A method for preparing carbon-nitrogen material and a method for removing antibiotics from water

By preparing a reaction system consisting of carbon-nitrogen materials and persulfate, the problem of low catalytic activity of existing carbon materials is solved, achieving efficient removal of antibiotics from water, avoiding metal pollution, and exhibiting good stability and reusability.

CN117000281BActive Publication Date: 2024-11-01CHINESE RES ACAD OF ENVIRONMENTAL SCI +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310731335.X
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-06-20
Publication Date
2024-11-01
Estimated Expiration
2043-06-20

AI Technical Summary

Technical Problem

Existing carbon materials have low catalytic activity against persulfate, making it difficult to efficiently remove antibiotics from water and posing a risk of metal leaching.

Method used

By preparing carbon-nitrogen materials, using graphitic carbon nitride as a nitrogen source and polyethylene glycol as a carbon source, and combining the calcination method to synthesize carbon-nitrogen materials, a catalyst with abundant active sites is formed. This catalyst forms a reaction system with persulfate, catalyzing the generation of active species such as sulfate free radicals, which degrade antibiotics.

Benefits of technology

It achieves efficient catalysis of persulfate to generate active species over a wide pH range, rapidly removing antibiotics from water, and the catalyst is stable and reusable, avoiding metal contamination.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN117000281B_ABST
    Figure CN117000281B_ABST
Patent Text Reader

Abstract

The present disclosure provides a method for preparing a carbon-nitrogen material and a method for removing antibiotics from water. On the one hand, the present disclosure provides a method for preparing a carbon-nitrogen material, comprising: mixing a precursor with ammonium chloride, heat shrinking and reacting to obtain a graphite-like carbon nitride; mixing and grinding the graphite-like carbon nitride with polyethylene glycol to obtain a mixture of graphite-like carbon nitride and polyethylene glycol, calcining the mixture, cooling to room temperature, and obtaining a carbon-nitrogen material. On the other hand, the present disclosure provides a method for removing antibiotics from water using a carbon-nitrogen material, comprising: adding a carbon-nitrogen material and persulfate to a water body containing antibiotics, wherein the carbon-nitrogen material is prepared according to the aforementioned preparation method; mixing and stirring the water body containing the carbon-nitrogen material, persulfate, and antibiotics at room temperature. The carbon-nitrogen material prepared by the present disclosure has high catalytic activity for persulfate, good removal effect for antibiotics in water, fast reaction rate, and good stability.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present disclosure relates to the field of water treatment technology and the field of materials, and in particular to a method for preparing a carbon-nitrogen material and a method for removing antibiotics from water. Background Art

[0002] With the development of social economy, the global use of antibiotics has increased year by year. Most antibiotics cannot be completely absorbed by the body. More than 85% of antibiotics are excreted from the body in the form of parent structures or metabolites, directly or indirectly entering the water environment, accumulating in the biota and maintaining biological activity for a long time. Long-term exposure of antibiotics in the environment can induce organisms to produce antibiotic resistance genes and lead to the spread of various antibiotic-resistant bacteria, threatening human health.

[0003] Conventional sewage treatment processes are difficult to remove antibiotics efficiently. Advanced oxidation technology is one of the common methods for removing refractory macromolecular organic matter. The main oxidants are hydrogen peroxide, potassium permanganate, persulfate, peracetic acid, etc. Persulfate-based advanced oxidation technology can produce sulfate free radicals, which can decompose refractory organic matter into easily degradable small molecules in a wide pH range.

[0004] In the prior art, homogeneous transition metals, heterogeneous transition metals, carbon materials and their composite materials are commonly used to activate persulfate. 2+ The activation efficiency is the highest, but its toxicity limits its practical application. Although transition metal materials have high catalytic activity for persulfate, there is more or less metal leaching in water, which may cause secondary pollution. Compared with transition metal catalysts, carbon materials are environmentally friendly, but existing carbon materials have low catalytic activity for persulfate and take a long time to remove difficult-to-degrade macromolecular organic matter. Summary of the invention

[0005] 1. Technical issues to be resolved

[0006] In view of this, the present disclosure provides a method for preparing a carbon-nitrogen material and a method for removing antibiotics from water, which are used to at least partially solve the technical problem that existing carbon materials have low catalytic activity towards persulfate.

