Composite conductive aerogel and preparation method and application thereof
MXenes-based composite conductive aerogels were prepared by electrospinning and heat treatment, which solved the problem of insufficient mechanical strength of MXenes aerogel materials and realized a composite material with high conductivity and compressibility, suitable for flexible electronic devices.
Patent Information
- Application Number
- CN202210397372.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-04-15
- Publication Date
- 2025-12-09
- Estimated Expiration
- 2042-04-15
AI Technical Summary
Existing MXenes aerogel materials have poor mechanical strength and lack elasticity, which limits their application in the field of flexible devices.
By dispersing carbon nanotubes and polyacrylonitrile into a composite fiber membrane through electrospinning, and combining it with MXenes materials and graphene oxide nanoribbons, a composite conductive aerogel with a three-dimensional interconnected porous network was prepared through freeze-thaw crosslinking and heat treatment.
The prepared composite conductive aerogel has high conductivity, compressibility and low specific gravity, making it suitable for flexible wearable electronics, energy and sensing fields.
Smart Images

Figure CN116943551B_ABST
Abstract
Description
TECHNICAL FIELD
[0001] The present application belongs to the field of preparation of conductive composite materials, and particularly relates to a composite conductive aerogel and a preparation method and application thereof. BACKGROUND
[0002] Mxenes (i.e., two-dimensional transition metal carbides, nitrides or carbonitrides) is a new type of layered two-dimensional material similar to graphene, which has a wide application prospect in the fields of biomedical, energy storage, catalysis and flexible electronics due to its high electrical conductivity, good hydrophilicity and excellent photo-thermal conversion characteristics.
[0003] To enrich the product form of Mxenes, two-dimensional Mxenes can be converted into three-dimensional aerogel materials by freeze-drying method, but the interaction (hydrogen bond) between MXenes is weak, the mechanical strength of single Mxenes aerogel material is poor, and it does not have any elasticity, which limits its application in the field of flexible devices. Therefore, it is necessary to provide a MXenes-based conductive aerogel material. SUMMARY
[0004] In view of this, the present application provides a MXenes-based composite conductive aerogel which takes into account high conductivity, high elasticity and ultra-light characteristics, and a preparation method and application thereof.
[0005] In a first aspect, the present application provides a preparation method of a composite conductive aerogel, comprising the following steps:
[0006] (1) dispersing carbon nanotubes and polyacrylonitrile in a first solvent to obtain a spinning solution; electrospinning the spinning solution to obtain a composite fiber membrane;
[0007] cutting the composite fiber membrane and placing it in a second solvent to obtain a colloidal solution containing polyacrylonitrile / carbon nanotube composite nanofibers by shearing;
[0008] (2) mixing the colloidal solution with MXenes material and graphene oxide nanoribbons, and performing freeze-thaw cycle treatment on the obtained mixed solution to occur physical crosslinking to obtain a composite hydrogel; freeze-drying the composite hydrogel to obtain a composite aerogel;
[0009] (3) pre-oxidizing the composite aerogel at 200-300℃ under an oxygen-containing atmosphere, and then carbonizing the composite aerogel at 700-1000℃ under a non-oxidizing atmosphere to obtain a composite conductive aerogel containing MXenes, carbon fibers, carbon nanotubes and graphene nanoribbons.
[0010] In the spinning solution in step (1), the mass ratio of the polyacrylonitrile to the carbon nanotube is 100:(1-5). The mass ratio of the polyacrylonitrile to the first solvent is 100:(5-15). In this way, the spinning solution can have a suitable viscosity, and the preparation efficiency of the composite fiber film obtained by spinning can be improved. In some embodiments, the mass ratio of the polyacrylonitrile to the ionic liquid-modified carbon nanotube is 100:(1-3), for example, 100:1.5, 100:2, 100:2.5; and the mass ratio of the polyacrylonitrile to the first solvent is 100:(5-10), for example, 100:6, 100:8, etc. The surface of the carbon nanotube can be without a modification layer or can have a modification layer (such as an ionic liquid modification layer) to facilitate the dispersion of the carbon nanotube in the first solvent.
[0011] In the spinning solution in step (1), the mass ratio of the polyacrylonitrile to the carbon nanotube is 100:(1-5). The mass ratio of the polyacrylonitrile to the first solvent is 100:(5-15). In this way, the spinning solution can have a suitable viscosity, and the preparation efficiency of the composite fiber film obtained by spinning can be improved. In some embodiments, the mass ratio of the polyacrylonitrile to the ionic liquid-modified carbon nanotube is 100:(1-3), for example, 100:1.5, 100:2, 100:2.5; and the mass ratio of the polyacrylonitrile to the first solvent is 100:(5-10), for example, 100:6, 100:8, etc. The surface of the carbon nanotube can be without a modification layer or can have a modification layer (such as an ionic liquid modification layer) to facilitate the dispersion of the carbon nanotube in the first solvent.
