A cathode electrode for hydrogen production by wastewater electrolysis, its composition design method, and its application.

By combining magnetron sputtering and machine learning, a high-entropy alloy electrode was prepared, which solved the problems of insufficient catalytic performance and preparation of high-entropy alloy electrodes, realized efficient hydrogen production from wastewater electrolysis, and improved the catalytic performance and corrosion resistance of the electrode.

CN117051422BActive Publication Date: 2026-11-17SOUTHWEST PETROLEUM UNIV
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202311268183.0
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-09-28
Publication Date
2026-11-17
Estimated Expiration
2043-09-28

AI Technical Summary

Technical Problem

Existing high-entropy alloy electrode materials have insufficient hydrogen evolution catalytic performance and are difficult to prepare on a large scale. Salt and organic matter in industrial wastewater reduce the catalytic performance and service life of the electrodes. Traditional alloy preparation has a long cycle and is not easy to scale up.

Method used

High-entropy alloys were prepared on the surface of a metal substrate by magnetron sputtering. High-entropy alloy components with high catalytic performance were quickly screened by combining machine learning prediction models. A database was established and active learning was performed to prepare porous high-entropy alloy electrodes.

Benefits of technology

This technology enables an efficient and sustainable wastewater electrolysis hydrogen production process, reducing the demand for freshwater resources, simplifying wastewater treatment processes and costs, and improving the catalytic performance and corrosion resistance of the electrodes.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN117051422B_ABST
    Figure CN117051422B_ABST
Patent Text Reader

Abstract

This invention relates to a cathode electrode for hydrogen production via wastewater electrolysis, its composition design method, and its application. The cathode electrode comprises a high-entropy alloy formed on the surface of a metal substrate. The high-entropy alloy contains Ni and Al, and also contains three or more elements selected from Zr, Ti, Cr, Mo, Co, Ce, P, and S. The atomic percentages of Ni and Al are 5–35% and 0.2–10%, respectively; the atomic percentages of the other elements are 0.3–35%. The composition design method employs magnetron sputtering technology to prepare a high-entropy alloy electrode with a compositional gradient distribution. By collecting information on the microstructure and catalytic performance of the high-entropy alloy, a database is constructed. Then, machine learning is applied to establish a model. By inputting morphological features, the model rapidly outputs the hydrogen evolution catalytic performance of the high-entropy alloy, thus achieving composition design. The high-entropy alloy electrode of this invention exhibits high catalytic activity and excellent corrosion resistance, enabling long-term stable operation in wastewater environments.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of electrode material technology for wastewater treatment and electrolytic hydrogen production, and particularly relates to a cathode electrode for wastewater electrolytic hydrogen production, its composition design method, and its application. Background Technology

[0002] Hydrogen, as a high-calorific-value clean energy source, has the potential to replace traditional fossil fuels and build a green, low-carbon energy system. However, most commercial electrolyzers currently use pure water to produce hydrogen, requiring extremely high purity of the raw water, which must not contain any chemicals that interfere with the electrolysis reaction. To improve electrolysis efficiency, an appropriate amount of electrolyte is usually added. With the advancement and large-scale application of water electrolysis hydrogen production technology, the consumption of scarce freshwater resources will become increasingly serious. With the rapid development of industries such as petrochemicals, metal smelting, pesticides, pharmaceuticals, food processing, and papermaking, the production of industrial wastewater is constantly increasing. Different industries and production methods result in significant differences in the types and quantities of pollutants in industrial wastewater, making industrial wastewater treatment processes complex and costly. If industrial wastewater could be used for water electrolysis to produce hydrogen, it would not only reduce the demand for freshwater resources but also lower the treatment process and costs. However, wastewater hydrogen production faces another serious problem: the salt and organic matter in the wastewater significantly reduce the catalytic performance and service life of the electrodes.

