drying at 60°C for 10 minutes. The mass increase of the substrate relative to before solution B coating was calculated to be 77 mg. Further firing at 400°C for 10 minutes resulted in the formation of a metal oxide layer on the substrate surface.
[0165] The coating, drying, and firing process was repeated 6 times with liquid A and 1 time with liquid B. This cycle was repeated 5 times, for a total of 30 coating, drying, and firing processes with liquid A and 5 times with liquid B.
[0166] Further firing at 650℃ for 1 hour resulted in an adhesion weight of 488g / m². 2 The metal oxide layer is used to obtain the electrode of Example A2.
[0167] Because the amount of metal oxide layer attached to the substrate is 4.88 g and 1 mole of LaNi 0.85 O 2.775 The mass of the coating is 233.1 g, and the mass of 1 mole of Nb₂O₅ is 265.8 g. Therefore, it can be concluded that by coating 385 mg of Nb₂O₅, a mass relative to 1 mole of LaNi was obtained. 0.85 O 2.775 A coating with Nb and a composition of LaNi was applied at a ratio of 0.15 mol / L. 0.85 Nb 0.15 O 3.15 The electrodes.
[0168] (Example A3)
[0169] The substrate for coating was prepared in the same manner as in Example A1. Next, liquid A and liquid B of Example A3, as shown in Tables 1 and 2, were prepared.
[0170] Similar to Example A2, after applying liquid A to both sides of the substrate, it was dried at 60°C for 10 minutes and then fired at 400°C for 10 minutes to form a metal oxide layer on the substrate surface.
[0171] After repeating the coating, drying, and firing cycle of solution A 25 times, solution B was applied to both sides of the substrate, followed by drying at 60°C for 10 minutes. The calculated mass increase of the substrate relative to its initial state was 14.6 mg. Further firing at 400°C for 10 minutes resulted in the formation of a metal oxide layer on the substrate surface.
[0172] Further firing at 700℃ for 1 hour resulted in an adhesion weight of 501g / m². 2 The metal oxide layer is used to obtain the electrode of Example A3.
[0173] Because the amount of metal oxide layer attached to the substrate is 5.01g, 1 mole of LaNi 0.795 O 2.6925 The mass of the sample is 228.6 g, and the mass of 1 mole of Nb₂O₅ is 265.8 g. Therefore, it can be concluded that by coating 14.6 mg of Nb₂O₅, a mass relative to 1 mole of LaNi was obtained. 0.795 O 2.6925 A coating of Nb with the composition LaNi was applied at a ratio of 0.005 mol. 0.795 Nb 0.005 O 2.705 The electrodes.
[0174] (Example A4)
[0175] Prepare the coating substrate in the same manner as in Example A1.
[0176] Dissolve 116.3g of Ni(NO3)2·6H2O, 173.2g of La(NO3)3·6H2O, and 16.52g of glycine in 200g of pure water to prepare solution A of Example A4.
[0177] Niobium oxalate ammonium was dissolved in pure water, and 30% hydrogen peroxide was added to prepare 200 g of an aqueous solution of hydrogen oxalate ammonium hydrogen peroxide with a Nb concentration of 20 mmol / kg and an H2O2 / Nb molar ratio of 2.5. This solution was used as solution B in Example A4. The concentration of Nb was confirmed by ICP-AES (inductively coupled plasma optical emission spectrometry).
[0178] Liquid A was fed at a rate of 0.64 mL / min and liquid B at a rate of 0.36 mL / min. Using a PEEK T-shaped reactor (sold by YMC Co., Ltd., Japan) with an inner diameter of 1 mm, liquids A and B were mixed immediately in front of the spraying device and supplied to the device at a rate of 1 mL / min. The mixture was then applied to both sides of the substrate using the spraying device, dried at 60°C for 10 minutes, and further fired at 400°C for 10 minutes to form a metal oxide layer on the substrate surface.
[0179] After repeating the coating, drying, and firing cycle of the mixture of liquid A and liquid B 13 times, it was further fired at 700℃ for 1 hour to form an adhesion weight of 506 g / m². 2 The metal oxide layer is used to obtain the electrode of Example A4.
[0180] Since the density of solution A is 1.45 g / cm³ 3 The density of solution B is 1 g / cm³.3 Solution A was mixed at a rate of 0.64 mL / min and solution B at a rate of 0.36 mL / min. Therefore, the mixture obtained by drying and calcining the mixture has a composition of LaNiNb. 0.01 O 3.025 .
[0181] (Example A5)
[0182] Prepare the coating substrate in the same manner as in Example A1. Next, prepare solution A and solution B of Example A5 as shown in Tables 1 and 2.
[0183] Similar to Example A2, liquid A was applied to both sides of the substrate, dried at 60°C for 10 minutes, and then fired at 400°C for 10 minutes to form a metal oxide layer on the substrate surface.
[0184] After repeating the coating, drying, and firing cycle of solution A 16 times, solution B was applied to both sides of the substrate, followed by drying at 60°C for 10 minutes. The mass increase of the substrate relative to its initial state was calculated to be 54 mg. Further firing at 400°C for 10 minutes resulted in the formation of a metal oxide layer on the substrate surface.
[0185] Further firing at 700℃ for 1 hour resulted in an adhesion weight of 505g / m². 2 The metal oxide layer is used to obtain the electrode of Example A5.
[0186] Since the amount of metal oxide layer attached to the substrate is 5.05 g, the mass of 1 mole of LaNiO3 is 245.5 g, and the mass of 1 mole of Nb2O5 is 265.8 g, it can be concluded that by coating 54 mg of Nb2O5, a coating of Nb with the composition LaNiNb is obtained at a ratio of 0.02 moles relative to 1 mole of LaNiO3. 0.02 O 3.05 The electrodes.
[0187] (Example A6)
[0188] Prepare the coating substrate in the same manner as in Example A1. Next, prepare solution A and solution B of Example A6 as shown in Tables 1 and 2.
[0189] Transfer liquid A into a polyethylene container with a bottom edge of 13cm × 13cm and a height of 10cm.
[0190] The substrate for coating is slowly immersed in solution A in a container at an angle, ensuring complete immersion for 5 seconds. The substrate is then lifted, placed horizontally, and the excess coating solution is blown away using a blower-based air jet. It is then dried at 60°C for 10 minutes, followed by firing at 400°C for 10 minutes to form a metal oxide layer on the substrate surface.
[0191] Repeat the coating, drying, and firing cycle 20 times. When placing the substrate into the coating solution in the container, slowly place it at an angle to ensure that the voids in the metal oxide layer are completely replaced by the coating solution.
[0192] Next, using a spraying device, liquid B was applied to both sides of the substrate and dried at 60°C for 10 minutes. The mass increase of the substrate relative to its initial state was calculated to be 67.7 mg. A further firing at 400°C for 10 minutes was then performed to form a metal oxide layer on the substrate surface. This process of applying, drying, and firing liquid B was repeated once more.
[0193] Subsequently, it was fired at 700°C for 1 hour to form an adhesion of 514 g / m² on the coating substrate. 2 The metal oxide layer is used to obtain the electrode of Example A6.
[0194] Since the amount of metal oxide layer attached to the substrate is 5.14 g, the mass of 1 mole of LaNiO3 is 245.5 g, and the mass of 1 mole of Nb2O5 is 265.8 g, it can be concluded that by coating 135 mg of Nb2O5, a coating of Nb with the composition LaNiNb is obtained at a ratio of 0.05 moles relative to 1 mole of LaNiO3. 0.05 O 3.125 The electrodes.
[0195] (Example A7)
[0196] Prepare the coating substrate in the same manner as in Example A1. Next, prepare solution A of Example A7 in Table 1.
[0197] Similar to Example A2, liquid A was applied to both sides of the substrate, dried at 60°C for 10 minutes, and then fired at 400°C for 10 minutes to form a metal oxide layer on the substrate surface.
[0198] The process of coating, drying, and firing the solution A was repeated four times.
[0199] Niobium oxalate ammonium was dissolved in pure water to prepare an aqueous solution of niobium oxalate ammonium with a Nb concentration of 310 mmol / kg, which was used as solution B in Example A7. This aqueous solution of niobium oxalate ammonium was then transferred to a polyethylene container with a bottom edge of 13 cm × 13 cm and a height of 10 cm.
[0200] The substrate with a metal oxide layer formed on its surface was completely immersed in solution B. It was then lifted up, and solution B was applied to the entire surface of the substrate. The substrate was then placed horizontally, and a weak airflow was used with an air gun to allow the solution B clogging the mesh of the substrate to fall off. When measuring the mass of the substrate after air gun treatment, 1.3g of solution B was applied to the substrate. The substrate coated with solution B was dried at 60°C for 10 minutes and then fired at 400°C for 10 minutes.
[0201] The coating process involved applying solution A four times and solution B once, followed by drying and firing. This process was repeated five times, and then further fired at 600°C for one hour, resulting in an adhesion weight of 526 g / m² on the substrate. 2 The metal oxide layer is used to obtain the electrode of Example A7.
[0202] Due to the adhesion amount of 5.26 g and 1 mole of LaNi to the substrate 1.1 O 3.15 The mass of 253.8 g and the mass of 1 mole of Nb₂O₅ are 265.8 g. Therefore, it can be concluded that by coating 1.3 g of niobium oxalate ammonium aqueous solution with 310 mmol / kg Nb concentration five times, the mass of LaNi₂O₅ relative to 1 mole of Nb₂O₅ was obtained. 1.1 O 3.15 A coating with Nb and a composition of LaNi was applied at a ratio of 0.1 mol. 1.1 Nb 0.1 O 3.4 The electrodes.
[0203] (Example A8)
[0204] Except that the firing time at 700°C for 1 hour is replaced with a firing time at 750°C for 1 hour, the same as in Example A5 results in an adhesion weight of 505 g / m². 2 The metal oxide layer is used to obtain the electrode of Example A8.
[0205] (Example A9)
[0206] The substrate for coating was prepared in the same manner as in Example A1. Next, liquid A and liquid B of Example A9, as shown in Tables 1 and 2, were prepared.
[0207] Similar to Example A2, liquid A was applied to both sides of the substrate, dried at 60°C for 10 minutes, and then fired at 400°C for 10 minutes to form a metal oxide layer on the substrate surface.
[0208] After repeating the coating, drying, and firing cycle of solution A 11 times, solution B was applied to both sides of the substrate, followed by drying at 60°C for 10 minutes. The mass increase of the substrate relative to its initial state was calculated to be 38 mg. Further firing at 400°C for 10 minutes resulted in the formation of a metal oxide layer on the substrate surface.
[0209] Further firing at 700℃ for 1 hour resulted in an adhesion weight of 354g / m². 2 The metal oxide layer is used to obtain the electrode of Example A9.
[0210] Since the amount of metal oxide layer attached to the substrate is 3.54 g, the mass of 1 mole of LaNiO3 is 245.5 g, and the mass of 1 mole of Nb2O5 is 265.8 g, it can be concluded that by coating 38 mg of Nb2O5, a coating of Nb with the composition LaNiNb is obtained at a ratio of 0.02 moles relative to 1 mole of LaNiO3. 0.02 O 3.05 The electrodes.
[0211] (Example A10)
[0212] The substrate for coating was prepared in the same manner as in Example A1. Next, liquid A and liquid B of Example A10, as shown in Tables 1 and 2, were prepared.
[0213] Similar to Example A2, liquid A was applied to both sides of the substrate, dried at 60°C for 10 minutes, and then fired at 400°C for 10 minutes to form a metal oxide layer on the substrate surface.
[0214] After repeating the coating, drying, and firing cycle of solution A 13 times, solution B was applied to both sides of the substrate, followed by drying at 60°C for 10 minutes. The mass increase of the substrate relative to its initial state was calculated to be 43 mg. Further firing at 400°C for 10 minutes resulted in the formation of a metal oxide layer on the substrate surface.
[0215] Further firing at 700℃ for 1 hour resulted in an adhesion weight of 404 g / m². 2 The metal oxide layer is used to obtain the electrode of Example A10.
[0216] Since the amount of metal oxide layer attached to the substrate is 4.04 g, the mass of 1 mole of LaNiO3 is 245.5 g, and the mass of 1 mole of Nb2O5 is 265.8 g, it can be concluded that by coating 43 mg of Nb2O5, a coating of Nb with the composition LaNiNb is obtained at a ratio of 0.02 moles relative to 1 mole of LaNiO3. 0.02 O 3.05 The electrodes.
[0217] (Comparative Example A1)
[0218] As a porous nickel substrate, a 10cm square nickel metal mesh with SW 3.0mm, LW 4.5mm, a thickness of 1.2mm, and an aperture ratio of 54% was prepared. After sandblasting, the nickel metal mesh was acid-treated in hydrochloric acid at 50℃ and 6N for 6 hours, followed by washing with water and drying, and used as a coating substrate.
[0219] Next, a coating solution was prepared by mixing lanthanum acetate 1,5-hydrate and nickel nitrate hexahydrate at concentrations of 0.20 mol / L and 0.20 mol / L, respectively.