[0012] In some embodiments of the present application, the electrospinning can be performed under the following conditions: the spinning voltage is 5-10 kV, the rotation speed of the fiber receiving device is 200-1000 rpm, the spinning distance is 5-10 cm, and the spinning time is 20-60 minutes. The fiber receiving device can be a roller for carrying the composite fiber film formed by the spinning solution. The spinning distance refers to the distance between the spinning needle head outputting the spinning solution and the fiber receiving device. Further, the composite fiber film obtained by spinning in step (1) can also be subjected to a drying treatment to remove the second solvent therefrom. The drying treatment can be performed at 100-120°C for 24-48 h under vacuum drying.
[0013] In step (1), the spinning solution containing polyacrylonitrile and carbon nanotubes is subjected to electrospinning, and the obtained composite fiber film includes a spinning film matrix formed by polyacrylonitrile fibers and carbon nanotubes coated therein. After being cut and sheared in a solvent, the composite fiber film is dissociated into polyacrylonitrile / carbon nanotube composite nanofibers that can be fully dispersed in the solvent. The composite nanofibers include carbon nanotubes and polyacrylonitrile fibers, and the polyacrylonitrile fibers wrap the carbon nanotubes.
[0014] Optionally, the polyacrylonitrile / carbon nanotube composite nanofiber has a diameter of 50-100 nm and a length of 1-10 μm. Optionally, the shearing speed can be 10,000-30,000 rpm, and the shearing time can be 5-60 min. A higher shearing speed is conducive to fully dissociating the entire composite fiber membrane into individual composite fibers. The shearing time can be adjusted according to the size of the composite fiber membrane. Optionally, the second solvent comprises a mixture of water and an alcohol solvent. The alcohol solvent can be t-butyl alcohol or a mixture of t-butyl alcohol and other alcohols (isobutyl alcohol, isopropyl alcohol, ethylene glycol, ethanol, etc.). Optionally, the mass ratio of water to alcohol solvent can be 100:20. The above composite fibers have good dispersibility in the second solvent containing water. Optionally, the concentration of the composite nanofiber in the colloidal solution is 2-10 mg / mL.
[0015] In step (2), the mass ratio of the MXenes material, the polyacrylonitrile / carbon nanotube composite nanofiber, and the graphene oxide nanoribbon is 100:(5-100):(10-100), preferably 100:(10-90):(50-90), for example, 100:60:60, 100:40:80, 100:20:50, etc. Controlling the mass ratio of the composite nanofiber to the MXenes material in the above range is conducive to the final product having good electrical conductivity and mechanical properties.
[0016] In step (2), when preparing the mixed solution for forming the composite hydrogel, the MXenes material and the graphene oxide nanoribbon can be added in solid form or in the form of a solution containing them. In some embodiments of the present application, the mixed solution of step (2) is obtained by mixing the colloidal solution with an aqueous solution of the MXenes material and an aqueous solution of the graphene oxide nanoribbon. The mixing can be performed by stirring at a speed of 10,000-30,000 rpm for 1-5 min. Optionally, the concentration of the aqueous solution of the MXenes material is 4-10 mg / mL. The concentration of the aqueous solution of the graphene oxide nanoribbon is 2-10 mg / mL.
[0017] In the present application, the chemical formula of MXenes is M n+1 X n T x , wherein M is a transition metal element, X is a carbon element and / or a nitrogen element, n is an integer of 1-3, and T x represents a surface group, and T can be selected from at least one of O 2- , OH - , F - , and NH4 + . Further, the MXenes material can be Ti3C2Tx Ti2CT x (Ti 0.5 Nb 0.5 )2CT x (V 0.5 Cr 0.5 )3C2T x Ta4C3T x V2CT x Nb2CT x Nb4C3T x (Nb 0.8 Ti 0.2 )4C3T x (Nb 0.8 Zr 0.2 )4C3T x Ti3CNT x Mo2TiC2T x Mo2Ti2C3T x and Cr2TiC2T x The above MXenes are two-dimensional layered materials with a nanometer thickness, which can be referred to as "MXenes nanosheets". The number of layers of the MXenes material is 1-20 layers. Further preferably, the number of layers is 2-10 layers. Preferably, the thickness of the MXenes material is 6-10 nm. Alternatively, the lateral size of the MXenes material can be 60-200 nm. The lateral size refers to the length or width of the two-dimensional layered material.