[0003] High-entropy alloys are a class of metallic materials possessing high strength, high hardness, and excellent corrosion resistance. Recent studies have also found that high-entropy alloys exhibit excellent hydrogen evolution catalytic performance. However, the hydrogen evolution catalytic performance of existing high-entropy alloy electrode materials needs further improvement, and there is no discernible pattern in the composition selection of high-entropy alloy electrode materials used for hydrogen electrolysis. Furthermore, current methods for preparing high-entropy alloys typically employ single methods, such as thermal spraying, vacuum arc melting, mechanical alloying, and magnetron sputtering, which make it difficult to prepare high-entropy alloys on a large scale and to quickly screen for the optimal metallic elements and their proportions.

[0004] In summary, it is essential to provide a cathode electrode and its composition design method and application for hydrogen production by wastewater electrolysis, which will help achieve an efficient and sustainable hydrogen production process by wastewater electrolysis and promote the development of cathode materials for hydrogen production by wastewater electrolysis. Summary of the Invention

[0005] To address one or more technical problems existing in the prior art, this invention provides a cathode electrode and its composition design method and application for hydrogen production by wastewater electrolysis.

[0006] The present invention provides a cathode electrode for hydrogen production by wastewater electrolysis in a first aspect. The cathode electrode comprises a metal substrate and a high-entropy alloy formed on the surface of the metal substrate. The high-entropy alloy contains Ni and Al, and also contains three or more elements selected from Zr, Ti, Cr, Mo, Co, Ce, P, and S. The atomic percentage of Ni in the high-entropy alloy is 5-35%, the atomic percentage of Al is 0.2-10%, and the atomic percentage of the other elements is 0.3-35%.

[0007] Preferably, the high-entropy alloy has the following general formula: Ni x A y B z Al w Wherein, A is one or more of Zr, Ti, and Cr, and B is at least two of Mo, Co, Ce, P, and S; x, y, z, and w are all atomic percentages, 5% ≤ x ≤ 35%, 5% ≤ y ≤ 35%, 10% ≤ z ≤ 70%, 0.2% ≤ w ≤ 10%, and x + y + z + w = ​​100%; preferably, A is Cr, B is Mo and Co, 30% ≤ x ≤ 35%, 5% ≤ y ≤ 15%, and in the high-entropy alloy, the atomic percentage of Mo is 25-35%, and the atomic percentage of Co is 20-32%; more preferably, A is Cr, B is Mo, Ce, and P, or B is Mo, Ce, and S, 30% ≤ x ≤ 35%, 5% ≤ y ≤ 15%, and in the high-entropy alloy, the atomic percentage of Mo is 25-35%, the atomic percentage of Ce is 20-32%, and the atomic percentage of P or S is 0.3-2%.

[0008] Preferably, the high-entropy alloy is prepared by magnetron sputtering; more preferably, the magnetron sputtering is magnetron co-sputtering; even more preferably, the high-entropy alloy is a porous high-entropy alloy, and the porous high-entropy alloy is prepared by: firstly preparing a high-entropy alloy on the surface of a metal substrate by magnetron sputtering, and then performing a dealloying treatment on the high-entropy alloy formed on the surface of the metal substrate to obtain a porous high-entropy alloy.

[0009] Preferably, the process parameters for magnetron sputtering are: a base vacuum of no more than 5 × 10⁻⁶. -4 The process gas pressure is 0.4–0.7 Pa, and magnetron sputtering is performed using a DC power supply with a power of 40–140 W and a sputtering time of 30–100 min. Preferably, the target material is subjected to ion bombardment glow discharge cleaning before preparing the high-entropy alloy on the surface of the metal substrate. Preferably, when the high-entropy alloy contains P and / or S elements, the magnetron sputtering temperature is 180–200 °C.

[0010] Preferably, the dealloying treatment is as follows: the high-entropy alloy formed on the surface of the metal substrate is immersed in a sodium hydroxide solution with a concentration of 0.05-0.15 mol / L for 1-3 hours; the thickness of the high-entropy alloy is 0.6-8 μm; the metal substrate is nickel or stainless steel; and / or preferably, the nickel is nickel plate, nickel mesh or nickel foam, and the stainless steel is 304L stainless steel, 316 stainless steel or 316L stainless steel.