[0007] (II) Technical solution

[0008] In order to achieve the above-mentioned purpose, the first aspect of the present disclosure provides a method for preparing a carbon-nitrogen material, comprising: S11, mixing a precursor with ammonium chloride, performing heat shrinkage and reaction to obtain a graphite-like carbon nitride; wherein the precursor is a nitrogen-rich material; S12, mixing and grinding the graphite-like carbon nitride with polyethylene glycol to obtain a mixture of the graphite-like carbon nitride and polyethylene glycol, calcining the mixture, and cooling it to room temperature to obtain a carbon-nitrogen material.

[0009] According to an embodiment of the present disclosure, the precursor in S11 is one or more of dicyandiamide, melamine, and urea.

[0010] According to an embodiment of the present disclosure, the molar ratio of the precursor to ammonium chloride in S11 is 0.84-2.2:1.

[0011] According to an embodiment of the present disclosure, the heating rate of the heat shrinkage and reaction in S11 is 2 to 8° C. / min; the reaction temperature is 500 to 600° C., and the reaction time is 150 to 250 min.

[0012] According to an embodiment of the present disclosure, the mass ratio of graphite-like carbon nitride to polyethylene glycol in S12 is 1:0.25-2.

[0013] According to an embodiment of the present disclosure, the calcination temperature in S12 is 600-800° C., the calcination time is 2-5 hours, and the calcination is carried out under the protection of an inert gas; wherein the calcination heating rate is 2-8° C. / min; and the inert gas is argon or nitrogen.

[0014] The second aspect of the present disclosure provides a carbon-nitrogen material obtained according to the aforementioned carbon-nitrogen material preparation method, which forms a reaction system with persulfate for removing antibiotics in water.

[0015] The third aspect of the present disclosure provides a method for removing antibiotics from water using carbon-nitrogen materials, comprising: S21, adding carbon-nitrogen materials and persulfate to water containing antibiotics, wherein the carbon-nitrogen material is prepared according to the aforementioned carbon-nitrogen material preparation method; S22, mixing water containing carbon-nitrogen materials, persulfate, and antibiotics at room temperature, wherein the initial pH of the water is controlled at 3 to 9; and the stirring speed is 200 to 400 rpm.

[0016] According to an embodiment of the present disclosure, the mass ratio of carbon-nitrogen material, persulfate and antibiotic in S22 is {2.5-15}:{3-9.5}:1; wherein the persulfate is one or more of KHSO5·0.5KHSO4·0.5K2SO4 and KHSO4.

[0017] According to an embodiment of the present disclosure, it also includes: recycling the carbon-nitrogen material, including: S31, washing the carbon-nitrogen material with deionized water and ethanol; S32, drying the filtered carbon-nitrogen material to obtain a reusable carbon-nitrogen material; wherein the drying temperature is 50 to 80°C.

[0018] (III) Beneficial effects

[0019] The present invention overcomes the deficiencies in the prior art and provides a method for preparing a carbon-nitrogen material and a method for removing antibiotics from water. On the one hand, polyethylene glycol is used as a carbon source and graphite-like carbon nitride is used as a nitrogen source to synthesize the target carbon-nitrogen material by a simple calcination method. Graphite-like carbon nitride contains abundant N species, and the tri-s-triazine ring in the structure can provide more coordination sites, making it easier to form a special form of complexation and agglomeration with polyethylene glycol, which helps to form active sites such as defects and carbonyl groups. On the other hand, the carbon-nitrogen material is used as a catalyst to form a reaction system with persulfate, which can catalyze persulfate to produce sulfate radicals (SO4 ·- ), hydroxyl radicals (·OH), and singlet oxygen ( 1 O2), degrading antibiotics in water. The carbon-nitrogen material disclosed in the present invention has good removal effect on antibiotics in water, fast reaction rate, and good stability, and is an efficient metal-free solid catalyst. BRIEF DESCRIPTION OF THE DRAWINGS

[0020] Figure 1 The schematic diagram of the process of preparing the carbon-nitrogen material according to the embodiment of the present disclosure is shown;

[0021] Figure 2 The schematic diagram of the process of removing antibiotics from water using carbon-nitrogen materials according to an embodiment of the present disclosure is shown;

[0022] Figure 3 The schematic diagram of the process of recycling carbon-nitrogen materials according to the embodiment of the present disclosure is shown;