[0018] In the present application, the preparation method of the MXenes material used in step (2) is not limited, which can be obtained by acid etching, high-temperature etching or gas-phase etching of the A element (such as Al element) in the precursor material MAX (M represents a transition metal element, A is usually Al or Si, and X includes C, N or C and N elements). Taking Ti3AlC2 as an example, a preparation method of MXenes is shown as follows, which specifically includes the following steps:
[0019] 1) slowly add Ti3AlC2 powder into a mixed solution of lithium fluoride (NaF) and concentrated hydrochloric acid (HCl) prepared in advance, and carry out etching reaction at a temperature of 25-50°C for 16-48 hours; after the reaction is completed, centrifuge, wash the obtained reaction liquid, and collect the solid precipitate until the centrifugal liquid is neutral or close to neutral;
[0020] 1) mix the solid precipitate with an intercalation agent (such as ethanol), and perform ultrasonic peeling in deionized water to obtain an aqueous solution containing MXenes material by centrifugation.
[0021] In the present application, the preparation method of graphene oxide nanoribbons used in step (2) is not limited, and it can be prepared by a chemical cutting method. An exemplary preparation method of graphene oxide nanoribbons includes the following steps:
[0022] a) mixing dry single-walled carbon nanotubes and concentrated sulfuric acid, wherein the mass-volume ratio of carbon nanotubes to concentrated sulfuric acid is 1 g: 150-200 mL, reacting at room temperature for 60-180 minutes, and then adding 10-50 mL of phosphoric acid and continuing to stir for 5-30 minutes;
[0023] b) adding potassium permanganate to the mixed solution of 2-a) in batches and continuing to react; wherein the mass ratio of potassium permanganate to carbon nanotubes is 100:5-20, the reaction temperature is 30-80°C, and the reaction time is 60-180 minutes; finally, a brown-red reaction solution is obtained;
[0024] c) after the temperature of the above reaction solution decreases to room temperature, it is added to a hydrogen peroxide / ice water mixture and left overnight; wherein the volume ratio of ice water to hydrogen peroxide is 100:1-5, and the concentration of the hydrogen peroxide used is 10wt%; subsequently, graphene oxide nanoribbons are obtained by filtration and washing, and dispersed in deionized water to obtain an aqueous solution of graphene oxide nanoribbons.
[0025] In step (2), the mixed solution of the colloidal solution and the MXenes material and graphene oxide nanoribbons can be physically cross-linked by freeze-thaw cycle treatment to form a composite hydrogel containing MXenes material, graphene oxide nanoribbons, and polyacrylonitrile / carbon nanotube composite nanofibers. After freeze-drying, a conductive network of MXenes material, graphene nanoribbons, and carbon nanotube / carbon fiber composite nanofibers is obtained.
[0026] In step (2), the freeze-thaw cycle process includes first placing the mixed solution of the colloidal solution and the MXenes material and graphene oxide nanoribbons on a hard substrate pre-cooled with liquid nitrogen (e.g., at a temperature of -80°C), and then freezing in a freezer at -5 to -20°C. Then, thawing is performed at room temperature. The above freezing and thawing processes are repeated multiple times. Before freezing, the precursor solution for forming the composite hydrogel is first placed on a hard substrate pre-cooled with liquid nitrogen, which can guide the precursor solution to perform "oriented freezing" to achieve oriented "physical cross-linking" in a freezing device with a higher temperature than the hard substrate, which is beneficial to improving the mechanical properties of the obtained composite hydrogel and ensuring the coherence and order of the gel network structure.
[0027] Optionally, the number of cycles of the freeze-thaw treatment is 3-10, preferably 5-8, for example 6, 7. Optionally, the total length of the freezing process and the total length of the thawing process are respectively in the range of 5-24h, preferably in the range of 12-20h, for example 14h, 18h, etc. The hard substrate can be a metal plate such as a copper plate, or other materials that can withstand low temperature. The freezer can be a refrigerator, a freezer, etc. with freezing function.
[0028] Optionally, after obtaining the composite hydrogel, it can be placed in deionized water for dialysis treatment, and then freeze-dried. The main purpose of the dialysis treatment is to remove the second solvent and purify the hydrogel. Optionally, the dialysis can be carried out at a temperature of 4-10℃, and the dialysis time can be 48-72h. The temperature for freeze-drying the composite hydrogel can be -20 to -80℃, for example -20 to -40℃; the freeze-drying time can be 24-96h, for example 48-96h, further can be 48-72h.
[0029] Optionally, in step (3), the pre-oxidation treatment time is 30-120min; the pre-oxidation treatment rate (referring to the rate from room temperature to the pre-oxidation temperature (200-300℃)) is 1-5℃ / min. Pre-oxidation can improve the electrical conductivity of the final product. The oxygen-containing atmosphere can be air or oxygen, and air is preferred due to its lower price.