[0220] A flat, square base containing the coating liquid is placed at the bottom of the coating roller, allowing the coating liquid to penetrate into the EPDM coating roller. A roller is placed above it to ensure continuous contact between the roller and the coating liquid. A PVC roller is then placed on top of the roller to apply the coating liquid to the substrate (roller method). Before the coating liquid dries, the substrate is quickly passed between two EPDM sponge rollers. After drying at 50°C for 10 minutes, it is fired in a muffle furnace at 400°C for 10 minutes to form a metal oxide layer on the substrate surface.
[0221] After repeating the cycle of coating, drying, and firing on the roller 75 times, a further firing at 600°C for 1 hour resulted in an adhesion weight of 303 g / m². 2 The metal oxide layer was used to obtain the electrode of Comparative Example A1.
[0222] (Comparative Example A2)
[0223] Prepare a substrate for coating in the same manner as in Comparative Example A1.
[0224] Next, the concentrations of lanthanum nitrate hexahydrate, nickel nitrate hexahydrate, niobium ammonium oxalate n-hydrate, and glycine were mixed at 0.20 mol / L, 0.16 mol / L, 0.04 mol / L, and 0.36 mol / L, respectively, to prepare the coating solution.
[0225] The same roller coating, drying, and firing process was performed as in Comparative Example A1, and this cycle was repeated 40 times. A further firing at 700°C for 1 hour was then carried out to form a metal oxide layer, resulting in an adhesion weight of 145 g / m². 2 The electrode of Comparative Example A2.
[0226] (Method for determining the oxygen overvoltage and double-layer capacitance of the electrodes in the initial stage and after 500 hours of energization)
[0227] The oxygen overvoltage of the electrode is determined using the following steps.
[0228] The test electrode was cut into a square measuring 2 cm long and 2 cm wide when viewed from the thickness direction, and fixed to a nickel rod coated with PTFE using nickel screws. A platinum mesh was used as the counter electrode, and the electrode was tested at 80°C in a 32% (w / w) sodium hydroxide aqueous solution at 6 kA / m. 2 Electrolysis was performed using a specific current density, and the oxygen overvoltage was measured. The electrode area was set to 2 × 2 = 4 cm². 2 The current density was calculated. To eliminate the influence of resistive loss due to solution impedance, the oxygen overvoltage was measured using a three-electrode method with a Luglin tube. The distance between the Luglin tube tip and the anode was always fixed at 1 mm. A Solartron potentiostat / current meter "1470E system" was used as the oxygen overvoltage measuring device. Silver-silver chloride (Ag / AgCl) was used as the reference electrode for the three-electrode method. The electrolyte impedance, which could not be eliminated by the three-electrode method, was measured using AC impedance analysis, and the oxygen overvoltage was calibrated based on the measured electrolyte impedance values. The real and imaginary parts were plotted using a Solartron frequency response analyzer "1255B" to obtain a Cole-Cole curve, which was then analyzed using Zview software (published by Scribner Associates, Inc.). Figure 5 The electrolyte impedance R was calculated using the equivalent circuit fitting model. s and double-layer capacitor C dl . Figure 5 In this context, f represents the frequency at the top, and R... f Represents the resistance of the oxide coating, R ct This represents the charge transfer resistance. The double-layer capacitance C is calculated using the following formula. dl .
[0229] [Number 1]
[0230]
[0231] The resistance loss, which could not be eliminated by the three-electrode method, was measured using the AC impedance method, and the oxygen overvoltage was calibrated based on the measured resistance loss. The resistance loss was measured using a Solartron 1255B frequency response analyzer.
[0232] Additionally, in an aqueous solution of 32% sodium hydroxide at 80°C, at 6 kA / m 2 Electrolysis was performed at a current density for 500 hours, followed by measurements of the oxygen overvoltage and double-layer capacitance of the electrodes. The electrode area was assumed to be 4 cm². 2 The double-layer capacitance was calculated.
[0233] The evaluation results of Examples A1-10 and Comparative Examples A1-2 are shown in Table 3.
[0234] (Electrode 1cm after 500 hours of energization) 2 (Method for determining the molar number of La)
[0235] From 6kA / m 2 The test electrode (2cm long × 2cm wide, 4cm² area) after 500 hours of electrolysis at a current density 2 Cut out an area of 2cm from the middle. 2 A sample (1 cm long × 2 cm wide) was sealed in a closed container along with a solution consisting of 6 mL of ultrapure water, 4.5 mL of 30% hydrochloric acid, and 1.5 mL of 68% nitric acid. The container was heated at 95°C for 30 minutes to dissolve both the electrode catalyst and a portion of the substrate. First, ultrapure water was added to dilute the solution to a total mass of 100 g. Next, 49 g of ultrapure water was added to 1 g of the diluted solution to further dilute it. The concentration of La was then determined using ICP-AES (Inductively Coupled Plasma Emission Spectrometry).
[0236] The area of 2 cm² was calculated based on the obtained La concentration and dilution rate. 2 The mass of La contained in the electrode sample was then calculated. The mass of La was then divided by the atomic weight of La, 138.9, to determine the area of 2 cm². 2 The number of moles (mmol) of La contained in the electrode sample. This number of moles of La is further divided by the electrode area of 2 cm². 2 Therefore, the electrode thickness per 1 cm after 500 hours of energization was calculated. 2 The number of moles of La (mmol / cm) 2 ).
[0237] The evaluation results of Examples A1-10 and Comparative Examples A1-2 are shown in Table 3.
[0238] (Calculation method of electrostatic capacitance of electrode per 1 mmol of La after 500 hours of energization)
[0239] The double-layer capacitance (F / cm) of the electrode after 500 hours of energization. 2 Divide by the number of moles of La per unit area (mmol / cm²) 2 From this, the electrostatic capacitance (F / mmol) of the electrode per 1 mmol of La after 500 hours of energization was calculated. La ).
[0240] The evaluation results of Examples A1-10 and Comparative Examples A1-2 are shown in Table 3.
[0241] (combustion byproduct gas / LaNi) x M y O 3-z (Calculation method of molar ratio)
[0242] Considering the preparation ratio, the reaction equations of the respective raw materials are added to create a reaction equation for firing a mixture of the anhydrous raw materials for La, Ni, and M, hydrogen peroxide, and a compound having a carboxyl group and an amino group and containing C, H, N, and O as constituent elements, in the form of molar ratio of combustion by-produced gas / LaNi x M y O 3-z to calculate the total number of moles of CO2, H2O, and N2 by-produced when 1 mole of LaNi x M y O 3-z is generated.
[0243] It should be noted that after LaNi is prepared by combustion x O 3-z is prepared, in the case where raw material M is separately added to prepare LaNi x M y O 3-z , the CO2, H2O, and N2 by-produced by the combustion of raw material M are not considered in the calculation of the molar ratio of combustion by-produced gas / LaNi x M y O 3-z .
[0244] The reaction equations of the respective raw materials are as described below.
[0245] <La(NO3)3·6H2O>
[0246] La(NO3)3→LaO 1.5 +1.5N2+3.75O2···(Equation 1)
[0247] <Lanthanum acetate sesquihydrate>
[0248] (CH3COO)3La+6O2→LaO 1.5 +6CO2+4.5H2O···(Equation 2)
[0249] <Ni(NO3)2·6H2O>
[0250] Ni(NO3)2→NiO 1.5 +N2+2.25O2···(Equation 3)
[0251] <Ammonium niobium oxalate>
[0252] NH4NbO(C2O4)2+1.75O2→0.5N2+4CO2+2H2O+NbO 2.5 ···(Equation 4)
[0253] <Nb2O5 sol>
[0254] Nb2O5→2NbO 2.5 (No by-product gas generated)···(Equation 5)
[0255] <Hydrogen peroxide>
[0256] H2O2→H2O+0.5O2···(Equation 6)
[0257] <Mn(NO3)2·6H2O>
[0258] Mn(NO3)2→MnO 1.5 +N2+2.25O2···(Equation 7)
[0259] <TiO2 sol>
[0260] TiO2→TiO2 (No by-product gas generated)···(Equation 8)
[0261] <ZrO(NO3)2·2H2O>
[0262] ZrO(NO3)2→ZrO2+N2+2.5O2···(Equation 9)
[0263] <tacl5>
[0264] TaCl5 + 1.25O2 → TaO 2.5 +2.5Cl2···(Equation 10)
[0265] Antimony tartrate
[0266] H(C4H2O6)Sb + 3O2 → 4CO2 + SbO 2.5 +1.5H₂O···(Equation 11)
[0267] <glycine>
[0268] C2H5NO2 + 2.25O2 → 2CO2 + 2.5H2O + 0.5N2 ··· (Equation 12)
[0269] Aspartic acid
[0270] C4H7NO4 + 3.75O2 → 4CO2 + 3.5H2O + 0.5N2 ··· (Equation 13)
[0271] For example, La(NO3)3·6H2O, Ni(NO3) 2· The reaction equation for the combustion of 6H2O, ammonium niobate oxalate, and glycine in a molar ratio of 1:0.8:0.2:1.38 is (Equation 1) + 0.8*(Equation 3) + 0.2*(Equation 4) + 1.38*(Equation 12), which is (Equation A) below. The combustion byproduct gas / LaNi x M y O 3-z The molar ratio is 3.09 + 3.85 + 3.56 = 10.5.
[0272] La(NO3)3+0.8Ni(NO3)2+0.2{NH4NbO(C2O4)2+1.75O2}+1.38(C2H5NO2+2.25O2)→(LaO 1.5 +1.5N2+3.75O2)+0.8(NiO 1.5 +N2+2.25O2)+0.2(0.5N2+4CO2+2H2O+NbO 2.5 )+1.38(2CO2+2.5H2O+0.5N2)→LaNi 0.8 Nb 0.2 O 3.2 +3.09N2 + 5.55O2 + 3.85H2O + 3.56CO2... (Formula A)
[0273] The evaluation results of Examples A1-10 and Comparative Examples A1-2 are shown in Table 3.
[0274] (Example A11)
[0275] The following describes the fabrication of an electrolysis unit and a bipolar electrolytic cell for alkaline water electrolysis.
[0276] -anode-
[0277] It is made using the same method as in Example A5.
[0278] -cathode-
[0279] As a conductive substrate, a flat woven mesh substrate is made by weaving nickel wire with a diameter of 0.15 mm into a 40-mesh substrate, and a substrate made by loading platinum on the flat woven mesh substrate is used.
[0280] -Next door, outer frame-
[0281] As a bipolar element, it uses a component with a partition separating the anode and cathode, and an outer frame surrounding the partition. All parts in contact with the electrolyte, such as the partition and the frame of the bipolar element, are made of nickel.
[0282] -Conductive elastomer-
[0283] The conductive elastomer uses the following material: a braided fabric made of nickel wire with a diameter of 0.15 mm, corrugated with a corrugation height of 5 mm.
[0284] -Septum-
[0285] A coating solution with the following composition was obtained using zirconium oxide (trade name "EP Zirconium Oxide", manufactured by Daiichi Rare Element Chemical Co., Ltd.), N-methyl-2-pyrrolidone (manufactured by Wako Pure Chemical Industries, Ltd.), polysulfone ("Udel" (registered trademark), manufactured by Solvay Advanced Polymers Co., Ltd.), and polyvinylpyrrolidone (weight average molecular weight (Mw) 900,000, manufactured by Wako Pure Chemical Industries, Ltd.).
[0286] Polysulfone: 15 parts by weight
[0287] Polyvinylpyrrolidone: 6 parts by weight
[0288] N-Methyl-2-pyrrolidone: 70 parts by weight
[0289] Zirconia: 45 parts by weight
[0290] The above coating solution was applied to both surfaces of a polyphenylene sulfide mesh (manufactured by Clever, 280 μm thick, 358 μm mesh size, 150 μm fiber diameter) serving as the substrate. Immediately after coating, the substrate coated with the solution was exposed to steam, followed by immersion in a coagulation bath to form a coating film on the substrate surface. The coating film was then thoroughly rinsed with pure water to obtain a porous membrane.
[0291] -Gasket-
[0292] The gasket uses a component that is a quadrilateral component with a thickness of 4.0 mm, a width of 18 mm, and an inner dimension of 504 mm square. It has an opening on the inside that is the same size as the electrode chamber when viewed from above, and has a slit structure for holding it in place by inserting a diaphragm.
[0293] -Zero-gap bipolar element-
[0294] The zero-gap battery cell 60 with an external manifold is rectangular, measuring 540mm × 620mm, with the current-carrying surfaces of the anode 2a and cathode 2c having areas of 500mm × 500mm. On the cathode side of the zero-gap bipolar element 60, the cathode 2c, conductive elastomer 2e, and cathode current collector 2r are laminated and connected to the partition wall 1 via the cathode rib 6, forming a cathode chamber 5c through which electrolyte flows. On the anode side, the anode 2a is connected to the partition wall 1 via the anode rib 6, forming an anode chamber 5a through which electrolyte flows. Figure 2 ).
