Preparation method of self-emulsifying cardanol water phase modified white carbon black and application thereof in rubber
By modifying silica with self-emulsifying cashew phenol, the problems of difficult dispersion of silica in rubber and VOC emissions have been solved, achieving efficient modification and environmentally friendly production of rubber materials and improving the performance of rubber composites.
Patent Information
- Application Number
- CN202311037491.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-08-17
- Publication Date
- 2026-11-10
- Estimated Expiration
- 2043-08-17
AI Technical Summary
Existing aqueous phase modification technologies for silica have problems such as difficulty in dispersion, complex processes, high costs, and serious VOC emissions, which affect the performance of rubber materials and the environment.
Self-emulsifying cashew phenol was used to modify silica in the aqueous phase. By introducing hydrophilic long-chain groups into the cashew phenol structure, it can self-emulsify in the aqueous phase, forming a chemical and physical adsorption structure, which improves the dispersibility of silica in rubber and enhances its performance through cross-linking with rubber.
This method achieves uniform dispersion of silica in rubber, improves the overall performance of rubber materials, reduces rolling resistance and VOC emissions, simplifies the process, and reduces costs.
Smart Images

Figure QLYQS_1 
Figure BDA0004399514780000031 
Figure BDA0004399514780000032
Abstract
Description
Technical Field
[0001] This invention belongs to the field of inorganic nanopowder modification technology, specifically relating to a method for preparing self-emulsifying cashew phenol aqueous phase modified silica and its application in rubber. Background Technology
[0002] Silica, an inorganic nanoparticle, is a white reinforcing agent with a reinforcing effect second only to carbon black. Replacing carbon black with silica as a filler in rubber composites can effectively improve the tear resistance, reduce the loss factor, and decrease rolling resistance. Data shows that tires using silica can reduce rolling resistance by 5-30% compared to using carbon black as a tire filler. For every 3-5% reduction in rolling resistance, fuel consumption can be reduced by 1%. Therefore, rubber / silica composites are ideal materials for preparing "green tire" tread compounds. However, due to its large specific surface area, silica tends to aggregate secondaryly. Furthermore, its high absorbency of moisture from the air leads to strong hydrogen bonding between hydroxyl groups, further increasing particle cohesion. Therefore, dispersing silica in rubber is much more difficult than dispersing carbon black. Moreover, in larger quantities, it easily forms gels, causing the rubber compound to harden and generate more heat.
[0003] To address the aforementioned issues, the common practice in the rubber industry is to use silane coupling agents to modify silica in situ during rubber compounding. This reduces the surface chemical properties of silica, improves its dispersibility in rubber, and maximizes the performance enhancements brought by silica's high specific surface area and high structure. While this method effectively utilizes the advantages of silica and mitigates its disadvantages, it also has significant drawbacks. First, it increases the complexity of the rubber compounding process. To ensure the effectiveness of silane coupling agent modification of silica, compounding often requires higher temperatures and longer compounding times, and the upper limit of the compounding temperature is significantly limited to prevent premature reaction between the coupling agent and the rubber. Second, to ensure the processability of the rubber material, multiple compounding stages must be added. Third, during the compounding modification process, the coupling agent is often affected by the rubber, powder, and processing oil, leading to reduced reaction efficiency, increased consumption, and higher raw material costs. Finally, the extensive use of traditional coupling agents will generate a large amount of VOC emissions during the modification process. If these emissions are not collected and treated in a timely manner, they will not only damage the environment but also corrode the equipment and reduce its lifespan.
[0004] Currently, pre-modifying silica is one of the most effective ways to solve the above problems, and aqueous pre-modification technology, as the most suitable solution for silica production processes, has become a key focus of technological research and development. Since coupling agents commonly used in the rubber industry are generally oily and easily hydrolyzed, a large amount of additives are often needed to help the coupling agent distribute evenly in water to modify silica. However, this approach also has obvious drawbacks. First, the introduction of additives significantly reduces the performance of silica / rubber composites; second, the coupling agent still undergoes significant hydrolysis in water, resulting in waste; and finally, VOC emissions during the modification process are not reduced. These problems significantly increase the cost of wet modification and make technology promotion more difficult.
[0005] Cashew phenol is made from natural cashew shell oil through advanced technology. It has good compatibility with rubber. The unsaturated long-chain alkanes in its molecular structure can cross-link with rubber through the action of sulfur. It has the characteristics of wide availability of raw materials, low cost and good application effect in rubber. Summary of the Invention
[0006] To address the problems existing in current aqueous phase modification technologies for silica, this invention provides a method for preparing self-emulsifying cashew phenol-modified silica and its application in rubber. This invention involves structural modification of cashew phenol to enable it to modify silica in an aqueous phase. Applying the modified silica to rubber not only improves its dispersion but also effectively enhances the overall performance of the rubber through cross-linking with the rubber matrix.