[0030] Optionally, the carbonization treatment time is 1-5h; the carbonization treatment rate (from room temperature to the carbonization treatment temperature) is 1-5℃ / min. Preferably, the carbonization treatment temperature is 800-900℃. The carbonization treatment is mainly to carbonize the polypropylene fibers in the composite aerogel to form high-conductive carbon fibers, so as to obtain a conductive composite material with good electrical conductivity; in addition, the graphene oxide nanobelt in the composite aerogel is also reduced to graphene nanobelt during the carbonization treatment. Optionally, the non-oxidizing atmosphere includes one or more of argon (Ar), helium (He), nitrogen (N2), hydrogen (H2), carbon monoxide (CO).
[0031] Optionally, the surface of the carbon fiber has a porous structure. The porous structure can be formed during the carbonization treatment in the aforementioned preparation method.
[0032] The preparation method of the above MXenes-based composite conductive aerogel provided in the application includes the following steps: dissolving a spinning film formed by electrospinning of carbon nanotubes and polypropylene into single composite nanofibers, cross-linking the composite nanofibers with MXenes material and graphene nanoribbon to form an aerogel material, and preparing the carbon fiber-carbon nanotube / MXenes / graphene nanoribbon composite conductive aerogel after pre-oxidation and carbonization. The composite conductive aerogel is expected to be applied in the fields of flexible wearable electronics, energy, sensing, environment, etc. The preparation method has the advantages of simple process, easy operation, low cost, high yield and easy industrialization.
[0033] The application further provides a composite conductive aerogel, which comprises MXenes material, graphene nanoribbon and composite fiber material, and has a three-dimensional interconnected porous network. The composite fiber material comprises carbon nanotubes and carbon fibers, and the carbon fibers wrap the carbon nanotubes.
[0034] In the application, the outer surface of the carbon nanotubes is coated with carbon fibers, and the two form a core-shell structure. The carbon nanotubes have better conductivity than the carbon fibers, and the core-shell structure can further improve the conductivity of the carbon fibers. The carbon fibers on the outer layer of the composite fibers have certain toughness, which is beneficial to contact and entanglement with the MXenes material and the graphene nanoribbon. The two-dimensional MXenes material, the quasi-one-dimensional graphene nanoribbon and the one-dimensional composite fiber material interpenetrate to form the three-dimensional interconnected porous network and enrich the multi-order nature of the network. The conductivity of the quasi-one-dimensional graphene nanoribbon and the electrical conductivity of the carbon fibers are higher than those of the MXenes material. The introduction of the graphene nanoribbon and the carbon fibers can significantly reduce the contact resistance between the MXenes, and the graphene nanoribbon can also reduce the contact resistance between the MXenes and the carbon fibers, thereby giving the overall composite conductive aerogel good conductivity. In addition, the density of the carbon fibers and the carbon nanotubes is low, and the toughness of the two is higher than that of the MXenes. In particular, the toughness of the carbon nanotubes is better, and the toughness of the graphene nanoribbon is also good. The presence of the carbon fibers and the carbon nanotubes can make the specific gravity of the composite conductive aerogel small, and give it certain toughness, so that it has certain compressibility and is beneficial to its application in flexible devices. Therefore, the above MXenes-based composite conductive aerogel has good conductivity, compressibility and low specific gravity.
[0035] Optionally, in the composite conductive aerogel, the mass percentage of the MXenes material is 33.33%-86.96%, the mass percentage of the graphene nanoribbon is 4.76%-48.78%, and the mass percentage of the composite fiber material is 2.44%-47.62%. Further, in the composite conductive aerogel, the mass percentage of the carbon nanotubes is 0.024%-2.27%, and the mass percentage of the carbon fibers is 2.32%-45.35%.
[0036] The above composite conductive aerogel provided by the present application enriches the product form of MXenes and has good conductivity, compressibility and light specific gravity as described above, and is expected to be applied in the fields of energy (solar cells, lithium ion batteries, aluminum ion batteries, etc.), optoelectronics, photothermal, electromagnetic shielding, sensing, etc.
[0037] The present application also provides the application of the above composite conductive aerogel in batteries, optoelectronic devices, photothermal devices, sensors, electromagnetic shielding devices.
[0038] The battery includes electrochemical batteries (such as lithium ion batteries, aluminum ion batteries, sodium secondary batteries, potassium secondary batteries, magnesium secondary batteries, zinc secondary batteries, etc.), solar cells, etc.