[0295] Depth of anode chamber 5a (anode chamber depth, Figure 2 The distance between the partition wall and the anode is 25mm, and the depth of the cathode chamber is 5c (cathode chamber depth, Figure 2 The distance between the partition wall and the cathode current collector is 25 mm, and the material is nickel. The anode rib 6, which is 25 mm high and 1.5 mm thick, is assembled with the cathode rib 6, which is 25 mm high and 1.5 mm thick, by welding. The resulting nickel partition wall 1 has a thickness of 2 mm.
[0296] As the cathode current collector 2r, a pre-sandblasted nickel mesh substrate is used. The substrate thickness is 1 mm and the aperture ratio is 54%. A conductive elastomer 2e is spot-welded to the cathode current collector 2r for fixation. This zero-gap type bipolar element is stacked with a diaphragm-holding gasket in between, thereby forming a zero-gap structure Z in which the anode 2a and cathode 2c are pressed against the diaphragm 4.
[0297] Using the electrolysis apparatus of Example A11 above, with an electrolyte temperature of 80°C and a current density of 6kA / m 2 Water electrolysis was performed continuously for 500 hours under positive current. The voltage of each unit in Example A11 was monitored and the voltage shift was recorded. For each unit voltage, the average value of three units in Example A11 was taken and compared.
[0298] In Example A11, the average overvoltage of the three cells was a low value of 1.73V after 500 hours of operation. Therefore, it can be concluded that the anode of Example A5 achieved a low cell voltage even after prolonged operation.
[0299]
[0300]
[0301]
[0302] (Example B1)
[0303] As a porous nickel substrate, a nickel metal mesh with an SW of 3.0 mm, an LW of 4.5 mm, a thickness of 1.2 mm, and an aperture ratio of 54% was prepared. After sandblasting the nickel metal mesh, a substrate measuring 10 cm in length and 10 cm in width was cut out. The substrate was then subjected to acid treatment in hydrochloric acid at 50°C and 6 N for 6 hours, followed by washing with water and drying, to serve as a coating substrate.
[0304] Next, solutions A and B, with the compositions of Example B1 in Table 4, were prepared. Solution B was prepared by dissolving ammonium niobate oxalate in pure water, and the concentration of Nb was confirmed by ICP-AES (inductively coupled plasma optical emission spectrometry).
[0305] Liquid A was poured into a square polyethylene container with a bottom edge of 6cm × 10cm and a height of 11cm. Liquid B was slowly mixed while stirring with a magnetic stirrer, which served as the coating liquid for Example B1.
[0306] While stirring the coating liquid, the substrate to be coated is placed vertically, with the lower half immersed in the coating liquid. Then, the substrate is flipped over so that the upper half is also immersed in the coating liquid. After the coating liquid is applied to the entire surface of the substrate, the excess coating liquid is blown away using a blower based on an air gun while the substrate is placed vertically.
[0307] It is then dried at 60°C for 10 minutes and then fired at 400°C for 10 minutes to form a metal oxide layer on the substrate surface.
[0308] After repeating the coating, drying, and firing cycle 13 times, a further firing at 800°C for 1 hour resulted in an adhesion weight of 40 g / m² on the coating substrate. 2 The metal oxide layer is used to obtain the anode for water electrolysis.
[0309] (Examples B2-6)
[0310] The substrate for coating was prepared using the same method as in Example B1. Liquid A and Liquid B, with the compositions of Examples B2-6 in Table 4, were prepared. Then, as in Example B1, Liquid A and Liquid B were mixed in a square polyethylene container to prepare the coating solutions of Examples B2-6. The coating, drying, and firing cycles were then repeated as in Example B1. After firing at 800°C for 1 hour, an adhesion weight of 40 g / m² was formed on the substrate for coating. 2 The metal oxide layer was used to obtain the anode for water electrolysis in Examples B2 to 6.
[0311] (Example B7)
[0312] Dissolve 9.30g of Ni(NO3)2·6H2O, 34.64g of La(NO3)3·6H2O, 30.03g of glycine (C2H5NO2), and 13.78g of Mn(NO3)2·6H2O in 400g of pure water to prepare the coating solution of Example B7. Transfer the coating solution to a polyethylene container with a bottom edge of 13cm × 13cm and a height of 10cm.
[0313] Prepare the coating substrate in the same manner as in Example B1. Immerse the substrate completely in the coating liquid in the container, then pull it up to coat the entire surface of the substrate with the coating liquid. Place the substrate vertically and use a blower based on an air gun to blow away the excess coating liquid.
[0314] It is then dried at 60°C for 10 minutes and then fired at 400°C for 10 minutes to form a metal oxide layer on the substrate surface.
[0315] After repeating the coating, drying, and firing cycle 13 times, a further firing at 800°C for 1 hour resulted in an adhesion weight of 40 g / m² on the coating substrate. 2 The metal oxide layer is used to obtain the anode for water electrolysis.
[0316] (Example B8)
[0317] Dissolve 18.61 g of Ni(NO3)2·6H2O, 34.64 g of La(NO3)3·6H2O, and 27.63 g of glycine in 200 g of pure water to prepare solution A of Example B8. Dilute TiO2 sol with pure water to prepare 200 g of TiO2 sol with a Ti concentration of 80 mmol / kg to prepare solution B of Example B8.
[0318] Similar to Example B1, liquids A and B were mixed in a square polyethylene container to form the coating liquid for Example B8. After repeating the coating, drying, and firing cycles as in Example B1, the mixture was fired at 800°C for 1 hour, resulting in an adhesion weight of 40 g / m² on the coating substrate. 2 The metal oxide layer is used to obtain the anode for water electrolysis in Example B8.
[0319] (Example B9)
[0320] The coating solution of Example B9 was prepared by dissolving 20.93g of Ni(NO3)2·6H2O, 34.64g of La(NO3)3·6H2O, 30.03g of glycine, and 2.14g of ZrO(NO3)2·2H2O in 400g of pure water.
[0321] Subsequently, the anode for water electrolysis of Example B9 was obtained in the same manner as in Example B7.
[0322] (Example B10)
[0323] The coating solution of Example B10 was prepared by dissolving 26.75g of Ni(NO3)2·6H2O, 34.64g of La(NO3)3·6H2O, 31.83g of glycine, and 1.43g of TaCl5 in 400g of pure water.
[0324] Subsequently, the anode for water electrolysis of Example B10 was obtained in the same manner as in Example B7.
[0325] (Example B11)
[0326] Dissolve 17.45 g of Ni(NO3)2·6H2O, 34.64 g of La(NO3)3·6H2O, and 27.03 g of glycine in 200 g of pure water to prepare solution A for Example B11. Dissolve antimony tartrate in pure water to prepare 200 g of antimony tartrate solution with an Sb concentration of 20 mmol / kg to prepare solution B for Example B11. The concentration of Sb was confirmed by ICP-AES (inductively coupled plasma optical emission spectrometry).
[0327] Similar to Example B1, liquids A and B were mixed in a square polyethylene container to form the coating liquid for Example B11. After repeating the coating, drying, and firing cycles as in Example B1, the mixture was fired at 800°C for 1 hour to form an adhesion weight of 40 g / m² on the coating substrate. 2 The metal oxide layer is used to obtain the anode for water electrolysis in Example B11.
[0328] (Example B12)
[0329] The coating solution of Example B12 was prepared by dissolving 23.26g of Ni(NO3)2·6H2O, 34.64g of La(NO3)3·6H2O, and 30.03g of glycine in 400g of pure water.
[0330] The substrate for coating was prepared using the same method as in Example B1. The coating liquid was applied to both sides of the substrate using a spraying device (rCoater sold by Asahi Sunac Co., Ltd.), and then dried at 60°C for 10 minutes. The substrate was then fired at 400°C for 10 minutes to form a metal oxide layer on the surface of the substrate.
[0331] The coating, drying, and firing cycle was repeated 24 times.
[0332] The Nb2O5 sol with a particle size of less than 5 nm was further diluted to prepare an Nb2O5 sol with a Nb concentration of 200 mmol / kg.
[0333] The Nb₂O₅ sol was applied to both sides using a spraying device and then dried at 60°C for 10 minutes. The weight increase relative to the substrate before coating was calculated to be 38 mg. Since the amount of LaNiO₃ adhering to the substrate is 1.4 g, the weight of 1 mole of LaNiO₃ is 245.6 g, and the weight of 1 mole of Nb₂O₅ is 265.2 g, it can be concluded that by coating with 38 mg of Nb₂O₅, Nb was coated at a ratio of 0.05 moles relative to 1 mole of LaNiO₃.
[0334] The substrate, dried at 60°C for 10 minutes, was fired at 400°C for 10 minutes, and then further fired at 800°C for 1 hour, resulting in an adhesion weight of 144 g / m². 2 The metal oxide layer is used to obtain the anode for water electrolysis in Example B12.
[0335] (Example B13)
[0336] The coating solution of Example B13 was prepared in the same manner as in Example B12. The coating solution was then transferred into a polyethylene container with a bottom edge of 13cm × 13cm and a height of 10cm.
[0337] The substrate for coating was prepared using the same method as in Example B1. The substrate was completely immersed in the coating liquid in the container, then lifted to coat the entire surface of the substrate with the coating liquid. The substrate was then laid horizontally, and excess coating liquid was blown away using a blower-based air jet. It was then dried at 60°C for 10 minutes, and further fired at 400°C for 10 minutes to form a metal oxide layer on the substrate surface.
[0338] The coating, drying, and firing cycle was repeated 24 times.
[0339] Niobium oxalate ammonium was dissolved in pure water to prepare an aqueous solution of niobium oxalate ammonium with a Nb concentration of 43.8 mmol / kg. This aqueous solution of niobium oxalate ammonium was then transferred to a polyethylene container with a bottom edge of 13 cm × 13 cm and a height of 10 cm.
[0340] The substrate with a metal oxide layer formed on its surface was completely immersed in an aqueous solution of ammonium niobate oxalate. Afterward, it was pulled up to coat the entire surface of the substrate with the coating solution. The substrate was then placed horizontally, and a weak airflow was used with an air gun to allow the coating solution clogging the mesh of the substrate to fall off. The weight of the substrate after air gun treatment was measured. 1.3 g of ammonium niobate oxalate aqueous solution was coated on the substrate. Since the amount of LaNiO3 adhering to the substrate was 1.4 g, and the weight of 1 mole of LaNiO3 was 245.6 g, it can be concluded that coating with 1.3 g of ammonium niobate aqueous solution with a Nb concentration of 43.8 mmol / kg resulted in Nb being coated at a ratio of 0.01 moles relative to 1 mole of LaNiO3.
[0341] The substrate coated with niobium ammonium oxalate aqueous solution was dried at 60°C for 10 minutes, then fired at 400°C for 10 minutes, and further fired at 800°C for 1 hour to form an adhesion weight of 141 g / m². 2 The metal oxide layer is used to obtain the anode for water electrolysis in Example B13.
[0342] (Example B14)
[0343] After repeating the drying and firing cycle 24 times in the same manner as in Example B13, the substrate was fired at 800°C for 1 hour to form a metal oxide layer on the substrate surface.
[0344] Niobium oxalate ammonium was dissolved in pure water to prepare an aqueous solution of niobium oxalate ammonium with a Nb concentration of 87.7 mmol / kg. This aqueous solution of niobium oxalate ammonium was then transferred to a polyethylene container with a bottom edge of 13 cm × 13 cm and a height of 10 cm.
[0345] The substrate with a metal oxide layer formed on its surface was completely immersed in an aqueous solution of ammonium niobate oxalate. Afterward, it was lifted, and the coating solution was applied to the entire surface of the substrate. The substrate was then placed horizontally, and a weak airflow was used with an air gun to allow the coating solution clogging the mesh of the substrate to fall off. The weight of the substrate after air gun treatment was measured. 1.3 g of the ammonium niobate oxalate aqueous solution was coated on the substrate. Since the amount of LaNiO3 adhering to the substrate was 1.4 g, and the weight of 1 mole of LaNiO3 was 245.6 g, it can be concluded that coating with 1.3 g of an 87.7 mmol / kg Nb concentration ammonium niobate aqueous solution resulted in a Nb coating ratio of 0.02 moles relative to 1 mole of LaNiO3.
[0346] The substrate coated with niobium ammonium oxalate aqueous solution was dried at 60°C for 10 minutes, then fired at 400°C for 10 minutes, and further fired at 800°C for 1 hour to form an adhesion weight of 142 g / m². 2 The metal oxide layer is used to obtain the anode for water electrolysis in Example B14.
[0347] (Example B15)
[0348] Similar to Example B13, after repeating the drying and firing cycle 33 times, the substrate was fired at 800°C for 1 hour to form a metal oxide layer on the substrate surface.