[0023] Figure 4 shows a TEM test image of the carbon-nitrogen material obtained according to an embodiment of the present disclosure;

[0024] Figure 5 shows an XRD test diagram of the carbon-nitrogen material obtained according to an embodiment of the present disclosure;

[0025] Figure 6 The XPS test diagram of the carbon-nitrogen material obtained according to the embodiment of the present disclosure is shown;

[0026] Figure 7 shows a BET test diagram of the carbon-nitrogen material obtained according to an embodiment of the present disclosure;

[0027] Figure 8 A comparison chart showing the removal of sulfamethoxazole by PMS alone or g-C3N4 / PMS or CN7 alone or CN7 / PMS system according to the embodiments of the present disclosure is shown;

[0028] Fig. 9A comparison diagram showing the removal of sulfamethoxazole in different water matrices using a method for removing antibiotics in water using carbon-nitrogen materials according to an embodiment of the present disclosure;

[0029] Fig.10 A comparison diagram showing the removal of sulfamethoxazole by persulfate activation of carbon-nitrogen materials prepared at different annealing temperatures according to the embodiments of the present disclosure;

[0030] Fig.11 A comparison diagram of the removal of sulfamethoxazole by activated persulfate after recovery of the carbon-nitrogen material obtained in the embodiment of the present disclosure is shown;

[0031] Description of reference numerals:

[0032] CN6-Carbon-nitrogen material prepared at a calcination temperature of 600°C;

[0033] CN6.5-Carbon-nitrogen material prepared under calcination temperature of 650°C;

[0034] CN7-Carbon-nitrogen material prepared at a calcination temperature of 700°C;

[0035] CN7.5-Carbon-nitrogen material prepared under calcination temperature of 750°C;

[0036] CN8-Carbon-nitrogen material prepared at a calcination temperature of 800℃. DETAILED DESCRIPTION

[0037] In order to make the objectives, technical solutions and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with specific embodiments and with reference to the accompanying drawings.

[0038] The terms used herein are only for describing specific embodiments and are not intended to limit the present disclosure. The terms "comprise", "include", etc. used herein indicate the existence of the features, steps, operations and / or components, but do not exclude the existence or addition of one or more other features, steps, operations or components.

[0039] The techniques and terms used in this disclosure have the same meanings as commonly understood by those skilled in the art. In addition, for numerical ranges in this disclosure, it should be understood that each intermediate value between the upper and lower limits of the range is specifically disclosed.

[0040] The present invention provides a method for preparing a carbon-nitrogen material. Figure 1 , the method includes S11~S12.

[0041] In operation S11, a precursor is mixed with ammonium chloride, and then heat-shrunk and reacted to obtain graphite-like carbon nitride (g-C3N4); wherein the precursor is a nitrogen-rich material.

[0042] In operation S12, graphite-like carbon nitride and polyethylene glycol are mixed and fully ground to obtain a mixture of graphite-like carbon nitride and polyethylene glycol, and the mixture is calcined and cooled to room temperature to obtain a carbonitride material. The polyethylene glycol is one or more of polyethylene glycol 2000, polyethylene glycol 4000, ethylene glycol 6000, and polyethylene glycol 8000.

[0043] Through the embodiments disclosed herein, the preparation process of the carbon-nitrogen material uses polyethylene glycol as a carbon source and nitrogen-rich graphene-like carbon nitride (57.1 at%) as a nitrogen source. The target catalyst is synthesized by a simple calcination method. It does not require acid or ethanol cleaning and can be used directly. The synthesis process is simple, the operation is simple, and the reaction conditions are mild, which is conducive to promotion and application. At the same time, the prepared carbon-nitrogen material has a large specific surface area, rich nanopores and micropore structures, and contains active sites such as defects, pyridine N, pyrrole N, graphite N, and carbonyl groups. The carbon-nitrogen material has a good removal effect on antibiotics by activating persulfate and a fast reaction rate, which can overcome the disadvantage of low catalytic activity of carbon materials to persulfate.

[0044] Based on the above embodiment, the precursor in S11 is one or more of dicyandiamide, melamine and urea.

[0045] According to the embodiments of the present disclosure, the nitrogen-rich precursor and ammonium chloride can be thermally condensed and reacted to directly synthesize graphite-like carbon nitride (g-C3N4), which is relatively easy to obtain.