[0039] Further, the MXenes-based composite conductive aerogel can be used as an electrode or a conductive agent in a battery, an optoelectronic device, a photothermal device, a sensor, etc. In particular, the above battery, optoelectronic device, photothermal device, sensor, etc. can be flexible, and they can be used in flexible wearable devices. BRIEF DESCRIPTION OF DRAWINGS
[0040] Figure 1 Macro photograph of the MXenes / composite fiber / graphene nanoribbon conductive aerogel prepared in Example 1 of the present application.
[0041] Figure 2 Macro photograph of the pure MXenes aerogel material prepared in Comparative Example 1.
[0042] Figure 3 Macro photograph of the MXenes / composite fiber conductive aerogel material prepared in Comparative Example 2,
[0043] Figure 4 Macro photograph of the MXenes / graphene nanoribbon conductive aerogel prepared in Comparative Example 3. DETAILED DESCRIPTION
[0044] The following is an exemplary embodiment of the present application. It should be noted that for those skilled in the art, without departing from the principles of the present application, a number of improvements and refinements can be made, which are also considered within the scope of protection of the present application.
[0045] The present application will be further described in the following embodiments. Unless otherwise specified, the raw materials and other chemical reagents used in the present application are commercially available.
[0046] The preparation method of the MXenes material used in the following examples and comparative examples can specifically include the following steps:
[0047] The Ti3AlC2 powder is slowly added into a mixed solution of lithium fluoride (NaF) and concentrated hydrochloric acid (HCl) which has been prepared in advance, and the etching reaction is carried out at a temperature of 30℃ for 24 hours. The obtained reaction solution is centrifuged, washed, and the solid precipitate is collected until the centrifuged solution is neutral or close to neutral.
[0048] Then the solid is mixed with an intercalation agent-ethanol, and then ultrasonic exfoliation is carried out in deionized water, and an aqueous solution of MXenes material (specifically Ti3C2T x nanosheets) with a concentration of 4-10 mg / mL is obtained by centrifugation.
[0049] The preparation method of the graphene oxide nanobelt used in the following examples and comparative examples can specifically include the following steps:
[0050] a) dry single-walled carbon nanotubes and concentrated sulfuric acid are mixed, wherein the mass-volume ratio of carbon nanotubes to concentrated sulfuric acid is 1 g:180 mL, and the reaction is carried out at room temperature for 120 minutes, and then 30 mL of phosphoric acid is added and stirring is continued for 15 minutes;
[0051] b) potassium permanganate is added to the above-mentioned mixed solution in batches, and the reaction is continued; wherein the mass ratio of potassium permanganate to carbon nanotubes is 100:10, the reaction temperature is 60℃, and the reaction time is 120 minutes; finally, a brown-red reaction solution is obtained;
[0052] c) after the temperature of the above-mentioned reaction solution decreases to room temperature, it is added to a hydrogen peroxide / ice water mixture and left to stand overnight; wherein the volume ratio of ice water to hydrogen peroxide is 100:3, and the concentration of the hydrogen peroxide used is 10wt%; then, the graphene oxide nanobelt is obtained by filtration and washing, and dispersed in deionized water to obtain an aqueous solution of graphene oxide nanobelt with a concentration of 5mg / mL.
[0053] Example 1
[0054] A preparation method of a composite conductive aerogel, comprising the following steps:
[0055] (1) preparing a colloidal solution containing polyacrylonitrile / carbon nanotube composite nanofibers, comprising the following steps:
[0056] 1-a): polyacrylonitrile and carbon nanotubes are vacuum dried at 110℃ for 48h, and then the dried polyacrylonitrile and carbon nanotubes are dispersed in N,N-dimethylformamide (DMF) at a mass ratio of 100:2, wherein the mass ratio of polyacrylonitrile to DMF is 100:8, and after continuous stirring, a uniform spinning solution is obtained.
[0057] 1-b): electrospinning the above spinning solution to obtain polyacrylonitrile / carbon nanotube / ionic liquid composite fiber membrane, wherein the electrospinning is carried out under the following conditions: the spinning voltage is 10 kV, the fiber receiving device is a roller, the rotating speed of which is 500 rpm, the spinning distance is 10 cm, and the spinning time is 60 minutes. Then, the composite fiber membrane is vacuum dried at 110°C for 48 hours and is ready for use.
[0058] 1-c): cutting the above composite fiber membrane and adding it into a mixed solvent prepared by deionized water and tert-butyl alcohol in a mass ratio of 100:20, and performing high-speed shearing at a rotating speed of 20000 rpm for 30 minutes to obtain a colloidal solution containing carbon nanotube / polyacrylonitrile composite nanofiber, which is ready for use; wherein the concentration of the composite nanofiber is 5 mg / mL.