[0349] Subsequently, an aqueous solution of ammonium niobate oxalate with a Nb concentration of 125 mmol / kg was prepared. Using the same method as in Example B14, Nb was coated at a ratio of 0.02 mol to 1 mol of LaNiO3. After drying at 60°C for 10 minutes, it was calcined at 400°C for 10 minutes, and then further calcined at 800°C for 1 hour, resulting in an adhesion weight of 202 g / m³. 2 The metal oxide layer is used to obtain the anode for water electrolysis in Example B15.
[0350] (Comparative Example B1)
[0351] Prepare the coating substrate in the same manner as in Example B1.
[0352] Next, a coating solution was prepared by mixing lanthanum acetate 1,5-hydrate and nickel nitrate hexahydrate at concentrations of 0.20 mol / L and 0.20 mol / L, respectively.
[0353] A flat, square base containing the coating liquid is placed at the bottom of the coating roller, allowing the coating liquid to penetrate into the EPDM coating roller. A roller is placed above it to ensure continuous contact between the roller and the coating liquid. A PVC roller is then placed on top of the roller to apply the coating liquid to the substrate (roller method). Before the coating liquid dries, the substrate is quickly passed between two EPDM sponge rollers. After drying at 50°C for 10 minutes, it is fired in a muffle furnace at 400°C for 10 minutes to form a metal oxide layer on the substrate surface.
[0354] After repeating the cycle of coating, drying, and firing on the roller 13 times, a further firing at 800°C for 1 hour resulted in an adhesion weight of 42 g / m². 2 The metal oxide layer is used to obtain the anode for water electrolysis.
[0355] (Comparative Example B2)
[0356] Prepare the coating substrate in the same manner as in Example B1.
[0357] Next, the coating solution was prepared with concentrations of lanthanum nitrate hexahydrate, nickel nitrate hexahydrate, niobium ammonium oxalate n-hydrate, and glycine of 0.20 mol / L, 0.16 mol / L, 0.04 mol / L, and 0.36 mol / L, respectively.
[0358] The same roller coating, drying, and firing process was performed as in Comparative Example B1, and this cycle was repeated 40 times. A further firing at 700°C for 1 hour was then carried out to form a metal oxide layer, resulting in an adhesion weight of 145 g / m². 2 Anode for water electrolysis.
[0359] (XRD determination method)
[0360] The test anode was cut into a square measuring 2 cm in length and 2 cm in width when viewed from the thickness direction, and measured using an XRD apparatus D8 ADVANCE (sold by Bruker Japan Co., Ltd.). The test anode was placed in a block sample holder (slot). A clay sheet (6 mm deep, PMMA material) was placed at the center of the sample electrode, with its surface height equal to the edge height of the sample holder, below the four corners. The sample electrode was then pressed down from the clay sheet to secure it. During the measurement, the sample was rotated at 15 rpm, and the range of 2θ = 10° to 70° was divided into 3080 steps, with each step lasting 4 seconds. Cu Kα1 X-rays were used, with an X-ray source voltage of 40 kV and a current of 40 mA. A 0.8° divergence slit was used. Table 5 shows the settings (overview data) of the detector, filters, and other devices, which can be verified using XRD WIZARD, the software for setting the measurement conditions.
[0361] Using the analysis software DIFFRAC.EVA, the "Peak Search" tool was used to perform peak search in the XRD spectrum to determine the 2θ of the peak position of each peak.
[0362] About LaNi x M y O 3-z The main peak position of NiO was detected by peak search near 2θ = 43.276°. The XRD spectrum was shifted using the "X-axis offset" tool so that the detected value of the main peak position 2θ of NiO was 2θ = 43.276° of the (200) plane of the PDF00-047-1049 card data of NiO. Then the calculation was performed.
[0363] LaNi x M y O 3-z The position of the main peak shifts depending on the sample. Referring to the main peak position of plane (104) of card PDF01-070-5757, 2θ = 33.166°, the peak position near 2θ = 32.5° to 33.2° is taken as LaNi x M y O 3-z The main peak location.
[0364] LaNi x M y O 3-z The main peak intensity was calculated using the "peak search" tool, and the LaNi x M y O 3-z The pure intensity of the main peak.
[0365] About LaNi x M y O 3-z The half-peak width of the main peak is calculated using the "Region Creation" tool in the analysis software DIFFRAC.EVA. The left end is set to 31° and the right end to 35° to select the region, and the half-peak width is calculated based on the calculated half-peak width.
[0366] The evaluation results of Examples B1-15 and Comparative Examples B1-2 are shown in Table 6.
[0367] (Alkali resistance test)
[0368] The test anode was cut into a square measuring 2 cm in length and 2 cm in width when viewed from the thickness direction, and XRD measurements were performed to calculate the LaNi content. x M y O 3-z The main peak intensity.
[0369] The alkali resistance test is conducted using the following steps.
[0370] The test anode was placed in a sealed PFA container with a capacity of 19 mL (outer diameter). The container (including a cap height of 44 mm and capacity) is filled with an 8 mol / L potassium hydroxide aqueous solution (sold by Kanto Chemical Co., Ltd.) and then sealed.
[0371] The PFA sealed container was then placed in a blower-controlled thermostat (product name DKN402, manufactured by Yamato Science Co., Ltd.) and heated to bring the liquid temperature inside the sealed container to 90°C. After maintaining the liquid temperature at 90°C for 24 hours, the sealed container was removed from the blower-controlled thermostat and ice-cooled.
[0372] The electrode was removed from the sealed container, washed with water and dried, and XRD measurements were performed again to calculate LaNi. x M y O 3-z The main peak intensity.
[0373] As an indicator of alkali resistance, the peak intensity retention rate is calculated using the following formula.
[0374] (Peak intensity retention rate (%)) = (LaNi after alkali resistance test) x M y O 3-z XRD main peak intensity) / (LaNi before alkali resistance test) x M y O 3-z (XRD main peak intensity) × 100
[0375] The evaluation results of Examples B1-15 and Comparative Examples B1-2 are shown in Table 6.
[0376] (Determination of oxygen overvoltage after alkali resistance test of the anode)
[0377] The oxygen overvoltage of the anode after the alkali resistance test is determined by the following steps.
[0378] After the alkali resistance test, the anode (2cm long x 2cm wide) was fixed to a nickel rod coated with PTFE using a nickel screw. A platinum mesh was used as the counter electrode in an 80°C, 32% wt% sodium hydroxide aqueous solution at 6kA / m. 2 Electrolysis was performed using a specific current density, and the oxygen overvoltage was measured. The electrode area was set to 2 × 2 = 4 cm². 2 The current density was calculated. To eliminate the influence of resistive loss due to solution impedance, the oxygen overvoltage was measured using a three-electrode method with a Luglin tube. The distance between the Luglin tube tip and the anode was kept constant at 1 mm. A Solartron potentiostat / galvanometer "1470E system" was used as the apparatus for measuring the oxygen overvoltage. Silver-silver chloride (Ag / AgCl) was used as the reference electrode for the three-electrode method. The electrolyte impedance, which could not be eliminated by the three-electrode method, was measured using AC impedance spectroscopy, and the oxygen overvoltage was calibrated based on the measured electrolyte impedance values.
[0379] The real and imaginary parts were plotted using a Solartron "1255B" frequency response analyzer to obtain the Cole-Cole curve. Equivalent circuit fitting was then used for analysis to calculate the electrolyte impedance and double-layer capacitance. The electrode area was set to 2 × 2 = 4 cm². 2 To calculate the double-layer capacitance.
[0380] The resistance loss, which could not be eliminated by the three-electrode method, was measured using the AC impedance method, and the oxygen overvoltage was calibrated based on the measured resistance loss. The resistance loss was measured using a Solartron 1255B frequency response analyzer.
[0381] The evaluation results of Examples B1-15 and Comparative Examples B1-2 are shown in Table 6.
[0382] (Method for determining the double-layer capacitance of the initial electrode)
[0383] The double-layer capacitance was measured using the same method as in Example A and Comparative Example A described above.
[0384] The measurement results of Examples B1-15 and Comparative Examples B1-2 are shown in Table 6.
[0385] (combustion byproduct gas / LaNi) x M y O 3-z (Calculation method of molar ratio)
[0386] The combustion byproduct gas / LaNi ratio was calculated using the same method as in Example A and Comparative Example A above. x M y O 3-z Molar ratio.
[0387] The measurement results of Examples B1-15 and Comparative Examples B1-2 are shown in Table 6.
[0388] (Example B16)
[0389] The following describes the fabrication of an electrolysis unit and a bipolar electrolytic cell for alkaline water electrolysis.
[0390] -anode-
[0391] It is made using the same method as in Example B14.
[0392] -cathode-
[0393] As a conductive substrate, a flat woven mesh substrate is made by weaving nickel wire with a diameter of 0.15 mm into a 40-mesh substrate, and a substrate made by loading platinum on the flat woven mesh substrate is used.
[0394] -Next door, outer frame-
[0395] As a bipolar element, it uses a component with a partition separating the anode and cathode, and an outer frame surrounding the partition. All parts in contact with the electrolyte, such as the partition and the frame of the bipolar element, are made of nickel.
[0396] -Conductive elastomer-
[0397] The conductive elastomer uses the following material: a braided fabric made of nickel wire with a diameter of 0.15 mm, corrugated with a corrugation height of 5 mm.
[0398] -Septum-
[0399] A coating solution with the following composition was obtained using zirconium oxide (trade name "EP Zirconium Oxide", manufactured by Daiichi Rare Element Chemical Co., Ltd.), N-methyl-2-pyrrolidone (manufactured by Wako Pure Chemical Industries, Ltd.), polysulfone ("Udel" (registered trademark), manufactured by Solvay Advanced Polymers Co., Ltd.), and polyvinylpyrrolidone (weight average molecular weight (Mw) 900,000, manufactured by Wako Pure Chemical Industries, Ltd.).
[0400] Polysulfone: 15 parts by weight
[0401] Polyvinylpyrrolidone: 6 parts by weight
[0402] N-Methyl-2-pyrrolidone: 70 parts by weight
[0403] Zirconia: 45 parts by weight
[0404] The above coating solution was applied to both surfaces of a polyphenylene sulfide mesh (manufactured by Clever, 280 μm thick, 358 μm mesh size, 150 μm fiber diameter) serving as the substrate. Immediately after coating, the substrate coated with the solution was exposed to steam, followed by immersion in a coagulation bath to form a coating film on the substrate surface. The coating film was then thoroughly rinsed with pure water to obtain a porous membrane.
[0405] -Gasket-
[0406] The gasket uses a component that is a quadrilateral component with a thickness of 4.0 mm, a width of 18 mm, and an inner dimension of 504 mm square. It has an opening on the inside that is the same size as the electrode chamber when viewed from above, and has a slit structure for holding it in place by inserting a diaphragm.
[0407] -Zero-gap bipolar element-
[0408] The zero-gap battery cell 60 with an external manifold is rectangular, measuring 540mm × 620mm, with the current-carrying surfaces of the anode 2a and cathode 2c having areas of 500mm × 500mm. On the cathode side of the zero-gap bipolar element 60, the cathode 2c, conductive elastomer 2e, and cathode current collector 2r are laminated and connected to the partition wall 1 via the cathode rib 6, forming a cathode chamber 5c through which electrolyte flows. On the anode side, the anode 2a is connected to the partition wall 1 via the anode rib 6, forming an anode chamber 5a through which electrolyte flows. Figure 2 ).
[0409] Depth of anode chamber 5a (anode chamber depth, Figure 2 The distance between the partition wall and the anode is 25mm, and the depth of the cathode chamber is 5c (cathode chamber depth, Figure 2 The distance between the partition wall and the cathode current collector is 25 mm, and the material is nickel. The anode rib 6, which is 25 mm high and 1.5 mm thick, is assembled with the cathode rib 6, which is 25 mm high and 1.5 mm thick, by welding. The resulting nickel partition wall 1 has a thickness of 2 mm.
[0410] As the cathode current collector 2r, a pre-sandblasted nickel mesh substrate is used as the current collector. The substrate thickness is 1 mm and the aperture ratio is 54%. A conductive elastomer 2e is spot-welded to the cathode current collector 2r for fixation. This zero-gap type bipolar element is stacked with a diaphragm in between, thereby forming a zero-gap structure Z in which the anode 2a and cathode 2c are pressed against the diaphragm 4.
[0411] (Comparative Example B3)
[0412] Except for using the same anode as Comparative Example B2, the zero-gap bipolar element was manufactured in the same manner as in Example B15.
[0413] Using the electrolysis apparatus of Example B16 and Comparative Example B3 described above, the electrolyte was circulated while being kept at 90°C and allowed to stand for 24 hours. Afterward, the electrolyte temperature was lowered to 80°C, and the current density was 6 kA / m. 2 Water electrolysis was performed continuously for 500 hours under positive current. The voltage of each unit in Example B16 and Comparative Example B3 was monitored and the voltage shift was recorded. For the unit voltage of each unit, the average value of three units in Example B16 and Comparative Example B3 was taken for comparison.