[0046] Based on the above embodiment, the molar ratio of the precursor to ammonium chloride in S11 is 0.84-2.2:1.

[0047] According to the embodiments of the present disclosure, the mass of the precursor is 2 to 5 times that of ammonium chloride, and the prepared graphite-like carbon nitride (g-C3N4) is rich in nitrogen, with nitrogen accounting for about 57.1%.

[0048] Based on the above embodiment, the heating rate of the heat shrinkage and reaction in S11 is 2-8°C / min, preferably 5°C / min; the reaction temperature is 500-600°C, preferably 550°C; and the reaction time is 150-250min, preferably 180min.

[0049] According to the embodiments disclosed in the present invention, if the reaction time is too short or the heating rate is too fast, the temperature change rate inside and outside the graphite crystal will be uneven, causing the prepared g-C3N4 crystal structure to be damaged; if the reaction time is too long or the heating rate is too slow, the preparation time is long and the energy consumption is high; if the preparation temperature is too low, the heat energy required for the condensation of the tri-s-triazine ring cannot be reached; if the preparation temperature is too high, the pore structure of g-C3N4 will be destroyed due to decomposition, and the product will be unstable. The reaction temperature within the above range is conducive to efficiently obtaining stable graphite-like carbon nitride.

[0050] Based on the above embodiment, the mass ratio of graphite-like carbon nitride to polyethylene glycol in S12 is 1:0.25-2.

[0051] According to the embodiments disclosed herein, if there is too little polyethylene glycol (mass ratio less than 1:0.25), the output of carbon-nitrogen materials will be too little and the economic cost will be too high; if there is too much polyethylene glycol (mass ratio greater than 1:2), the active sites of the carbon-nitrogen materials will accumulate, affecting the catalytic activity of the carbon-nitrogen catalyst.

[0052] On the basis of the above embodiment, the calcination temperature in S12 is 600-800°C, the calcination time is 2-5h, and the calcination is carried out under the protection of an inert gas; wherein the calcination heating rate is 2-8°C / min; and the inert gas is argon or nitrogen.

[0053] According to the embodiments of the present disclosure, the calcination temperature is lower than 600°C and the heating rate is higher than 8°C / min, which will affect the performance of the carbon-nitrogen material; the calcination temperature is higher than 800°C and the heating rate is lower than 2°C / min, which will result in high energy consumption and long time for the catalyst preparation process. The inert gas can isolate the mixture from the air to prevent the mixture from reacting with oxygen and reducing the catalyst yield.

[0054] A second aspect of the embodiments of the present disclosure provides a carbon-nitrogen material obtained according to the aforementioned method for preparing the carbon-nitrogen material, which forms a reaction system with persulfate for removing antibiotics from water.

[0055] According to the embodiments of the present disclosure, the carbon-nitrogen material is used as a catalyst to activate persulfate, which has the advantages of high activation efficiency, fast reaction rate, good antibiotic removal effect, etc.

[0056] The third aspect of the embodiment of the present disclosure provides a method for removing antibiotics in water using carbon-nitrogen materials, see Figure 2 , the method includes S21~S22.

[0057] In operation S21, a carbon-nitrogen material is obtained by using the aforementioned method for preparing the carbon-nitrogen material, and the carbon-nitrogen material and persulfate are added to a water body containing antibiotics.

[0058] In operation S22, at room temperature, water containing carbon-nitrogen materials, persulfate, and antibiotics is mixed and stirred, wherein the initial pH of the water is controlled at 3 to 9; and the stirring speed is 200 to 400 rpm.

[0059] In the embodiments of the present disclosure, the degradation reaction time is 4 to 30 minutes.

[0060] Through the embodiments of the present disclosure, the carbon-nitrogen material prepared has high catalytic activity and good stability, can efficiently activate persulfate within a wide pH range to produce sulfate radicals, hydroxyl radicals, and singlet oxygen, and can quickly remove antibiotics from water. After 5 minutes of reaction, the removal rate of antibiotics reaches more than 90%.

[0061] Based on the above embodiments, the mass ratio of carbon-nitrogen material, persulfate and antibiotic in S22 is {2.5-15}:{3-9.5}:1, preferably 5:6:1; wherein the persulfate is one or more of KHSO5·0.5KHSO4·0.5K2SO4, KHSO4, preferably KHSO5·0.5KHSO4·0.5K2SO4.