[0059] (2) Preparation of MXenes / composite nanofiber / graphene oxide nanoribbon composite aerogel, specifically comprising:
[0060] 2-a): mixing the aqueous solution of MXenes, the aqueous solution of graphene oxide nanoribbon and the colloidal solution of composite nanofiber in step (1), and stirring at a rotating speed of 20000 rpm for 3 minutes to obtain a uniform mixed solution; wherein the mass ratio of MXenes material to composite nanofiber to graphene oxide nanoribbon is 100:60:60.
[0061] 2-b): placing the mixed solution obtained in 2-a) on a copper plate pre-frozen by liquid nitrogen to perform "oriented freezing", and then placing it in a freezing refrigerator to freeze slowly to slowly "physically crosslink"; and then slowly thawing at room temperature; and repeating the above freezing and thawing processes for 7 times to obtain a physically crosslinked MXenes / composite nanofiber / graphene oxide nanoribbon composite hydrogel; wherein the total time of freezing and thawing is 14 hours respectively.
[0062] 2-c): after dialysis of the above physically crosslinked composite hydrogel in deionized water, freeze-drying at -40°C for 72 hours, finally obtaining a MXenes / composite nanofiber / graphene oxide nanoribbon composite aerogel.
[0063] (3) Heat treatment of the composite aerogel
[0064] The composite aerogel obtained in step (2) is subjected to pre-oxidation treatment in air, wherein the pre-oxidation temperature is 280°C, the heating rate from room temperature to the pre-oxidation temperature is 4°C / min, and the pre-oxidation time is 60 minutes.
[0065] The pre-oxidized composite aerogel is subjected to carbonization treatment under Ar atmosphere, wherein the carbonization temperature is 1000°C, the temperature rising rate from room temperature to the carbonization temperature is 5°C / min, the carbonization time is 3h, and finally a composite conductive aerogel containing MXenes, carbon fibers, carbon nanotubes and graphene nanoribbons is obtained.
[0066] The composite conductive aerogel prepared in Example 1 has a three-dimensional interconnected porous network formed by interpenetration of MXenes material, graphene nanoribbons and composite fiber material, wherein the composite fiber material includes carbon nanotubes and carbon fibers, and the carbon fibers wrap the carbon nanotubes. In the composite conductive aerogel, the mass percentage of MXenes material is 45.45%, the mass percentage of graphene nanoribbons is 27.27%, the mass percentage of carbon nanotubes is 0.54%, and the mass percentage of carbon fibers is 26.74%.
[0067] To highlight the beneficial effects of the present application, the following comparative examples are provided.
[0068] Comparative Example 1
[0069] A pure MXenes aerogel is prepared by the following process, which is different from Example 1 in that: the MXenes solution is directly subjected to physical crosslinking in step 2-b), followed by freeze-drying in step 2-c), and then subjected to carbonization treatment under Ar atmosphere in step (4) to obtain a pure MXenes aerogel, i.e. the mass percentage of MXenes material is 100%.
[0070] Comparative Example 2
[0071] A MXenes / composite fiber conductive aerogel is prepared by the following process, which is different from Example 1 in that: no graphene oxide nanoribbons are added to the mixed solution in step 2-a).
[0072] In the conductive aerogel prepared in Comparative Example 2, the mass percentage of MXenes material is 62.5%, the mass percentage of graphene nanoribbons is 0, the mass percentage of carbon nanotubes is 0.74%, and the mass percentage of carbon fibers is 36.8%.
[0073] Comparative Example 3
[0074] Comparative Example 3 provides a MXenes / graphene nanoribbon conductive aerogel, which is different from Comparative Example 1 in that: only graphene oxide nanoribbons are mixed with MXenes material in step 2-a), and no polyacrylonitrile fibers are added.
[0075] In the conductive aerogel prepared in Comparative Example 3, the mass percentage of MXenes material is 62.5%, the mass percentage of graphene nanoribbons is 37.5%, and it does not contain carbon nanotubes and carbon fibers.