[0414] In Example B16, the average overvoltage of the three cells was a low value of 1.77V after 500 hours of operation, while in Comparative Example B3, the average overvoltage of the three cells was a high value of 1.95V after 500 hours of operation. Therefore, it can be concluded that the anode of Example B16 exhibits higher alkali durability compared to Comparative Example B3, achieving a low cell voltage even during prolonged operation.
[0415]
[0416] [Table 5]
[0417] Overview data:
[0418] Range-independent data Detector PSD: LynxEye K-Beta Filter yes Prime Soller 2.5 Fixed Div Slit 0.6 Secondary Soller Slit 2.5 Detector Slit 12.21 Fixed Anti-Sc Slit 6.94
[0419]
[0420] (Example C1)
[0421] Prepare solutions A and B according to the composition of Example C1 in Table 7. Solution B was prepared by dissolving ammonium niobate oxalate in pure water, and the concentration of Nb was confirmed by ICP-AES (inductively coupled plasma optical emission spectrometry).
[0422] Liquid A was poured into a square polyethylene container with a bottom edge of 6cm × 10cm and a height of 11cm. Liquid B was slowly mixed while stirring with a magnetic stirrer, which served as the coating liquid for Example C1.
[0423] As a porous nickel substrate, a nickel metal mesh with SW 3.0 mm, LW 4.5 mm, a thickness of 1.2 mm, and an aperture ratio of 54% was prepared. The nickel metal mesh was sandblasted using #100 white molten alumina abrasive, then acid-treated in hydrochloric acid at 50°C and 6N for 6 hours, followed by washing with water and drying, to serve as a coating substrate.
[0424] For this substrate, the substrate is placed vertically in the coating solution within the container, with the lower half immersed in the solution. The substrate is then lifted, flipped over, and the upper half is also immersed in the coating solution, which is applied to the entire surface of the substrate. The substrate is then placed horizontally, and an excessive amount of coating solution is blown away using a blower-like process based on an air gun. It is then dried at 60°C for 10 minutes, followed by a further firing at 400°C for 10 minutes to form a metal oxide layer on the substrate surface.
[0425] The coating, drying, and firing cycle was repeated 50 times. A further firing at 800°C for 1 hour resulted in an adhesion of 503 g / m² on the coated substrate. 2 The metal oxide layer is used to obtain the anode for water electrolysis in Example C1.
[0426] (Example C2)
[0427] Except for preparing liquids A and B as described in Example C2 of Table 7, the process was carried out in the same manner as in Example C1, repeating the coating, drying, and firing cycles 33 times. Subsequently, a firing at 800°C for 1 hour was performed to form an adhesion weight of 496 g / m² on the coating substrate. 2 The metal oxide layer is used to obtain the anode for water electrolysis in Example C2.
[0428] (Example C3)
[0429] Except for preparing liquids A and B as described in Example C3 of Table 7, the process was the same as in Example C1, repeating the coating, drying, and firing cycle 25 times. A further firing at 750°C for 1 hour resulted in an adhesion weight of 498 g / m² on the coating substrate. 2 The metal oxide layer is used to obtain the anode for water electrolysis in Example C3.
[0430] (Example C4)
[0431] The coating solution of Example C4 was prepared by dissolving 34.89 g of Ni(NO3)2·6H2O, 51.96 g of La(NO3)3·6H2O, and 45.04 g of glycine in 400 g of pure water. The coating solution was then transferred to a polyethylene container with a bottom edge of 13 cm × 13 cm and a height of 10 cm.
[0432] The substrate was prepared in the same manner as in Example C1. The substrate was completely immersed in the coating solution in the container, then lifted up and placed horizontally. Excess coating solution was blown away using a blower-based air jet. It was then dried at 60°C for 10 minutes, followed by firing at 400°C for 10 minutes to form a metal oxide layer on the substrate surface. This coating, drying, and firing cycle was repeated 49 times.
[0433] Niobium oxalate ammonium was dissolved in pure water to prepare an aqueous solution of niobium oxalate ammonium with a Nb concentration of 157 mmol / kg. This aqueous solution of niobium oxalate ammonium was then transferred to a polyethylene container with a bottom edge of 13 cm × 13 cm and a height of 10 cm.
[0434] The substrate with a metal oxide layer formed on its surface was completely immersed in an aqueous solution of ammonium niobate oxalate. Afterward, it was lifted, and the coating solution was applied to the entire surface of the substrate. The substrate was then placed horizontally, and a weak airflow was used with an air gun to allow the coating solution clogging the mesh of the substrate to fall off. The weight of the substrate after air gun treatment was measured. 1.3 g of the ammonium niobate oxalate aqueous solution was coated on the substrate. Since the amount of LaNiO3 adhering to the substrate is 5.0 g, and the weight of 1 mole of LaNiO3 is 245.6 g, it can be concluded that by coating with 1.3 g of an ammonium niobate aqueous solution with a Nb concentration of 157 mmol / kg, Nb is coated at a ratio of 0.01 moles relative to 1 mole of LaNiO3.
[0435] The substrate coated with niobium ammonium oxalate aqueous solution was dried at 60°C for 10 minutes, then fired at 400°C for 10 minutes, and further fired at 800°C for 1 hour to form an adhesion weight of 512 g / m². 2 The metal oxide layer is used to obtain the anode for water electrolysis in Example C4.
[0436] (Example C5)
[0437] The coating solution of Example C5 was prepared by dissolving 40.71 g of Ni(NO3)2·6H2O, 60.62 g of La(NO3)3·6H2O, and 52.55 g of glycine in 400 g of pure water. The coating solution was then transferred to a polyethylene container with a bottom edge of 13 cm × 13 cm and a height of 10 cm.
[0438] Similar to Example C4, the substrate was completely immersed in the coating liquid in the container, then the substrate was lifted up and placed horizontally, and an excessive amount of coating liquid was blown away using a blower-like process based on an air gun. It was then dried at 60°C for 10 minutes, and further fired at 400°C for 10 minutes to form a metal oxide layer on the substrate surface. This coating, drying, and firing cycle was repeated 32 times.
[0439] Niobium oxalate ammonium was dissolved in pure water to prepare an aqueous solution of niobium oxalate ammonium with a Nb concentration of 261 mmol / kg. This aqueous solution of niobium oxalate ammonium was then transferred to a polyethylene container with a bottom edge of 13 cm × 13 cm and a height of 10 cm.
[0440] The substrate with a metal oxide layer on its surface was completely immersed in an aqueous solution of niobium ammonium oxalate. Afterward, it was lifted, and the coating solution was applied to the entire surface of the substrate. The substrate was then placed horizontally, and a weak airflow was used with an air gun to allow the coating solution clogging the substrate's mesh to fall off. The weight of the substrate after air gun treatment was measured, showing that 1.3 g of niobium ammonium oxalate aqueous solution was coated onto the substrate. The substrate coated with niobium ammonium oxalate aqueous solution was dried at 60°C for 10 minutes, followed by firing at 400°C for 10 minutes. This process of coating with 1.3 g of niobium ammonium oxalate aqueous solution, drying at 60°C for 10 minutes, and then firing at 400°C for 10 minutes was performed three times, followed by firing at 800°C for 1 hour, resulting in an adhesion weight of 492 g / m². 2 The metal oxide layer is used to obtain the anode for water electrolysis in Example C5.
[0441] Since the amount of LaNiO3 adhering to the substrate is 5.0g and the weight of 1 mole of LaNiO3 is 245.6g, it can be concluded that by coating 1.3g of Nb concentration 261mmol / kg of ammonium niobate oxalate aqueous solution three times, for a total coating of 3.9g, Nb was coated at a ratio of 0.05 moles relative to 1 mole of LaNiO3.
[0442] (Example C6)
[0443] Except for preparing liquids A and B as described in Example C6 of Table 7, the process was carried out in the same manner as in Example C1, repeating the coating, drying, and firing cycle 24 times. Subsequently, a firing at 750°C for 1 hour was performed to form an adhesion weight of 486 g / m² on the coating substrate. 2 The metal oxide layer is used to obtain the anode for water electrolysis in Example C6.
[0444] (Example C7)
[0445] Dissolve 18.61g of Ni(NO3)2·6H2O, 69.28g of La(NO3)3·6H2O, 60.06g of glycine (C2H5NO2), and 27.56g of Mn(NO3)2·6H2O in 400g of pure water to prepare the coating solution of Example C7. Transfer the coating solution to a polyethylene container with a bottom edge of 13cm × 13cm and a height of 10cm.
[0446] Prepare the coating substrate in the same manner as in Example C1. Immerse the substrate completely in the coating liquid in the container, then lift it up to apply the coating liquid to the entire surface of the substrate. Place the substrate horizontally and use a blower based on an air gun to blow away the excess coating liquid.
[0447] It is then dried at 60°C for 10 minutes and then fired at 400°C for 10 minutes to form a metal oxide layer on the substrate surface.
[0448] After repeating the coating, drying, and firing cycle 25 times, a further firing at 750°C for 1 hour resulted in an adhesion weight of 508 g / m² on the coating substrate. 2 The metal oxide layer is used to obtain the anode for water electrolysis in Example C7.
[0449] (Example C8)
[0450] Dissolve 37.22 g of Ni(NO3)2·6H2O, 69.28 g of La(NO3)3·6H2O, and 55.25 g of glycine in 200 g of pure water to prepare solution A for Example C8. Dilute TiO2 sol with pure water to prepare 200 g of TiO2 sol with a Ti concentration of 160 mmol / kg to prepare solution B for Example C8.
[0451] Similar to Example C1, liquid A and liquid B were mixed in a square polyethylene container to form the coating liquid of Example C8.
[0452] The substrate for coating was prepared in the same manner as in Example C1. For this substrate, a cycle of coating with the coating liquid, drying at 60°C for 10 minutes, and firing at 400°C for 10 minutes was repeated 26 times using the same method as in Example C1. Subsequently, a firing at 750°C for 1 hour was performed, resulting in an adhesion weight of 496 g / m² on the substrate. 2 The metal oxide layer is used to obtain the anode for water electrolysis in Example C8.
[0453] (Example C9)
[0454] Dissolve 41.87g of Ni(NO3)2·6H2O, 69.28g of La(NO3)3·6H2O, 60.06g of glycine, and 4.28g of ZrO(NO3)2·2H2O in 400g of pure water to prepare the coating solution of Example C9. Transfer the coating solution to a polyethylene container with a bottom edge of 13cm × 13cm and a height of 10cm.
[0455] The substrate for coating was prepared in the same manner as in Example C1. For this substrate, the same method as in Example C7 was used to repeat 28 cycles of coating with the coating liquid, drying at 60°C for 10 minutes, and firing at 400°C for 10 minutes, followed by a further firing at 750°C for 1 hour, resulting in an adhesion weight of 502 g / m² on the substrate. 2 The metal oxide layer is used to obtain the anode for water electrolysis in Example C9.
[0456] (Example C10)
[0457] Dissolve 53.50 g of Ni(NO3)2·6H2O, 69.28 g of La(NO3)3·6H2O, and 63.66 g of glycine in 200 g of pure water to prepare solution A for Example C10. Dissolve 2.87 g of TaCl5 in 200 g of pure water to prepare solution B for Example C10.
[0458] Similar to Example C1, liquid A and liquid B were mixed in a square polyethylene container to form the coating liquid for Example C10.
[0459] The substrate for coating was prepared in the same manner as in Example C1. For this substrate, the same method as in Example C1 was used to repeat 25 cycles of coating with the coating liquid, drying at 60°C for 10 minutes, and firing at 400°C for 10 minutes. Subsequently, a firing at 750°C for 1 hour was performed to form an adhesion weight of 498 g / m² on the substrate. 2 The metal oxide layer is used to obtain the anode for water electrolysis in Example C10.
[0460] (Example C11)
[0461] Dissolve 34.89 g of Ni(NO3)2·6H2O, 69.28 g of La(NO3)3·6H2O, and 54.06 g of glycine in 200 g of pure water to prepare solution A for Example C11. Dissolve 200 g of antimony tartrate in pure water to prepare a solution with an Sb concentration of 40 mmol / kg to prepare solution B for Example C11. The Sb concentration was confirmed by ICP-AES (inductively coupled plasma optical emission spectrometry).
[0462] Similar to Example C1, liquid A and liquid B were mixed in a square polyethylene container to form the coating liquid of Example C11.
[0463] The substrate for coating was prepared in the same manner as in Example C1. For this substrate, the same method as in Example C1 was used to repeat 27 cycles of coating with the coating liquid, drying at 60°C for 10 minutes, and firing at 400°C for 10 minutes. Subsequently, a further firing at 750°C for 1 hour resulted in an adhesion weight of 504 g / m² on the substrate. 2 The metal oxide layer is used to obtain the anode for water electrolysis in Example C11.
[0464] (Comparative Example C1)
[0465] As a porous nickel substrate, a nickel metal mesh with SW 3.0 mm, LW 4.5 mm, a thickness of 1.2 mm, and an aperture ratio of 54% was prepared. After sandblasting, the nickel metal mesh was acid-treated in hydrochloric acid at 50°C and 6N for 6 hours, followed by washing with water and drying, and used as a coating substrate.