[0007] To achieve the above objectives, the technical solution adopted by the present invention is as follows:
[0008] This invention first provides a method for preparing self-emulsifying cashew phenol aqueous phase modified silica, comprising the following steps:
[0009] 1) Preparation of self-emulsifying cashew nut shell modifier: Add concentrated ammonia to the solvent to adjust the pH to 8-10, add cashew nut shell and formaldehyde and stir thoroughly. Then heat to 70-100℃, reflux and stir for 0.5-3h, add polyethylene glycol (PEG), continue reflux and stir for 0.5-3h, and finally evaporate the solvent to obtain the self-emulsifying cashew nut shell modifier;
[0010] 2) Preparation of water-phase modified silica: Add the self-emulsifying cashew phenol modifier to a silica slurry with a solid content of 5% to 35%, stir and heat to 70 to 100°C, react for 0.5 to 3 hours, and dry the product in an oven or spray dryer to obtain self-emulsifying cashew phenol water-phase modified silica.
[0011] In step 1), the solvent is a mixture of deionized water and an organic solvent, wherein the organic solvent is one or more of methanol, ethanol, acetone, and toluene. The mass ratio of the deionized water to the organic solvent is 1:0.1 to 7.
[0012] In step 1), the cashew phenol is one or a mixture of several of the structural formulas (i), (ii), (iii), and (IV):
[0013]
[0014] In step 1), the chemical formula of polyethylene glycol is HO(CH2CH2O). m H, to ensure the self-emulsification effect of cashew phenol in water, m ≥ 6 in the chemical formula.
[0015] In step 1), the mass ratio of cashew phenol, formaldehyde, and polyethylene glycol is 1:0.1-0.5:1-3.
[0016] In step 2), the mass ratio of the self-emulsifying cashew phenol modifier to the silica in the silica slurry is 0.01 to 0.3:1.
[0017] The present invention also provides the application of self-emulsifying cashew phenol aqueous phase modified silica in rubber, wherein the self-emulsifying cashew phenol aqueous phase modified silica is used to prepare rubber composite materials, the rubber composite materials comprising the following raw materials in parts by weight: 100 parts rubber, 30-120 parts self-emulsifying cashew phenol aqueous phase modified silica, 1-10 parts zinc oxide, 0.25-8 parts stearic acid, 0.5-8 parts antioxidant, 0.1-10 parts sulfur, and 0.1-10 parts accelerator.
[0018] The rubber mentioned is one or more of the following: natural rubber, styrene-butadiene rubber, cis-butadiene rubber, isoprene rubber, butyl rubber, nitrile rubber, ethylene propylene rubber, and silicone rubber.
[0019] This invention employs the above technical solution, introducing hydrophilic long-chain groups into the cashew phenol structure, enabling cashew phenol to self-emulsify in water, thereby achieving aqueous surface modification of precipitated silica. The resulting self-emulsifying cashew phenol-modified precipitated silica not only blends well with rubber, but also, due to the removal of some hydroxyl groups on the precipitated silica surface, reduces the cohesive force between precipitated silica particles, resulting in more uniform dispersion of precipitated silica in rubber and significantly improving the overall performance of rubber products. Specifically, the beneficial effects of this invention are as follows:
[0020] 1. This invention introduces an active group at the ortho position of cashew nut shell powder via hydroxymethylation, and then introduces a long polyethylene glycol chain with good hydrophilic properties into the cashew nut shell powder structure through a condensation reaction between the active group and PEG molecules, thereby enabling the cashew nut shell powder to self-emulsify in an aqueous phase. The reaction process is as follows:
[0021]
[0022] 2. In an aqueous phase, the self-emulsifying cashew phenol synthesized according to this invention is used to modify silica. The hydroxyl groups at the ends of the hydrophilic long chain of cashew phenol can condense with the hydroxyl groups on the surface of silica to form a chemical grafting structure; at the same time, the oxygen atoms in the hydrophilic long chain of cashew phenol can also form hydrogen bonds with the hydroxyl groups on the surface of silica to form a physical adsorption structure. The above effects achieve the surface modification of silica.