[0011] In a second aspect, the present invention provides a method for preparing the cathode electrode for hydrogen production from wastewater as described in the first aspect, the method comprising the following steps:

[0012] (1) Surface pretreatment of the metal substrate;

[0013] (2) A high-entropy alloy is prepared on the surface of the metal substrate after step (1) by magnetron sputtering; optionally, the high-entropy alloy formed on the surface of the metal substrate is subjected to dealloying treatment.

[0014] In a third aspect, the present invention provides a method for designing the composition of a cathode electrode for hydrogen production by wastewater electrolysis, the method comprising the following steps:

[0015] S1. A high-entropy alloy with a compositional gradient distribution is prepared on the surface of a metal substrate by magnetron sputtering. The high-entropy alloy is then cut into multiple samples. The microstructure of each cut sample is observed by scanning electron microscopy. The elemental composition of each cut sample is recorded by X-ray energy dispersive spectroscopy or X-ray photoelectron spectroscopy. The electrochemical characteristics of each cut sample are tested by a three-electrode system.

[0016] S2. Collect known data on high-entropy alloys and establish a database. The data on high-entropy alloys includes the entropy value of the cut sample, elemental composition, physicochemical properties of the elements, surface microstructure characteristics, preparation information, electrochemical characteristics, and catalytic conditions for testing electrochemical characteristics.

[0017] S3. The collected data information is screened and normalized to construct a machine learning prediction model with the preparation information, elemental composition, physicochemical properties of elements, surface microstructure characteristics, entropy value and catalytic conditions of high-entropy alloy as input information and the electrochemical characteristics of high-entropy alloy as output information.

[0018] S4. Train the machine learning prediction model. When the training accuracy reaches the target, obtain the target machine learning prediction model. Then, use the target machine learning prediction model to predict the electrochemical characteristics of the cut sample to obtain the composition of multiple cathode electrodes with excellent catalytic performance for hydrogen production by wastewater electrolysis.

[0019] Preferably, after the target machine learning prediction model obtains the composition of multiple cathode electrodes with excellent catalytic performance for wastewater electrolysis hydrogen production, multiple cathode electrodes with the same composition and excellent catalytic performance are prepared. These cathode electrodes are then used in long-term experiments for wastewater electrolysis hydrogen production. The relevant experimental data from the long-term experiments are input into the database of step S2, and the target machine learning prediction model is used for active learning to further enhance the accuracy of the predictions. Preferably, the current density in the long-term experiments is not less than 250 mA / cm². 2 The long-term test duration shall not be less than 1000 hours; preferably, the relevant experimental data of the long-term test include the measured catalytic performance of the cathode electrode and the recorded surface microstructure and physicochemical characteristics of the cathode electrode sample.

[0020] Preferably, the electrochemical features include active surface area and overpotential; and / or, when constructing a machine learning prediction model, the surface microstructure features are digitized through machine learning to obtain information on lattice spacing, number of defects, number of pores, and specific surface area.

[0021] The present invention provides, in a fourth aspect, the application of the cathode electrode for hydrogen production by wastewater electrolysis as described in the first aspect of the present invention, or the cathode electrode for hydrogen production by wastewater electrolysis obtained by the composition design method described in the third aspect of the present invention, in hydrogen production by wastewater electrolysis.

[0022] Compared with the prior art, the present invention has at least the following beneficial effects:

[0023] (1) The cathode electrode for hydrogen production by wastewater electrolysis described in this invention is composed of a metal matrix and a high-entropy alloy. The metal matrix is ​​preferably made of foamed nickel with good hydrogen evolution performance or stainless steel with good corrosion resistance. The high-entropy alloy described in this invention is prepared from five or six or more elements selected from Ni-Zr-Ti-Cr-Mo-Co-Ce-Al-PS. Specifically, the high-entropy alloy contains Ni and Al, and also contains three or more other elements selected from Zr, Ti, Cr, Mo, Co, Ce, P, and S. The cathode electrode has high catalytic activity, good mechanical properties, and excellent corrosion resistance, enabling it to serve for a long time under harsh wastewater conditions.