[0466] Next, a coating solution was prepared by mixing lanthanum acetate 1,5-hydrate and nickel nitrate hexahydrate at concentrations of 0.20 mol / L and 0.20 mol / L, respectively.
[0467] A flat, square base containing the coating liquid is placed at the bottom of the coating roller, allowing the coating liquid to penetrate into the EPDM coating roller. A roller is placed above it to ensure continuous contact between the roller and the coating liquid. A PVC roller is then placed on top of the roller to apply the coating liquid to the substrate (roller method). Before the coating liquid dries, the substrate is quickly passed between two EPDM sponge rollers. After drying at 50°C for 10 minutes, it is fired in a muffle furnace at 400°C for 10 minutes to form a metal oxide layer on the substrate surface.
[0468] After repeating the cycle of coating, drying, and firing on the roller 75 times, a further firing at 600°C for 1 hour resulted in an adhesion weight of 303 g / m². 2 The metal oxide layer was used to obtain the anode for water electrolysis of Comparative Example C1.
[0469] (Comparative Example C2)
[0470] Prepare a substrate for coating in the same manner as in Comparative Example C1.
[0471] Next, the coating solution was prepared with concentrations of lanthanum nitrate hexahydrate, nickel nitrate hexahydrate, niobium ammonium oxalate n-hydrate, and glycine of 0.20 mol / L, 0.16 mol / L, 0.04 mol / L, and 0.36 mol / L, respectively.
[0472] The same roller coating, drying, and firing process was performed as in Comparative Example C1, and this cycle was repeated 40 times. A further firing at 700°C for 1 hour was then carried out to form a metal oxide layer, resulting in an adhesion weight of 145 g / m². 2 Comparative example C2 is the anode used for water electrolysis.
[0473] (greater than 0.785μm) 2 And it is 20μm 2 The following are the calculation methods for the sum of pore areas, average pore area, average number of pores, and porosity.
[0474] The fabricated electrode pieces were embedded in epoxy resin, and then a cross-section was prepared. This cross-section was then processed using an argon ion beam (Hitachi High-Tech Co., Ltd. "E3500") wide-area irradiation BIB processing device at an accelerating voltage of 6 kV. It should be noted that the cross-section of the electrode being observed was parallel to the strands of the metal mesh and passed through the center of the strands.
[0475] The cross-section was observed using an electron microscope (Hitachi High-Tech S4800) at an accelerating voltage of 5kV and a magnification of 500x. The cross-sectional photographs obtained using the reflected electron image with a YAG detector were saved as BMP files with a data size of 1280×960 pixels. The size of 1 pixel is 198.4375nm.
[0476] Using the image processing software "Image J", follow steps 1) to 11) below to cut out a 20μm × 20μm region from the cross-sectional photograph. Extract the pores in each cut-out region using binarization. After measuring the area of all pores, calculate the area greater than 0.785μm. 2 And it is 20μm 2 The following are the sum of pore areas, average pore area, number of pores, and porosity. Ten 20μm × 20μm regions were extracted from the cross-sectional photograph in a non-overlapping manner, and the area greater than 0.785μm was calculated for each of the ten regions. 2 And it is 20μm 2 The following values for the sum of pore areas, average pore area, number of pores, and average porosity are used as the average values for the examples and comparative examples with pore sizes greater than 0.785 μm. 2 And it is 20μm 2 The following are the measurement results of the sum of the micropore areas, the average micropore area, the average number of micropores, and the porosity.
[0477] The measurement results of Examples C1-6 and Comparative Examples C1-2 are shown in Table 8.
[0478] 1) Open the BMP file of the cross-sectional photo, and select 8-bit in the Type submenu of the Image menu. Figure 6 An example of a cross-sectional photograph of an electrode is shown in the image.
[0479] 2) In the Set scale submenu of the Analyze menu, set Distance in Pixels: 1, Known distance: 0.1984375, Pixel aspect ratio: 1.0, Unit of length: μm, and click OK.
[0480] 3) In the Selection submenu of the Edit menu, select the Specify command, check the Scaled units (μm) checkbox, set Width: 20, Height: 20, and further adjust the values of X coordinate and Y coordinate as appropriate. Click OK to set a 20μm square area for image processing within the cross-sectional photograph. Figure 6 The image shows an example of the setting of a 20μm square region cut from a cross-sectional photograph. The 20μm square region where image processing is performed is set in such a way that it does not contain any cracks on the outer surface or leading to the outer surface.
[0481] 4) Execute the Crop command in the Image menu to cut out a 20μm square area for extracting fine pores. Figure 7 The text shows from Figure 6 An example of an image of a 20μm square region.
[0482] 5) Name and save the 20μm square region that has been cut.
[0483] 6) In the Process menu, select Median... in the Filters submenu, set Radius to 0.5, and click OK to perform filtering.
[0484] 7) Select the Threshold command from the Adjust submenu of the Image menu. Choose Otsu as the automatic threshold setting method and B&W as the display method. Do not check the Dark background option. Click the Auto button and then click the Apply button to perform binarization extraction of the pores. Figure 8 The text shows the output of a document. Figure 7 An example of an image obtained by binarizing and extracting the pores.
[0485] 8) Select the "Set Measurements..." command from the "Analyze" menu, and check the boxes in the "Area" section.
[0486] 9) Select the Analyze Particles... command from the Analyze menu, set Size (Pixel^2): 0-Infinity, Circularity: 0.00-1.00, Show: Outlines, check the boxes for Display results, Clear results, and Summerize, and do not check the boxes for Exclude on Edges and Include Holes. Click OK.
[0487] 10) The Count displayed in the Summary window represents the number of pores, and the Average Size represents the average pore area (μm²). 2 ) %Area represents the porosity (%).
[0488] 11) The first column at the left of the Results window displays the number of each pore, and the Area column displays the pore area (μm²) of each pore. 2 The numbering of each pore can be confirmed by the image with a number assigned to the measured pore outline, displayed in the "Image File Name" window created in "Drawing of 5". Among the pore area values in the Area column, those greater than 0.785 μm... 2 And it is 20μm 2 The areas below are all added together, and the result is greater than 0.785 μm. 2 And it is 20μm 2 The sum of the following pore areas.
[0489] (Determination of oxygen overvoltage in 55% potassium hydroxide aqueous solution)
[0490] The oxygen overvoltage in a 55% by weight potassium hydroxide aqueous solution was determined by the following steps.
[0491] Evaluation electrodes were cut from the electrodes of the examples and comparative examples, each measuring 2 cm in length and 2 cm in width when viewed from the thickness direction. They were then fixed to a nickel rod coated with PTFE using nickel screws. A platinum mesh was used as the counter electrode, and the electrodes were tested at 80°C and 6 kA / m in a 55% (w / w) potassium hydroxide aqueous solution. 2 Electrolysis was performed at a current density of [value missing], and the oxygen overvoltage was measured. The electrode area was assumed to be 2 × 2 = 4 cm². 2 The current density was calculated. To eliminate the influence of resistive loss due to solution impedance, the oxygen overvoltage was measured using a three-electrode method with a Luglin tube. The distance between the Luglin tube tip and the anode was kept constant at 1 mm. A Solartron potentiostat / galvanometer "1470E system" was used as the apparatus for measuring the oxygen overvoltage. Silver-silver chloride (Ag / AgCl) was used as the reference electrode for the three-electrode method. The electrolyte impedance, which could not be eliminated by the three-electrode method, was measured using AC impedance spectroscopy, and the oxygen overvoltage was calibrated based on the measured electrolyte impedance values.
[0492] The real and imaginary parts were plotted using a Solartron "1255B" frequency response analyzer to obtain the Cole-Cole curve. Analysis was then performed using equivalent circuit fitting to calculate the electrolyte impedance and double-layer capacitance. The electrode area was assumed to be 2 × 2 = 4 cm². 2 The double-layer capacitance was calculated.
[0493] The resistance loss, which could not be eliminated by the three-electrode method, was measured using the AC impedance method, and the oxygen overvoltage was calibrated based on the measured resistance loss. The resistance loss was measured using a Solartron 1255B frequency response analyzer.
[0494] The evaluation results of Examples C1-6 and Comparative Examples C1-2 are shown in Table 8.
[0495] (An early method for measuring the double-layer capacitance of electrodes)
[0496] The double-layer capacitance was measured using the same method as in Example A and Comparative Example A described above.
[0497] The evaluation results of Examples C1-6 and Comparative Examples C1-2 are shown in Table 8.
[0498] (combustion byproduct gas / LaNi) x M y O 3-z (Calculation method of molar ratio)
[0499] The combustion byproduct gas / LaNi ratio was calculated using the same method as in Example A and Comparative Example A described above. x M y O 3-z Molar ratio.
[0500] The measurement results of Examples C1-6 and Comparative Examples C1-2 are shown in Table 8.
[0501] (Example C7)
[0502] The following describes the fabrication of an electrolysis unit and a bipolar electrolytic cell for alkaline water electrolysis.
[0503] -anode-
[0504] It is prepared using the same method as in Example C4.
[0505] -cathode-
[0506] As a conductive substrate, a flat woven mesh substrate is made by weaving nickel wire with a diameter of 0.15 mm into a 40-mesh substrate, and platinum is loaded onto the flat woven mesh substrate to form a substrate.
[0507] -Next door, outer frame-
[0508] As a bipolar element, it uses a component with a partition separating the anode and cathode, and an outer frame surrounding the partition. All parts in contact with the electrolyte, such as the partition and the frame of the bipolar element, are made of nickel.
[0509] -Conductive elastomer-
[0510] The conductive elastomer uses the following material: a braided fabric made of nickel wire with a diameter of 0.15 mm, corrugated with a corrugation height of 5 mm.
[0511] -Septum-
[0512] A coating solution with the following composition was obtained using zirconium oxide (trade name "EP Zirconium Oxide", manufactured by Daiichi Rare Element Chemical Co., Ltd.), N-methyl-2-pyrrolidone (manufactured by Wako Pure Chemical Industries, Ltd.), polysulfone ("Udel" (registered trademark), manufactured by Solvay Advanced Polymers Co., Ltd.), and polyvinylpyrrolidone (weight average molecular weight (Mw) 900,000, manufactured by Wako Pure Chemical Industries, Ltd.).
[0513] Polysulfone: 15 parts by weight
[0514] Polyvinylpyrrolidone: 6 parts by weight
[0515] N-Methyl-2-pyrrolidone: 70 parts by weight
[0516] Zirconia: 45 parts by weight
[0517] The above coating solution was applied to both surfaces of a polyphenylene sulfide mesh (manufactured by Clever, 280 μm thick, 358 μm mesh size, 150 μm fiber diameter) serving as the substrate. Immediately after coating, the substrate coated with the solution was exposed to steam, followed by immersion in a coagulation bath to form a coating film on the substrate surface. The coating film was then thoroughly rinsed with pure water to obtain a porous membrane.
[0518] -Gasket-
[0519] The gasket uses a component that is a quadrilateral component with a thickness of 4.0 mm, a width of 18 mm, and an inner dimension of 504 mm square. It has an opening on the inside that is the same size as the electrode chamber when viewed from above, and has a slit structure for holding it in place by inserting a diaphragm.
[0520] -Zero-gap bipolar element-
[0521] The zero-gap battery cell 60 with an external manifold is rectangular, measuring 540mm × 620mm, with the current-carrying surfaces of the anode 2a and cathode 2c having areas of 500mm × 500mm. On the cathode side of the zero-gap bipolar element 60, the cathode 2c, conductive elastomer 2e, and cathode current collector 2r are laminated and connected to the partition wall 1 via the cathode rib 6, forming a cathode chamber 5c through which electrolyte flows. On the anode side, the anode 2a is connected to the partition wall 1 via the anode rib 6, forming an anode chamber 5a through which electrolyte flows. Figure 2 ).
[0522] Depth of anode chamber 5a (anode chamber depth, Figure 2 The distance between the partition wall and the anode is 25mm, and the depth of the cathode chamber is 5c (cathode chamber depth, Figure 2 The distance between the partition wall and the cathode current collector is 25 mm, and the material is nickel. The anode rib 6, which is 25 mm high and 1.5 mm thick, is assembled with the cathode rib 6, which is 25 mm high and 1.5 mm thick, by welding. The resulting nickel partition wall 1 has a thickness of 2 mm.
[0523] As the cathode current collector 2r, a pre-sandblasted nickel mesh substrate is used. The substrate thickness is 1 mm and the aperture ratio is 54%. A conductive elastomer 2e is spot-welded to the cathode current collector 2r for fixation. This zero-gap type bipolar element is stacked with a diaphragm-holding gasket in between, thereby forming a zero-gap structure Z in which the anode 2a and cathode 2c are pressed against the diaphragm 4.
[0524] (Comparative Example C3)
[0525] Except for using the same anode as Comparative Example C2, the zero-gap bipolar element was manufactured in the same manner as in Example C7.