[0023] 3. When the self-emulsifying cashew phenol aqueous phase modified silica synthesized in this invention is used in rubber materials, the aggregation tendency of the silica surface is weakened due to the organic modification, thus enhancing its compatibility with rubber and achieving good dispersion of silica in the rubber matrix. Simultaneously, the unsaturated long-chain hydrocarbons of the self-emulsifying cashew phenol can crosslink with rubber through the action of sulfur, thereby constructing a bridging effect between silica and rubber, enhancing the interaction between them, significantly reducing the rolling resistance of rubber composites, and improving the dynamic and static mechanical properties of rubber composites. Furthermore, the reaction product in the self-emulsifying cashew phenol modified silica process is only water, without the generation of other small organic molecules, which is of great help in reducing VOC emissions during silica modification.
[0024] 4. Compared with the traditional method of modifying silica with silane coupling agents, self-emulsifying cashew phenol can modify silica in the aqueous phase. The process is compatible with the production process of silica and has the characteristics of mild reaction conditions, low cost and suitability for large-scale production.
[0025] 5. The cashew phenol described in this invention is a natural phenolic compound extracted from cashew shells, which are agricultural and forestry residues. It is one of the most commonly used renewable resources and has the unique advantages of being renewable, inexpensive, and abundant. Detailed Implementation
[0026] The present invention will be further described in detail below with reference to the embodiments.
[0027] The endpoints and any values of the ranges disclosed herein are not limited to the precise ranges or values, and these ranges or values should be understood to include values close to these ranges. For numerical ranges, the endpoint values of the various ranges, the endpoint values of the various ranges and individual point values, and individual point values can be combined with each other to obtain one or more new numerical ranges, which should be considered as specifically disclosed in this invention.
[0028] All raw materials used in the examples are commercially available products.
[0029] Example 1
[0030] The preparation method of self-emulsifying cashew phenol aqueous phase modified silica includes the following steps:
[0031] 1) Mix deionized water and ethanol at a mass ratio of 1:2 until homogeneous. Adjust the pH to 9±0.3 with concentrated ammonia. Add cashew nut powder and formaldehyde at a mass ratio of 1:0.2. Stir thoroughly and heat to 85℃. Reflux and stir for 0.5h. Add PEG-300 at a mass ratio of 1:1 with cashew nut powder. Continue to reflux and stir for 2.5h. Then evaporate the solvent to dryness to obtain the self-emulsifying cashew nut powder modifier.
[0032] 2) Add 8% by weight of self-emulsifying cashew phenol modifier to a 10% solid content slurry of silica, stir and heat to 85°C, react for 1.5 h, and then place the product in a spray dryer to dry, to obtain self-emulsifying cashew phenol aqueous phase modified silica.
[0033] Example 2
[0034] The preparation method of self-emulsifying cashew phenol aqueous phase modified silica includes the following steps:
[0035] 1) Mix deionized water and ethanol at a mass ratio of 1:2 until homogeneous. Adjust the pH to 9±0.3 with concentrated ammonia. Add cashew nut powder and formaldehyde at a mass ratio of 1:0.2. Stir thoroughly and heat to 85℃. Reflux and stir for 0.5h. Add PEG-600 at a mass ratio of 1:1 with cashew nut powder. Continue to reflux and stir for 2.5h. Then evaporate the solvent to dryness to obtain the self-emulsifying cashew nut powder modifier.
[0036] 2) Add 8% by weight of self-emulsifying cashew phenol modifier to a 10% solid content slurry of silica, stir and heat to 85°C, react for 1.5 h, and then place the product in a spray dryer to dry, to obtain self-emulsifying cashew phenol aqueous phase modified silica.
[0037] Example 3
[0038] The preparation method of self-emulsifying cashew phenol aqueous phase modified silica includes the following steps:
[0039] 1) Mix deionized water and ethanol at a mass ratio of 1:2 until homogeneous. Adjust the pH to 9±0.3 with concentrated ammonia. Add cashew nut powder and formaldehyde at a mass ratio of 1:0.2. Stir thoroughly and heat to 85℃. Reflux and stir for 0.5h. Add PEG-1000 at a mass ratio of 1:1 with cashew nut powder. Continue to reflux and stir for 2.5h. Then evaporate the solvent to dryness to obtain the self-emulsifying cashew nut powder modifier.
[0040] 2) Add 8% by weight of self-emulsifying cashew phenol modifier to a 10% solid content slurry of silica, stir and heat to 85°C, react for 1.5 h, and then place the product in a spray dryer to dry, to obtain self-emulsifying cashew phenol aqueous phase modified silica.
[0041] Example 4
[0042] The preparation method of self-emulsifying cashew phenol aqueous phase modified silica includes the following steps:
[0043] 1) Mix deionized water and ethanol at a mass ratio of 1:2 until homogeneous. Adjust the pH to 9±0.3 with concentrated ammonia. Add cashew nut powder and formaldehyde at a mass ratio of 1:0.2. Stir thoroughly and heat to 85℃. Reflux and stir for 0.5h. Add PEG-2000 at a mass ratio of 1:1 with cashew nut powder. Continue to reflux and stir for 2.5h. Then evaporate the solvent to dryness to obtain the self-emulsifying cashew nut powder modifier.