[0076] Figure 1 The macroscopic photo of the MXenes / composite fiber / graphene nanoribbon conductive aerogel material prepared in Example 1 is shown in FIG. 1. It can be seen that the volume shrinkage of the conductive aerogel material in the reaction container is small, which not only ensures the small density of the aerogel, but also maintains its rich internal pore structure; at the same time, the conductive aerogel product has a regular shape, and the surface is free of obvious pores, gullies and cracks, etc., and the apparent morphology of the aerogel sample from bottom to top is uniform. However, the pure MXenes aerogel material provided in Comparative Example 1 shows a significant collapse phenomenon (FIG. 2), and cannot form a regular configuration, which indicates that the pure MXenes material cannot independently form a three-dimensional material with certain mechanical strength. Figure 1 Figure 2 Figure 3 The macroscopic photo of the MXenes / composite fiber conductive aerogel material prepared in Comparative Example 2 is shown in FIG. 3. It can be seen that, compared with the pure MXenes aerogel material, the introduction of carbon fibers can improve the close packing degree of MXenes, and the composite aerogel sample shows improved regularity of appearance. Figure 3 Figure 4 The macroscopic photo of the MXenes / graphene nanoribbon conductive aerogel prepared in Comparative Example 3 is shown in FIG. 4. It can be seen that, compared with the pure MXenes aerogel material, the introduction of one-dimensional graphene nanoribbons can also improve the close packing degree of MXenes material, and the composite aerogel sample also shows high regularity. The above results show that pure MXenes cannot form an aerogel material with certain strength, and one-dimensional carbon fibers or one-dimensional graphene nanoribbons can help improve the mechanical properties of MXenes and improve the macroscopic regularity of MXenes-based aerogel, but the regularity of the shape and the consistency of the appearance of the obtained composite aerogel are still inferior to the composite aerogel containing MXenes, graphene nanoribbons and composite fibers in Example 1, for example, the aerogel product in FIG. 5 has a loose segment of pore arrangement near the bottom of the bottle. Figure 4 Figure 3
[0077] Further, the electrical conductivity and mechanical recovery performance of each conductive aerogel sample of Example 1 and Comparative Examples 1-3 were tested, and the results are shown in Table 1. The mechanical property test conditions are as follows: instrument equipment: Instron 9566, pressure sensor: 500N; test fixture: compression type fixture; test condition: room temperature; compression speed: 1mm / min; detection mode: compression recovery mode. The electrical conductivity test is tested by using Mitsubishi Chemical Low Resistance Meter (four-probe method).
[0078] Table 1
[0079] Sample No. First recovery rate (%) Third recovery rate (%) Sixth recovery rate (%) Resistivity (mΩ-cm) Example 1 90.5 90.0 86.5 15.6 Comparative Example 1 0 0 0 14.5 Comparative Example 2 86.5 84.3 80.2 25.1 Comparative Example 3 30.6 0 0 10.0
[0080] It can be learned from Table 1 that the pure MXene aerogel material does not have mechanical recovery, and after introducing polyacrylonitrile fibers or graphene oxide nanoribbons in the preparation process of Comparative Example 2 and Comparative Example 3, the obtained composite aerogel product can have certain recovery, but the conductivity is obviously reduced.
[0081] In summary, the composite conductive aerogel provided by the embodiment 1 of the present application has regular shape and high recovery, and the recovery rate of the composite aerogel can reach 90% after six times of stretching and reciprocating, and the conductivity is also good, which has great potential in the field of flexible electronic devices.
[0082] Embodiment 2
[0083] The difference between embodiment 2 and embodiment 1 is that in step (1), the mass ratio of polyacrylonitrile to carbon nanotube is 100:1.
[0084] In the composite conductive aerogel obtained by embodiment 2, the mass percentage of MXenes material is 45.45%, the mass percentage of graphene nanoribbon is 27.28%, the mass percentage of carbon nanotube is 0.27%, and the mass percentage of carbon fiber is 27%.
[0085] Embodiment 3
[0086] The difference between embodiment 3 and embodiment 1 is that in step (1), the mass ratio of polyacrylonitrile to carbon nanotube is 100:3.
[0087] In the composite conductive aerogel obtained by embodiment 3, the mass percentage of MXenes material is 45.45%, the mass percentage of graphene nanoribbon is 27.28%, the mass percentage of carbon nanotube is 0.79%, and the mass percentage of carbon fiber is 26.48%.
[0088] Embodiment 4
[0089] The difference between embodiment 4 and embodiment 1 is that in step (1), the mass ratio of polyacrylonitrile to carbon nanotube is 100:5.
[0090] In the composite conductive aerogel obtained by embodiment 4, the mass percentage of MXenes material is 45.45%, the mass percentage of graphene nanoribbon is 27.28%, the mass percentage of carbon nanotube is 1.30%, and the mass percentage of carbon fiber is 25.97%.
[0091] Embodiment 5
[0092] The difference between embodiment 5 and embodiment 1 is that in step (2), the mass ratio of MXenes material to composite nanofiber and graphene oxide nanoribbon in the colloidal solution is 100:90:90.
[0093] The mass ratio of the MXenes material in the composite conductive aerogel obtained in Example 5 is 35.71%, the mass ratio of the graphene nanoribbon is 32.15%, the mass ratio of the carbon nanotube is 0.63%, and the mass ratio of the carbon fiber is 31.51%.