[0526] Using the electrolysis apparatus of Example C7 and Comparative Example C3 above, the electrolyte of a 55% by weight potassium hydroxide aqueous solution was circulated at 80°C, with a current density of 6 kA / m. 2 The water electrolysis was performed continuously for 100 hours with positive current applied. The voltage of each unit in Example C7 and Comparative Example C3 was monitored, and the voltage shift was recorded. For the unit voltage of each unit, the average value of three units in Example C7 and Comparative Example C3 was taken and compared.
[0527] In Example C7, the average overvoltage of the three units was a low value of 1.70V after 100 hours of energization, while in Comparative Example C3, the average overvoltage of the three units was a high value of 1.90V after 100 hours of energization. Therefore, it can be concluded that, compared to Comparative Example C3, the anode of Example C7 exhibited a lower oxygen overvoltage in a high-concentration alkaline electrolyte, achieving a low unit voltage even after prolonged operation.
[0528]
[0529]
[0530] (Example D1)
[0531] As a porous nickel substrate, a nickel metal mesh with an SW of 3.0 mm, an LW of 4.5 mm, a thickness of 1.2 mm, and an aperture ratio of 54% was prepared. After sandblasting the nickel metal mesh, a substrate measuring 10 cm in length and 10 cm in width was cut out. The substrate was then subjected to acid treatment in hydrochloric acid at 50°C and 6 N for 6 hours, followed by washing with water and drying, to serve as a coating substrate.
[0532] The coating solution of Example D1 was prepared by dissolving 186.1g of Ni(NO3)2·6H2O, 692.8g of La(NO3)3·6H2O, 90.08g of glycine (C2H5NO2), and 275.6g of Mn(NO3)2·6H2O in 400g of pure water.
[0533] Using a spraying device (rCoater sold by Asahi Sunac Co., Ltd.), the coating liquid of Example D1 was applied to both sides of the substrate, dried at 60°C for 10 minutes, and then fired at 400°C for 10 minutes to form a metal oxide layer on the substrate surface.
[0534] The coating process of applying, drying, and firing was repeated 20 times, followed by firing at 700°C for 1 hour to achieve an adhesion weight of 1001 g / m². 2 The metal oxide layer is used to obtain the electrode of Example D1.
[0535] (Example D2)
[0536] Mix 372.2g of Ni(NO3)2·6H2O, 692.8g of La(NO3)3·6H2O, 99.45g of glycine, and 200g of TiO2 sol with a Ti concentration of 1.6mol / kg in 200g of pure water. Disperse the suspension using a T18 digital display ULTRA-TURRAX homogenizer (equipped with an S18N-19G Shaft Generator) sold by IKA Japan Co., Ltd., as the coating solution for Example D2.
[0537] Similar to Example D1, the coating liquid of Example D2 was applied to both sides of the substrate, dried at 60°C for 10 minutes, and then fired at 400°C for 10 minutes to form a metal oxide layer on the substrate surface.
[0538] The coating process of applying, drying, and firing was repeated 15 times, followed by firing at 700°C for 1 hour to achieve an adhesion weight of 752 g / m². 2 The metal oxide layer is used to obtain the electrode of Example D2.
[0539] (Example D3)
[0540] The coating solution of Example D3 was prepared by dissolving 418.7g of Ni(NO3)2·6H2O, 692.8g of La(NO3)3·6H2O, 102.1g of glycine, and 42.76g of ZrO(NO3)2·2H2O in 400g of pure water.
[0541] Similar to Example D1, the coating liquid of Example D3 was applied to both sides of the substrate, dried at 60°C for 10 minutes, and then fired at 400°C for 10 minutes to form a metal oxide layer on the substrate surface.
[0542] The coating process of applying, drying, and firing was repeated 30 times, followed by firing at 700°C for 1 hour to achieve an adhesion weight of 1505 g / m². 2 The metal oxide layer is used to obtain the electrode of Example D3.
[0543] (Example D4)
[0544] In 400g of pure water, Ni(NO3)2·6H2O: 535.0g, La(NO3)3·6H2O: 692.8g, glycine: 70.03g, and TaCl5: 28.66g were mixed. The suspension was dispersed using a T18 digital display ULTRA-TURRAX homogenizer (equipped with an S18N-19G Shaft Generator) sold by IKA Japan Co., Ltd., as the coating solution for Example D4.
[0545] Similar to Example D1, the coating liquid of Example D4 was applied to both sides of the substrate, dried at 60°C for 10 minutes, and then fired at 400°C for 10 minutes to form a metal oxide layer on the substrate surface.
[0546] The coating process of applying, drying, and firing was repeated 40 times, followed by firing at 700°C for 1 hour to achieve an adhesion weight of 2006 g / m². 2 The metal oxide layer was used to obtain the electrode of Example D4.
[0547] (Example D5)
[0548] As a porous nickel substrate, a nickel metal mesh with an SW of 3.0 mm, an LW of 4.5 mm, a thickness of 1.2 mm, and an aperture ratio of 54% was prepared. After sandblasting the nickel metal mesh, a substrate measuring 10 cm in length and 10 cm in width was cut out. The substrate was then subjected to acid treatment in hydrochloric acid at 50°C and 6 N for 6 hours, followed by washing with water and drying, to serve as a coating substrate.
[0549] Dissolve 39.54 g of Ni(NO3)2·6H2O, 69.28 g of La(NO3)3·6H2O, and 10.81 g of glycine in 200 g of pure water to prepare solution A for Example D5. Dissolve antimony tartrate in pure water to prepare an antimony tartrate solution with an Sb concentration of 40 mmol / kg to prepare solution B for Example D5. The Sb concentration was confirmed by ICP-AES (inductively coupled plasma optical emission spectrometry).
[0550] Liquid A was poured into a square polyethylene container with a bottom edge of 6cm × 10cm and a height of 11cm. Liquid B was slowly mixed while stirring with a magnetic stirrer, which served as the coating liquid for Example D5.
[0551] While stirring the coating liquid, the substrate to be coated is placed vertically, with the lower half immersed in the coating liquid. Then, the substrate is flipped over, and the upper half is also immersed in the coating liquid. After the coating liquid is applied to the entire surface of the substrate, the substrate is placed horizontally, and the excess coating liquid is blown away using a blower based on an air gun.
[0552] It is then dried at 60°C for 10 minutes and then fired at 400°C for 10 minutes to form a metal oxide layer on the substrate surface.
[0553] After repeating the coating, drying, and firing cycle 50 times, a further firing at 700°C for 1 hour resulted in an adhesion weight of 503 g / m² on the coating substrate. 2 The metal oxide layer is used to obtain the electrode of Example D5.
[0554] (Example D6)
[0555] A mixture of 488.5 g Ni(NO3)2·6H2O, 692.8 g La(NO3)3·6H2O, 70.03 g glycine, and 235.3 g of an aqueous solution of ammonium niobate with a Nb concentration of 0.34 mol / kg was mixed in 164.7 g of pure water. The suspension was dispersed using a T18 digital display ULTRA-TURRAX homogenizer (equipped with an S18N-19G Shaft Generator) sold by IKA Japan Co., Ltd., and used as the coating solution for Example D6.
[0556] Similar to Example D1, the coating liquid of Example D6 was applied to both sides of the substrate, dried at 60°C for 10 minutes, and then fired at 400°C for 10 minutes to form a metal oxide layer on the substrate surface.
[0557] The coating process of applying, drying, and firing was repeated 20 times, followed by firing at 700°C for 1 hour to achieve an adhesion weight of 1004 g / m². 2 The metal oxide layer was used to obtain the electrode of Example D6.
[0558] (Example D7)
[0559] Except for repeating the coating, drying, and firing cycles of the coating liquid 30 times, the process was carried out in the same manner as in Example D6, resulting in an adhesion weight of 1507 g / m². 2 The metal oxide layer is used to obtain the electrode of Example D7.
[0560] (Example D8)
[0561] Except for repeating the coating, drying, and firing cycles of the coating liquid 40 times, the process was carried out in the same manner as in Example D6, resulting in an adhesion weight of 2009 g / m². 2 The metal oxide layer is used to obtain the electrode of Example D8.
[0562] (Example D9)
[0563] A mixture of 465.2 g Ni(NO3)2·6H2O, 692.8 g La(NO3)3·6H2O, 90.08 g glycine, and 94.12 g of an aqueous solution of ammonium niobate with a Nb concentration of 0.34 mol / kg was mixed in 305.9 g of pure water. The suspension was dispersed using a T18 digital display ULTRA-TURRAX homogenizer (equipped with an S18N-19G Shaft Generator) sold by IKA Japan Co., Ltd., and used as the coating solution for Example D9.
[0564] Similar to Example D1, the coating liquid of Example D9 was applied to both sides of the substrate, dried at 60°C for 10 minutes, and then fired at 400°C for 10 minutes to form a metal oxide layer on the substrate surface.
[0565] The coating process of applying, drying, and firing was repeated 20 times, followed by firing at 700°C for 1 hour to achieve an adhesion weight of 1005 g / m². 2 The metal oxide layer is used to obtain the electrode of Example D9.
[0566] (Example D10)
[0567] Except for repeating the coating, drying, and firing cycles of the coating liquid 50 times, the process was carried out in the same manner as in Example D9, resulting in an adhesion weight of 2500 g / m². 2 The metal oxide layer is used to obtain the electrode of Example D10.
[0568] (Example D11)
[0569] Except for repeating the coating, drying, and firing cycles of the coating liquid 60 times, the process was carried out in the same manner as in Example D9, resulting in an adhesion weight of 3000 g / m². 2 The metal oxide layer is used to obtain the electrode of Example D11.
[0570] (Example D12)
[0571] As a porous nickel substrate, a nickel metal mesh with an SW of 3.0 mm, an LW of 4.5 mm, a thickness of 1.2 mm, and an aperture ratio of 54% was prepared. After sandblasting the nickel metal mesh, a substrate measuring 10 cm in length and 10 cm in width was cut out. The substrate was then subjected to acid treatment in hydrochloric acid at 50°C and 6 N for 6 hours, followed by washing with water and drying, to serve as a coating substrate.
[0572] Dissolve 26.75g of Ni(NO3)2·6H2O, 34.64g of La(NO3)3·6H2O, and 3.99g of aspartic acid in 200g of pure water, and transfer the solution to a square polyethylene container with a bottom edge of 6cm × 10cm and a height of 11cm, as solution A of Example D12.
[0573] Niobium oxalate ammonium was dissolved in pure water to prepare an aqueous solution of 200 g containing 20 mmol / kg Nb, which was used as solution B in Example D12. The concentration of Nb was confirmed by ICP-AES (inductively coupled plasma optical emission spectrometry).
[0574] While stirring liquid A of Example D12 using a magnetic stirrer, liquid B of Example D12 was slowly mixed to form the coating liquid of Example D12.
[0575] While stirring the coating solution, the substrate is held vertically, and the lower half is slowly immersed in the coating solution for 5 seconds. Then, the substrate is lifted and flipped over, and the upper half is also slowly immersed in the coating solution for 5 seconds. After the coating solution is applied to the entire surface of the substrate, the substrate is placed horizontally, and excess coating solution is blown away using a blower-like process based on an air gun. It is then dried at 60°C for 10 minutes, followed by a firing at 400°C for 10 minutes to form a metal oxide layer on the substrate surface.
[0576] The coating, drying, and firing cycle was repeated 60 times. A further firing at 700°C for 1 hour resulted in an adhesion of 505 g / m² on the coated substrate. 2 The metal oxide layer is used to obtain the electrode of Example D12.
[0577] (Method for determining the oxygen overvoltage and double-layer capacitance of the electrodes in the initial stage and after 500 hours of energization)
[0578] The oxygen overvoltage and double-layer capacitance of the electrodes were measured initially and after 500 hours of energization using the same method as in Example A and Comparative Example A described above.
[0579] The evaluation results of Examples D1 to D12 are shown in Table 9.
[0580] (Electrode 1cm after 500 hours of energization) 2 (Method for determining the molar number of La)
[0581] The electrode was subjected to the same method as in Example A and Comparative Example A above after 500 hours of energization, at 1 cm intervals. 2 The number of moles of La was determined.
[0582] The evaluation results of Examples D1 to D12 are shown in Table 9.
[0583] (Calculation method of electrostatic capacitance of electrode per 1 mmol of La after 500 hours of energization)
[0584] The electrostatic capacitance of the electrode per 1 mmol of La after 500 hours of energization was measured using the same method as in Example A and Comparative Example A above.
[0585] The evaluation results of Examples D1 to D12 are shown in Table 9.
[0586] (combustion byproduct gas / LaNi) x M y O 3-z (Calculation method of molar ratio)
[0587] The combustion byproduct gas / LaNi ratio was calculated using the same method as in Example A and Comparative Example A above. x M y O 3-z Molar ratio.
[0588] The evaluation results of Examples D1 to D12 are shown in Table 9.
[0589] (Example D13)
[0590] The following describes the fabrication of an electrolysis unit and a bipolar electrolytic cell for alkaline water electrolysis.