[0044] 2) Add 8% by weight of self-emulsifying cashew phenol modifier to a 10% solid content slurry of silica, stir and heat to 85°C, react for 1.5 h, and then place the product in a spray dryer to dry, to obtain self-emulsifying cashew phenol aqueous phase modified silica.
[0045] Example 5
[0046] Application of self-emulsifying cashew nut shell aqueous phase modified silica in rubber materials
[0047] To verify the effectiveness of self-emulsifying cashew phenol-modified silica in rubber, an experiment was conducted to demonstrate its effectiveness:
[0048] Test Sample 1: The cashew phenol-modified silica prepared in Example 1 was compounded with other components in the rubber composite material formulation to obtain Test Sample 1.
[0049] Test Sample 2: The cashew phenol-modified silica prepared in Example 2 was compounded with other components in the rubber composite material formulation to obtain Test Sample 2.
[0050] Test Sample 3: The cashew phenol-modified silica prepared in Example 3 was combined with other components in the rubber composite material formulation to obtain Test Sample 3.
[0051] Test Sample 4: The cashew phenol-modified silica prepared in Example 4 was combined with other components in the rubber composite material formulation to obtain Test Sample 4.
[0052] Control Sample 1: Control Sample 1 was obtained by combining silica with other components in the rubber composite material formulation.
[0053] Control Sample 2: Control Sample 2 was prepared by combining silica, cashew phenol, and other components in the rubber composite material formulation. The PEG in the formulation of Control Sample 2 was PEG-300.
[0054] The experimental formulations for the test and control samples are shown in Table 1, where phr represents parts by weight.
[0055] Table 1 Rubber Material Formulation
[0056]
[0057]
[0058] The preparation methods of the rubber composite materials in Table 1 are all carried out according to the following steps:
[0059] (1) First stage mixing: Add the formulation components (except sulfur, DPG, CZ, TBzTD) into the internal mixer. After the rubber compound is mixed to 145℃ in the internal mixer, continue to maintain the rubber compound at 145℃ at a speed of 3-15 rpm for another 5 minutes, and then discharge the rubber to obtain the first stage masterbatch;
[0060] (2) Two-stage mixing: After cooling and standing for 24 hours, the first-stage masterbatch is mixed in an internal mixer to 148°C. The mixture is then kept at 148°C at a speed of 3-15 rpm for another 5 minutes. The mixture is then discharged to obtain the second-stage masterbatch.
[0061] (3) Three-stage mixing: The second-stage masterbatch rubber that has been cooled and left to stand for 4 hours is added together with sulfur, DPG, CZ and TBzTD into a mixer. The rubber compound is then mixed in the mixer to a temperature of 110℃ to obtain the test rubber composite material.
[0062] The performance of the test sample and the control sample was tested, and the results are shown in Table 2.
[0063] Table 2 Performance Tests of Rubber Composite Materials
[0064]
[0065] Test sample 1 was prepared by pre-processing self-emulsified cashew phenol aqueous phase modified silica using the preparation method of this invention, and then compounding it with other rubber components. Control sample 1 was prepared by compounding Si-69, a silane coupling agent commonly used in the tire industry, silica, and other rubber components. Performance testing of the rubber composites revealed that test sample 1 showed improvements in tensile strength, elongation at break, and tear strength compared to control sample 1, indicating better mechanical properties and tear resistance. Furthermore, test sample 1 exhibited higher tanδ0℃ and lower tanδ60℃ than control sample 1, indicating better wet grip and lower rolling resistance. The Akron abrasion test showed that test sample 1 performed worse than control sample 1, demonstrating better abrasion resistance. The data comparison demonstrates that rubber materials using cashew phenol modified silica have superior performance compared to Si-69 system rubber materials, resulting in tires with better wet grip, lower rolling resistance, and improved abrasion resistance.
[0066] Both Test Sample 1 and Control Sample 2 used cashew nut shell powder and PEG-300 modified silica. However, Test Sample 1 was prepared using the method of this invention to pre-process self-emulsifying cashew nut shell powder with an aqueous phase, while Control Sample 2 was obtained by directly mixing cashew nut shell powder, PEG-300, and silica with other rubber components in a mixer. Testing revealed that Test Sample 1 exhibited better tensile strength, elongation at break, and tear strength than Control Sample 2. Furthermore, Test Sample 1 showed higher tanδ0℃, lower tanδ60℃, and a lower Akron abrasion index compared to Control Sample 2. These trends in the properties of the rubber composites clearly demonstrate that using self-emulsifying cashew nut shell powder modified silica yields superior rubber composite properties compared to directly mixing cashew nut shell powder, PEG-300, and silica with other rubber components.