[0094] Example 6
[0095] The difference between Example 6 and Example 1 is that in step (2), the mass ratio of the MXenes material to the composite nanofiber and the graphene oxide nanoribbon in the colloidal solution is 100:100:100.
[0096] The mass ratio of the MXenes material in the composite conductive aerogel obtained in Example 6 is 33.33%, the mass ratio of the graphene nanoribbon is 33.34%, the mass ratio of the carbon nanotube is 0.65%, and the mass ratio of the carbon fiber is 32.68%.
[0097] The MXenes-based composite conductive aerogel provided in Examples 2-6 also has excellent mechanical recovery performance and good conductivity, and the related test results are summarized in Table 2 below.
[0098] Table 2
[0099] Sample No. First recovery rate (%) Sixth recovery rate (%) Resistivity (mΩ-cm) Example 2 90.6 85.5 15.8 Example 3 89.5 88.9 15.6 Example 4 90.1 87.5 15.5 Example 5 91.5 91.0 21.9 Example 6 90.9 85.5 20.5
[0100] The above-described examples only express several exemplary embodiments of the present application, and the description is more specific and detailed, but it should not be understood as limiting the scope of the patent of the present application. It should be noted that for ordinary skilled in the art, without departing from the concept of the present application, a number of modifications and improvements can be made, and these modifications and improvements all belong to the protection scope of the present application.
Claims
1. A method of preparing a composite conductive aerogel, characterized by, The method comprises the following steps: (1) dispersing carbon nanotubes and polyacrylonitrile in a first solvent to obtain a spinning solution; electrospinning the spinning solution to obtain a composite fiber membrane; cutting the composite fiber membrane and placing it in a second solvent to obtain a colloidal solution containing polyacrylonitrile / carbon nanotube composite nanofibers by shearing; (2) mixing the colloidal solution with MXenes material and graphene nanoribbon, and performing freeze-thaw cycle treatment on the obtained mixed solution to occur physical crosslinking to obtain a composite hydrogel; freeze-drying the composite hydrogel to obtain a composite aerogel; (3) pre-oxidizing the composite aerogel at 200-300℃ in an oxygen-containing atmosphere, and then carbonizing the composite aerogel at 700-1000℃ in a non-oxidizing atmosphere to obtain a composite conductive aerogel containing MXenes, carbon fibers, carbon nanotubes and graphene nanoribbons.
2. The production method according to claim 1, wherein In step (1), the mass ratio of polyacrylonitrile to carbon nanotubes is 100:(1-5).
3. The production method according to claim 1, wherein In step (2), the mass ratio of MXenes material, polyacrylonitrile / carbon nanotube composite nanofiber and graphene oxide nanoribbon is 100:(5-100):(10-100).
4. The production method according to claim 1, wherein In step (1), the rotation speed of shearing is 10,000-30,000 rpm.
5. The production method according to claim 1, wherein In step (2), the freeze-thaw cycle treatment comprises: first placing the mixed solution of the colloidal solution, MXenes material and graphene oxide nanoribbon on a hard substrate pre-cooled by liquid nitrogen, then placing it in a freezer at-10 to-20℃ for freezing; then thawing at room temperature; and repeating the above freezing and thawing processes multiple times.
6. The production method according to claim 1, wherein In step (3), the oxygen-containing atmosphere is air; the heating rate of the pre-oxidation treatment is 1-5℃ / min, and the pre-oxidation treatment time is 30-120 min.
7. The production method according to claim 1, wherein The heating rate of the carbonization treatment is 1-5℃ / min, and the carbonization treatment time is 1-5 h.
8. A composite conductive aerogel, characterized in that, The composite conductive aerogel comprises MXenes material, graphene nanoribbon and composite fiber material, and has a three-dimensional interconnected porous network, wherein the composite fiber material comprises carbon nanotubes and carbon fibers, and the carbon fibers wrap the carbon nanotubes.
9. The composite conductive aerogel of claim 8, wherein, In the composite conductive aerogel, the mass percentage of MXenes material is 33.33%-86.96%, the mass percentage of graphene nanoribbon is 4.76%-48.78%, the mass percentage of carbon nanotubes is 0.024%-2.27%, and the mass percentage of composite fiber material is 2.44%-47.62%.
10. The composite conductive aerogel of any one of claims 8-9 or prepared by the method of any one of claims 1-7 for use in batteries, optoelectronic devices, photothermal devices, sensors, electromagnetic shielding.
Citation Information
Patent Citations
Graphene / black phosphorus nanosheet / sulfur-containing ionic liquid composite aerogel and preparation method thereof
CN107416846A
Flexible compressible 3D full-carbon nano fiber aerogel and preparation method thereof
CN108314008A