[0591] -anode-
[0592] It is made using the same method as in Example D10.
[0593] -cathode-
[0594] As a conductive substrate, a flat woven mesh substrate is made by weaving nickel wire with a diameter of 0.15 mm into a 40-mesh substrate, and a substrate made by loading platinum on the flat woven mesh substrate is used.
[0595] -Next door, outer frame-
[0596] As a bipolar element, it uses a component with a partition separating the anode and cathode, and an outer frame surrounding the partition. All parts in contact with the electrolyte, such as the partition and the frame of the bipolar element, are made of nickel.
[0597] -Conductive elastomer-
[0598] The conductive elastomer uses the following material: a braided fabric made of nickel wire with a diameter of 0.15 mm, corrugated with a corrugation height of 5 mm.
[0599] -Septum-
[0600] A coating solution with the following composition was obtained using zirconium oxide (trade name "EP Zirconium Oxide", manufactured by Daiichi Rare Element Chemical Co., Ltd.), N-methyl-2-pyrrolidone (manufactured by Wako Pure Chemical Industries, Ltd.), polysulfone ("Udel" (registered trademark), manufactured by Solvay Advanced Polymers Co., Ltd.), and polyvinylpyrrolidone (weight average molecular weight (Mw) 900,000, manufactured by Wako Pure Chemical Industries, Ltd.).
[0601] Polysulfone: 15 parts by weight
[0602] Polyvinylpyrrolidone: 6 parts by weight
[0603] N-Methyl-2-pyrrolidone: 70 parts by weight
[0604] Zirconia: 45 parts by weight
[0605] The above coating solution was applied to both surfaces of a polyphenylene sulfide mesh (manufactured by Clever, 280 μm thick, 358 μm mesh size, 150 μm fiber diameter) serving as the substrate. Immediately after coating, the substrate coated with the solution was exposed to steam, followed by immersion in a coagulation bath to form a coating film on the substrate surface. The coating film was then thoroughly rinsed with pure water to obtain a porous membrane.
[0606] -Gasket-
[0607] The gasket uses a component that is a quadrilateral component with a thickness of 4.0 mm, a width of 18 mm, and an inner dimension of 504 mm square. It has an opening on the inside that is the same size as the electrode chamber when viewed from above, and has a slit structure for holding it in place by inserting a diaphragm.
[0608] -Zero-gap bipolar element-
[0609] The zero-gap battery cell 60 with an external manifold is rectangular, measuring 540mm × 620mm, with the current-carrying surfaces of the anode 2a and cathode 2c having areas of 500mm × 500mm. On the cathode side of the zero-gap bipolar element 60, the cathode 2c, conductive elastomer 2e, and cathode current collector 2r are laminated and connected to the partition wall 1 via the cathode rib 6, forming a cathode chamber 5c through which electrolyte flows. On the anode side, the anode 2a is connected to the partition wall 1 via the anode rib 6, forming an anode chamber 5a through which electrolyte flows. Figure 2 ).
[0610] Depth of anode chamber 5a (anode chamber depth, Figure 2 The distance between the partition wall and the anode is 25mm, and the depth of the cathode chamber is 5c (cathode chamber depth, Figure 2 The distance between the partition wall and the cathode current collector is 25 mm, and the material is nickel. The anode rib 6, which is 25 mm high and 1.5 mm thick, is assembled with the cathode rib 6, which is 25 mm high and 1.5 mm thick, by welding. The resulting nickel partition wall 1 has a thickness of 2 mm.
[0611] As the cathode current collector 2r, a pre-sandblasted nickel mesh substrate is used. The substrate thickness is 1 mm and the aperture ratio is 54%. A conductive elastomer 2e is spot-welded to the cathode current collector 2r for fixation. This zero-gap type bipolar element is stacked with a diaphragm-holding gasket in between, thereby forming a zero-gap structure Z in which the anode 2a and cathode 2c are pressed against the diaphragm 4.
[0612] Using the electrolysis apparatus of Example D13 above, with an electrolyte temperature of 80°C and a current density of 6 kA / m 2 Water electrolysis was performed continuously for 500 hours under positive current. The voltage of each unit in Example D13 was monitored and the voltage shift was recorded. For each unit voltage, the average value of the three units in Example D13 was taken and compared.
[0613] In Example D13, the average overvoltage of the three cells was a low value of 1.71V after 500 hours of operation. Therefore, it can be concluded that the anode of Example D10 achieved a low cell voltage even after prolonged operation.
[0614]
[0615] Industrial applicability
[0616] Because the electrode of the present invention has a large initial double-layer capacitance, the oxygen overvoltage is low after long-term energization, making it suitable as the anode of a water electrolyzer in the electrolysis of alkaline water.
[0617] Symbol Explanation
[0618] 1. Next door
[0619] 2 electrodes
[0620] 2a Anode
[0621] 2c cathode
[0622] 2e Conductive elastomer
[0623] 2r cathode current collector
[0624] 3. Outer frame
[0625] 4. Diaphragm
[0626] 5a Anode Chamber
[0627] 5c Cathode Chamber
[0628] 6 ribs
[0629] 7 gaskets
[0630] 50 Bipolar Electrolyzer
[0631] 51g Fixed head, movable head
[0632] 51i Insulation Board
[0633] 51a Anode Terminal Component
[0634] 51c Cathode Terminal Element
[0635] 51r pull rod
[0636] 60 bipolar components
[0637] 65 Electrolysis Units
[0638] 70 Electrolysis Unit
[0639] 71 Liquid delivery pump
[0640] 72 Gas-Liquid Separator
[0641] 74 Rectifier
[0642] 75 Oxygen Concentration Meter
[0643] 76 Hydrogen Concentration Meter
[0644] 77 Flow Meter
[0645] 78 Pressure gauge
[0646] 79 Heat Exchanger
[0647] 80 Pressure control valve
[0648] Z-zero pole gap structure
Claims
1. An electrode, characterized in that, It has LaNi on the substrate x M y O 3-z The initial double-layer capacitance was greater than 0.6 F / cm. 2 LaNi x M y O 3-z In the LaNi, x+y is 0.8 to 1.2, y is 0.001 to 0.6, z is -0.5 to 0.5, and M contains at least one of Nb, Ta, Sb, Ti, Mn, and Zr. x M y O 3-z The adhesion amount is 350g / m 2 Above and above 3500g / m 2 the following.
2. The electrode as claimed in claim 1, wherein, per 1cm 2 The molar amount of La is between 0.06 mmol and 1.1 mmol.
3. The electrode as described in claim 1 or 2, wherein, The electrostatic capacitance of each mmol of La is between 10F and 25F.
4. The electrode as claimed in claim 1 or 2, wherein, The LaNi x M y O 3-z The position of the main peak in the XRD pattern is between 32.6° and 33.2°.
5. The electrode as claimed in claim 1 or 2, wherein, The LaNi x M y O 3-z The y is greater than 0.002 and less than 0.
2.
6. The electrode as claimed in claim 1 or 2, wherein, The LaNi x M y O 3-z The position of the main peak in the XRD pattern is above 32.7° and below 33.2°.
7. The electrode as claimed in claim 1 or 2, wherein, The LaNi x M y O 3-z M is Nb.
8. The electrode as claimed in claim 1 or 2, wherein, In the LaNi x M y O 3-z A 20μm square region in the layer, larger than 0.785μm. 2 And it is 20μm 2 The total area of the following pores is 10 μm. 2 Above 200μm 2 the following.
9. The electrode as claimed in claim 8, wherein, In the LaNi x M y O 3-z A 20μm square region within the layer, wherein the average pore area is greater than 0.785μm. 2 And it is 10μm 2 the following.
10. The electrode as claimed in claim 8, wherein, In the LaNi x M y O 3-z The 20μm square region in the layer has an average number of pores of more than 20 and less than 150.
11. The electrode as claimed in claim 1 or 2, wherein, x+y is greater than 0.9 and less than 1.
1.
12. The electrode as claimed in claim 1 or 2, wherein, x+y is greater than 1.0 and less than 1.
05.
13. The electrode as claimed in claim 1 or 2, wherein, y is between 0.005 and 0.
15.
14. The electrode as claimed in claim 1 or 2, wherein, y is above 0.01 and below 0.
1.
15. The electrode as claimed in claim 1 or 2, wherein, The initial double-layer capacitance was 1.0 F / cm. 2 above.
16. The electrode as claimed in claim 2, wherein, per 1cm 2 The molar amount of La is between 0.13 mmol and 0.91 mmol.
17. The electrode as claimed in claim 2, wherein, per 1cm 2 The molar amount of La is between 0.15 mmol and 0.68 mmol.
18. The electrode as claimed in claim 3, wherein, The electrostatic capacitance of each mmol of La is between 12F and 23F.
19. The electrode as claimed in claim 3, wherein, The electrostatic capacitance of each mmol of La is between 14F and 21F.
20. The electrode as claimed in claim 1 or 2, wherein, The LaNi x M y O 3-z The adhesion amount is 350g / m 2 Above 3000g / m 2 the following.
21. The electrode as claimed in claim 1 or 2, wherein, The LaNi x M y O 3-z The half-peak width of the main peak in the XRD pattern is above 0.6° and below 0.85°.
22. The electrode as claimed in claim 1 or 2, wherein, The LaNi x M y O 3-z The XRD main peak intensity is above 6,000 and below 20,000.
23. The electrode as claimed in claim 8, wherein, In the LaNi x M y O 3-z A 20μm square region in the layer, larger than 0.785μm. 2 And it is 20μm 2 The total area of the following pores is 20 μm. 2 Above 160μm 2 the following.
24. The electrode as claimed in claim 8, wherein, In the LaNi x M y O 3-z A 20μm square region in the layer, larger than 0.785μm. 2 And it is 20μm 2 The total area of the following pores is 30 μm. 2 Above 130μm 2 the following.
25. The electrode as claimed in claim 9, wherein, In the LaNi x M y O 3-z A 20μm square region within the layer, the average pore area of the micropores is 1.2μm. 2 Above 6.8μm 2 the following.
26. The electrode as claimed in claim 9, wherein, In the LaNi x M y O 3-z A 20μm square region within the layer, the average pore area of the micropores is 3.2μm. 2 Above 4.5μm 2 the following.
27. The electrode of claim 10, wherein, In the LaNi x M y O 3-z The 20μm square region in the layer has an average number of pores of more than 22 and less than 140.
28. The electrode of claim 10, wherein, In the LaNi x M y O 3-z The 20μm square region in the layer has an average number of pores of 29 to 51.
29. The electrode as claimed in claim 1 or 2, wherein, The LaNi x M y O 3-z The porosity in a 20μm square region of the layer is greater than 29% and less than 55%.
30. An electrolysis unit, characterized in that, It is made by using the electrode according to any one of claims 1 to 29 in the anode.
31. A method for producing hydrogen, characterized in that, A variable power source is input into the electrolysis unit as described in claim 30.
32. A method for producing hydrogen, comprising producing hydrogen by electrolyzing water containing alkali in an electrolytic cell, characterized in that, The electrolytic cell includes at least an anode and a cathode, and the anode has a LaNi substrate. x M y O 3-z The initial double-layer capacitance was greater than 0.6 F / cm. 2 LaNi x M y O 3-z In the LaNi, x+y is 0.8 to 1.2, y is 0.001 to 0.6, z is -0.5 to 0.5, and M contains at least one of Nb, Ta, Sb, Ti, Mn, and Zr. x M y O 3-z The adhesion amount is 350g / m 2 Above and above 3500g / m 2 the following.
33. The method for producing hydrogen as described in claim 32, wherein, The anode is the electrode according to any one of claims 2 to 29.
34. A method for preparing an electrode according to any one of claims 1 to 29, characterized in that, It includes a process of calcining a mixture of La(NO3)3, Ni(NO3)2, and compounds having carboxyl and amino groups and with C, H, N, and O as constituent elements, wherein the combustion byproducts generated during the calcination, namely CO2, H2O, and N2, are relative to the LaNi x M y O 3-z The molar ratio, i.e., combustion byproduct gas / LaNi x M y O 3-z It is greater than 5 and less than 12.
6.
35. The method for preparing the electrode as described in claim 34, wherein, Combustion byproduct gas / LaNi x M y O 3-z The value is between 5.3 and 10.
5.
36. A method for preparing an electrode according to any one of claims 1 to 29, characterized in that, It includes a step of calcining a mixture of La(NO3)3, Ni(NO3)2 and glycine, wherein the glycine / NO3 ratio in the mixture is... - The molar ratio is between 0.1 and 0.
3.
37. The method for preparing the electrode as described in claim 36, wherein, glycine / NO3 in the mixture - The molar ratio is between 0.1 and 0.2.
Citation Information
Patent Citations
Positive electrode, positive electrode for water electrolysis, electrolysis cell, and method for producing hydrogen
WO2018155503A1
Positive electrode, positive electrode for water electrolysis, electrolysis cell, and method for producing hydrogen
CN110199055A