[0067] Self-emulsifying cashew nut shells with different hydrophilic groups were prepared using PEG with relative molecular masses of 300, 600, 1000, and 2000. These were then applied to test samples 1 through 4 to obtain different self-emulsifying cashew nut shell aqueous-phase modified silica rubber composites. The different molecular weights of the hydrophilic groups not only affected the self-emulsifying ability of cashew nut shells in the aqueous phase but also significantly impacted the surface modification effect of silica. Table 2 shows that the hardness, tensile strength, stress at a given elongation, and elongation at break indicate that as the molecular weight of the hydrophilic groups in the self-emulsifying cashew nut shells increases, the rubber composites exhibit a certain plasticizing trend, and the Akron abrasion index decreases accordingly. However, the change in the molecular weight of the hydrophilic groups in the self-emulsifying cashew nut shells has a relatively smaller effect on tanδ0℃ and tanδ60℃, with tanδ60℃ showing a decreasing trend. This indicates that different self-emulsifying cashew nut shells prepared using PEG with different molecular weights all possess good wet grip and rolling resistance in tires.
[0068] The preferred embodiments of the present invention have been described in detail above; however, the present invention is not limited thereto. Within the scope of the inventive concept, various simple modifications can be made to the technical solutions of the present invention, including combinations of various technical features in any other suitable manner. These simple modifications and combinations should also be considered as the content disclosed in the present invention and are all within the protection scope of the present invention.
Claims
1. A method for preparing self-emulsifying cashew phenol aqueous phase modified silica, characterized in that, Includes the following steps: 1) Adjust the pH of the solvent to 8-10, add cashew nut powder and formaldehyde to the solvent and stir thoroughly. Then heat to 70-100℃, reflux and stir for 0.5-3h, add polyethylene glycol, continue to reflux and stir for 0.5-3h, and finally evaporate the solvent to obtain the self-emulsifying cashew nut powder modifier. The solvent is a mixture of water and an organic solvent in a mass ratio of 1:0.1~7, wherein the organic solvent is one or more of methanol, ethanol, acetone, and toluene; The mass ratio of cashew phenol, formaldehyde, and polyethylene glycol is 1:0.1~0.5:1~3; 2) Add the self-emulsifying cashew phenol modifier to a 5%~35% solid content slurry of silica, stir and heat to 70~100℃, react for 0.5~3h, and dry the product to obtain self-emulsifying cashew phenol aqueous phase modified silica.
2. The method for preparing self-emulsifying cashew phenol aqueous phase modified silica according to claim 1, characterized in that, In step 1), the cashew phenol is one or a mixture of several of the structural formulas (i), (ii), (iii), and (IV): 。 3. The method for preparing self-emulsifying cashew phenol aqueous phase modified silica according to claim 1, characterized in that, In step 1), the chemical formula of polyethylene glycol is HO(CH2CH2O). m H, to ensure the self-emulsification effect of cashew phenol in water, m ≥ 6 in the chemical formula.
4. The method for preparing self-emulsifying cashew phenol aqueous phase modified silica according to claim 1, characterized in that, In step 2), the mass ratio of the self-emulsifying cashew phenol modifier to the silica in the silica slurry is 0.01~0.3:
1.
5. A self-emulsifying cashew phenol aqueous phase modified silica obtained by the preparation method according to any one of claims 1 to 4.
6. The application of self-emulsifying cashew phenol aqueous phase modified silica as described in claim 5 in rubber, characterized in that, The self-emulsifying cashew phenol aqueous phase modified silica is used to prepare rubber composite materials, which include the following raw materials in parts by weight: 100 parts rubber, 30-120 parts self-emulsifying cashew phenol aqueous phase modified silica, 1-10 parts zinc oxide, 0.25-8 parts stearic acid, 0.5-8 parts antioxidant, 0.1-10 parts sulfur, and 0.1-10 parts accelerator.
7. The application according to claim 6, characterized in that, The rubber mentioned is one or more of the following: natural rubber, styrene-butadiene rubber, cis-butadiene rubber, isoprene rubber, butyl rubber, nitrile rubber, ethylene propylene rubber, and silicone rubber.
Citation Information
Patent Citations
Method for preparing anacardol polyoxyethylene ether
CN103449983A
Rubber composite material using cardanol glycidyl ether modified silica and preparation method thereof