[0062] According to the embodiments of the present disclosure, too much carbon-nitrogen material and persulfate will increase the economic cost; too little carbon-nitrogen material and persulfate will affect the effect of removing antibiotics.

[0063] Based on the above embodiment, the carbon-nitrogen material is also recycled. Figure 3 , the method includes S31~S32.

[0064] In operation S31, the carbon-nitrogen material is washed with deionized water and ethanol; wherein the above washing process is performed at least once.

[0065] In operation S32, the filtered carbon-nitrogen material is dried to obtain a reusable carbon-nitrogen material; wherein the drying is completed in a blast drying oven at a drying temperature of 50 to 80°C.

[0066] Through the embodiments of the present disclosure, the prepared carbon-nitrogen material has a certain durability, and the carbon-nitrogen material can be separated and recovered from water and reused, thereby reducing the cost of using materials and is an environmentally friendly catalyst.

[0067] Embodiment 1

[0068] The preparation of carbon-nitrogen materials is as follows:

[0069] (1) 5 g of a precursor and 1.25 g of ammonium chloride were mixed and placed in a 15 mL corundum crucible. The mixture was reacted at 550 ° C for 3 h at a heating rate of 5 ° C / min in a muffle furnace and then cooled to room temperature to obtain graphite-like carbon nitride (g-C3N4); wherein the precursor was melamine.

[0070] (2) 1.25 g g-C3N4 and 0.75 g polyethylene glycol were mixed respectively, ground evenly, placed in a covered corundum crucible, and calcined in a nitrogen atmosphere at a calcination temperature of 700°C and a heating rate of 5°C / min; the calcination time was 5 h, and the mixture was cooled to room temperature to obtain a carbon nitrogen material (CN7); wherein the polyethylene glycol was polyethylene glycol 2000.

[0071] Characterization test analysis of carbon-nitrogen material (CN7):

[0072] (1) The morphology and structure of the prepared materials were observed using a Talos F200S electron microscope and a SUPER X transmission electron microscope (TEM). Figure 4 From the TEM test image shown, it can be observed that the morphology of the carbon nitride material is a lamellar structure.

[0073] (2) The crystal structure of the carbon-nitrogen material was characterized by using a German Bruker D8 Advance X-ray diffractometer (XRD), and the following was obtained: Figure 5 The XRD test diagram shown in the figure shows that the sharp characteristic peak of g-C3N4 at 25° is 002 face crystalline carbon, while the wide characteristic peak of the carbon nitrogen material at 24° is 002 face amorphous carbon structure, indicating that the structure of the g-C3N4 material is destroyed and the carbon nitrogen material is successfully prepared.

[0074] (3) The elemental composition of the carbon-nitrogen material was analyzed using ESCALAB 250X X-ray photoelectron spectroscopy (X-ray photoecectron spectroscopy, XPS) (ThermoFischer, USA), and the following was obtained: Figure 6 The XPS test graph shown in the figure shows that the carbon-nitrogen material contains abundant active sites such as sp2 carbon, carbonyl, pyridinic N, pyrrolic N, and graphitic N. The Raman spectrum shows that the carbon-nitrogen material I D / I G It is 1.08, indicating that the material contains abundant defect sites, which makes it have high catalytic activity.

[0075] (4) The specific surface area, total pore volume and pore size distribution of the carbon-nitrogen material were analyzed using the American Micromeritics ASAP 2460 fully automatic physical adsorption instrument (multilayer adsorption model proposed by Brunauer, Emmett and Teller, BET), and the following results were obtained: Figure 7 The BET test graph shown in the figure shows that the carbon nitrogen material has a nanostructure and its pore volume is 0.38 cm 3 / g, with a large specific surface area of ​​950.10m 2 / g.

[0076] In this embodiment, the carbon-nitrogen material has a certain durability, and the carbon-nitrogen material can be reused after being separated from the liquid phase.

[0077] Embodiment 2

[0078] The preparation of carbon-nitrogen materials is as follows:

[0079] (1) 5 g of a precursor and 1.25 g of ammonium chloride were mixed and placed in a 15 mL corundum crucible, and reacted at 550 ° C for 3 h at a heating rate of 5 ° C / min in a muffle furnace, and then cooled to room temperature to obtain graphite-like carbon nitride (g-C3N4); wherein the precursor is melamine;

[0080] (2) Take 1.25g g-C3N4 and 0.75g polyethylene glycol respectively, mix them, grind them evenly, place them in a corundum crucible with a lid, and calcine them in a nitrogen atmosphere at 600℃, 650℃, 750℃, and 800℃, respectively, with a heating rate of 5℃ / min; the calcination time is 5h, and cool to room temperature to obtain carbon nitrogen materials (CN6, CN6.5, CN7, CN7.5, CN8).