[0024] (2) This invention provides a novel method for designing the composition of a cathode electrode for hydrogen production by wastewater electrolysis. It introduces machine learning methods, combines high-throughput preparation with high-throughput screening, and establishes a predictive model to predict the hydrogen evolution catalytic performance of the cathode electrode from the microscopic morphology characteristics of the high-entropy alloy surface. This allows for rapid screening of catalysts with unknown performance, resulting in high-entropy alloy compositions with high catalytic performance. Compared with traditional alloy preparation, this method significantly reduces the amount of experimentation, saves labor costs, significantly improves preparation efficiency, reduces screening costs, and accelerates the development of high-performance materials. This composition design method can provide guidance for the design and preparation of cathode electrodes for hydrogen production by electrolysis of industrial wastewater, and is also applicable to the design and preparation of multi-element alloys in other fields.

[0025] (3) This invention uses magnetron sputtering to prepare multi-component high-entropy alloys with compositional gradients on the surface of a metal substrate in high throughput. This overcomes the shortcomings of traditional alloy materials, such as long preparation cycle, difficulty in large-scale preparation, non-uniform composition, and large experimental characterization requirements. It can quickly obtain cathode electrode materials with precise atomic ratios.

[0026] (4) The present invention uses a cathode electrode with a high-entropy alloy obtained by magnetron sputtering to produce hydrogen from wastewater by electrolysis, which reduces the demand for freshwater resources on the one hand, and reduces the process and cost of wastewater treatment on the other hand.

[0027] (5) This invention combines high-throughput preparation using magnetron sputtering technology with machine learning to develop a new method for designing the composition of cathode electrodes for hydrogen production by wastewater electrolysis. This method enables rapid selection of the composition and proportion of high-entropy alloying elements in the cathode electrode, thereby promoting the development of cathode materials for hydrogen production by wastewater electrolysis. This invention will help realize an efficient and sustainable hydrogen production process by wastewater electrolysis and make an important contribution to the field of clean energy. Attached Figure Description

[0028] Figure 1 This is a flowchart of the preparation of a cathode electrode for hydrogen production by wastewater electrolysis in some specific embodiments of the present invention;

[0029] Figure 2 This is a schematic diagram of the process of constructing a machine learning prediction model in some specific embodiments of the present invention. Detailed Implementation

[0030] To make the objectives, technical solutions, and advantages of this invention clearer, the technical solutions of this invention will be clearly and completely described below in conjunction with the embodiments of this invention. Obviously, the described embodiments are only some, not all, of the embodiments of this invention. All other embodiments obtained by those skilled in the art based on the embodiments of this invention without creative effort are within the scope of protection of this invention.

[0031] In a first aspect, this invention provides a cathode electrode for hydrogen production by wastewater electrolysis. The cathode electrode (hereinafter referred to as the cathode electrode) comprises a metal substrate and a high-entropy alloy (also referred to as a high-entropy alloy electrode layer) formed on the surface of the metal substrate. In this invention, the high-entropy alloy is preferably prepared by magnetron sputtering, which offers the advantage of high-throughput preparation. The high-entropy alloy contains Ni (nickel) and Al (aluminum), and also contains elements selected from Zr (zirconium), Ti (titanium), Cr (chromium), Mo (molybdenum), Co (cobalt), Ce (cerium), and P. The high-entropy alloy contains three or more elements, including phosphorus and sulfur; the atomic percentage of Ni is 5-35%, the atomic percentage of Al is 0.2-10%, and the atomic percentage of other elements is 0.3-35%; in this invention, the sum of the atomic percentages of all elements in the high-entropy alloy is 100%; in this invention, the wastewater includes, but is not limited to, oilfield wastewater (e.g., chlorinated oilfield wastewater), domestic sewage, industrial wastewater, and / or pharmaceutical wastewater, such as industrial COD wastewater (e.g., high COD industrial wastewater or food industry wastewater).