[0081] Embodiment 3

[0082] In this example, the carbon-nitrogen material (CN7) prepared in Example 1 was selected as a catalyst to activate persulfate to remove sulfamethoxazole (SMX) from water, as follows:

[0083] In a 20 mg / L SMX solution, 0.1 g / L carbon-nitrogen material and 0.4 mM PMS were added to trigger the test at a stirring speed of 300 rpm. Samples were taken at regular intervals and then filtered with a 0.22 μm filter membrane to separate the activated material. Sodium thiosulfate was added to terminate the reaction and the collected solution was subjected to HPLC analysis for SMX concentration.

[0084] At the same time, three groups of comparative tests were conducted as follows: adding persulfate (PMS) alone without adding carbon-nitrogen material, and other conditions were the same as above; adding carbon-nitrogen material (CN7) alone without adding PMS, and other conditions were the same as above; adding g-C3N4 as a catalyst, and other conditions were the same as above.

[0085] like Figure 8 As shown in the figure, the removal rate of SMX by the oxidant PMS itself is negligible; the carbon-nitrogen material (CN7) alone can adsorb 39.7% of SMX in 10 minutes; g-C3N4 as a catalyst cannot effectively activate PMS to degrade SMX; when carbon-nitrogen materials and PMS are added at the same time, SMX can be almost completely removed in 10 minutes. The results show that the direct oxidation of PMS and carbon-nitrogen materials have limited effects on the removal of SMX, but the activation effect of carbon-nitrogen materials on persulfate is much greater than that of g-C3N4.

[0086] Embodiment 4

[0087] In this example, the carbon-nitrogen material (CN7) prepared in Example 1 was selected as a catalyst to activate persulfate to remove SMX in different water matrices, as follows:

[0088] The test was triggered by adding 0.1 g / L carbon-nitrogen material and 0.4 mM PMS to 20 mg / L SMX solutions in ultrapure water, tap water and lake water at a stirring speed of 300 rpm. Samples were taken at regular intervals and then filtered through a 0.22 μm filter membrane to separate the activated material. Sodium thiosulfate was added to terminate the reaction and the collected solutions were subjected to HPLC analysis for SMX concentration.

[0089] like Fig. 9 As shown in the figure, in the water matrix of ultrapure water, tap water and lake water, the removal of SMX in 10 minutes was 95.1%, 76.7% and 69.92% respectively. The carbon-nitrogen material / PMS system has a good removal effect on SMX and a fast reaction rate.

[0090] Embodiment 5

[0091] In this example, the carbon-nitrogen materials (CN6, CN6.5, CN7, CN7.5, CN8) prepared at different temperatures in Example 2 were selected as catalysts to activate persulfate to remove SMX from water, as follows:

[0092] In a 20 mg / L SMX solution, 0.1 g / L carbon-nitrogen material and 0.4 mM PMS were added to trigger the test at a stirring speed of 300 rpm. Samples were taken at regular intervals and then filtered with a 0.22 μm filter membrane to separate the activated material. Sodium thiosulfate was added to terminate the reaction and the collected solution was subjected to HPLC analysis for SMX concentration.

[0093] like Fig.10 As shown, the results indicate that increasing the calcination temperature will improve the SMX removal performance of the carbon-nitrogen material in this embodiment.

[0094] Embodiment 6

[0095] In this example, the carbon-nitrogen material recovered in Example 3 was selected as a catalyst to activate persulfate to remove SMX from water, as follows:

[0096] In a 20 mg / L SMX solution, under the condition of stirring at 300 rpm, 0.1 g / L of recovered carbon-nitrogen material and 0.4 mM PMS were added to trigger the test, and samples were taken at regular intervals, and then filtered with a 0.22 μm filter membrane to separate the activated material, sodium thiosulfate was added to terminate the reaction, and the collected solution was analyzed by high performance liquid chromatography for SMX concentration. The reaction conditions after the 1st to 4th recovery of carbon-nitrogen catalysts were as above.

[0097] The results of the first use of carbon-nitrogen catalyst to activate persulfate to remove SMX from water and the 1st to 4th recycling of carbon-nitrogen catalyst to activate persulfate to remove SMX from water are as follows: Fig.11 As shown, the catalytic performance of the carbon-nitrogen catalyst is less affected and can be recycled.

[0098] It should be noted that the method for preparing the carbon-nitrogen material and the method for removing antibiotics from water provided by the embodiments of the present disclosure also have at least one of the following effects and advantages:

[0099] (1) The carbon-nitrogen material disclosed in the present invention is prepared by a calcination method, and the synthesis process is simple, the operation is simple, and the reaction conditions are mild, which is conducive to promotion and application.

[0100] (2) The carbon-nitrogen material prepared by the present disclosure has a large specific surface area, rich nanopore and micropore structures, and contains defects, pyridinic N, pyrrolic N, graphitic N, and carbonyl groups as active sites. The carbon-nitrogen material activates persulfate to produce SO4 ·- , OH and 1 O2 has good removal effect and fast reaction rate in removing antibiotics from water, and can efficiently activate persulfate in a wide pH range, which can overcome the disadvantage of low catalytic activity of carbon materials for persulfate.

[0101] (3) The carbon-nitrogen material prepared in the present invention also has good reusability and is an environmentally friendly catalyst.

[0102] The specific embodiments described above further illustrate the purpose, technical solutions and beneficial effects of the present disclosure. It should be understood that the above description is only a specific embodiment of the present disclosure and is not intended to limit the present disclosure. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present disclosure should be included in the protection scope of the present disclosure.

Claims

1. A method for preparing a carbon-nitrogen material, characterized in that: include: S11, mixing a precursor with ammonium chloride, and obtaining graphite-like carbon nitride by heat shrinkage and reaction; wherein the precursor is a nitrogen-rich material; S12, mixing and grinding the graphite-like carbon nitride and polyethylene glycol to obtain a mixture of graphite-like carbon nitride and polyethylene glycol, calcining the mixture, and cooling it to room temperature to obtain the carbon nitrogen material; Wherein, the precursor in S11 is one or more of dicyandiamide, melamine and urea; The molar ratio of the precursor to ammonium chloride in S11 is 0.84-2.2:1; The heating rate of the heat shrinkage and reaction in S11 is 2-8°C / min; the reaction temperature is 500-600°C, and the reaction time is 150-250min; The mass ratio of graphite-like carbon nitride to polyethylene glycol in S12 is 1:0.25~2.

2. The method for preparing the carbon-nitrogen material according to claim 1, characterized in that: The calcination temperature in S12 is 600-800°C, the calcination time is 2-5 h, and the calcination is carried out under the protection of an inert gas; wherein the heating rate of the calcination is 2-8°C / min; and the inert gas is argon or nitrogen.

3. A carbon-nitrogen material obtained by the carbon-nitrogen material preparation method according to any one of claims 1 to 2, which forms a reaction system with persulfate and is used to remove antibiotics in water.

4. A method for removing antibiotics from water using carbon-nitrogen materials, characterized in that: include: S21, adding a carbon-nitrogen material and persulfate to water containing antibiotics, wherein the carbon-nitrogen material is prepared according to the method for preparing a carbon-nitrogen material according to any one of claims 1 to 2; S22, mixing and stirring the water containing the carbon-nitrogen material, the persulfate, and the antibiotic at room temperature; The initial pH of the water body is controlled at 3-9; the carbon-nitrogen material reacts with the persulfate and degrades the antibiotics in the water; and the stirring speed is 200-400 rpm.

5. The method for removing antibiotics from water using carbon-nitrogen materials according to claim 4, wherein the mass ratio of the carbon-nitrogen material, persulfate, and antibiotics in S22 is 2.5-15: 3-9.5: 1; in, The persulfate is one or more of KHSO5•0.5KHSO4•0.5K2SO4, and KHSO4.

6. The method for removing antibiotics in water using carbon-nitrogen materials according to claim 4, further comprising: Recycling of carbon and nitrogen materials, including: S31, washing the carbon-nitrogen material with deionized water and ethanol; S32, drying the filtered carbon-nitrogen material to obtain a reusable carbon-nitrogen material; Wherein, the drying temperature is 50-80°C.