[0032] The cathode electrode for hydrogen production by wastewater electrolysis described in this invention is composed of a metal matrix and a high-entropy alloy. The metal matrix is ​​preferably made of foamed nickel with good hydrogen evolution performance or stainless steel with good corrosion resistance. The high-entropy alloy in this invention is prepared from five or six or more elements selected from Ni-Zr-Ti-Cr-Mo-Co-Ce-Al-PS. Specifically, the high-entropy alloy contains Ni and Al, and also contains three or more other elements selected from Zr, Ti, Cr, Mo, Co, Ce, P, and S. This cathode electrode has high catalytic activity, good mechanical properties, and excellent corrosion resistance, enabling it to operate for a long time under harsh wastewater conditions.

[0033] According to some preferred embodiments, the general formula for the composition of the high-entropy alloy is: Ni x A y B z Al wWherein, A is one or more of Zr, Ti, and Cr, and B is at least two of Mo, Co, Ce, P, and S; x, y, z, and w are atomic percentages, 5% ≤ x ≤ 35%, 5% ≤ y ≤ 35%, 10% ≤ z ≤ 70%, 0.2% ≤ w ≤ 10%, and x + y + z + w = ​​100%; In this invention, the high-entropy alloy is based on Ni, preferably with the addition of one or more passivating elements Zr, Ti, and Cr, which improves the surface passivation capability of the cathode electrode used for hydrogen production from wastewater in this invention and provides long-term stability in high-COD wastewater. Preferably, at least two of the synergistic elements Mo, Co, Ce, P, and S are added to further enhance the catalytic activity of the cathode electrode. At the same time, Al is added, which can be used to adjust the crystal structure of the high-entropy alloy and is also beneficial for dealloying to form a porous nanostructure; In some more preferred embodiments, the addition of synergistic elements P and / or S can cause partial sulfidation or phosphating of the high-entropy alloy, which is beneficial for promoting the hydrogen evolution performance of the high-entropy alloy, etc. The high-entropy alloy in this invention can effectively improve intrinsic catalytic activity by utilizing the synergistic effect between alloying elements and adjust the structure of the catalytic interface to increase the number of catalytic active sites; at the same time, the synergistic effect between alloying elements can also improve the corrosion resistance of metallic materials.

[0034] According to some preferred embodiments, A is Cr, B is Mo and Co, 30% ≤ x ≤ 35% (x can be, for example, 30%, 31%, 32%, 33%, 34%, or 35%), 5% ≤ y ≤ 15% (y can be, for example, 5%, 6%, 7%, 8%, 9%, 10%, 11%, 12%, 13%, 14%, or 15%), and in the high-entropy alloy, the atomic percentage of Mo is 25-35% (e.g., 25%, 26%, 27%). 28%, 29%, 30%, 31%, 32%, 33%, 34%, or 35%, with an atomic percentage of Co of 20–32% (e.g., 20%, 21%, 22%, 23%, 24%, 25%, 26%, 27%, 28%, 29%, 30%, 31%, or 32%); more preferably, A is Cr, B is Mo, Ce, and P, or B is Mo, Ce, and S, 30% ≤ x ≤ 35% (x can be, for example, 30%, 31%, 28%, 29%, 30%, 31%, or 32%). 5% ≤ y ≤ 15% (y can be, for example, 5%, 6%, 7%, 8%, 9%, 10%, 11%, 12%, 13%, 14%, or 15%), in the high-entropy alloy, the atomic percentage of Mo is 25%–35% (e.g., 25%, 26%, 27%, 28%, 29%, 30%, 31%, 32%, 33%, 34%, or 35%), and the atomic percentage of Ce is 20%–32%. % (e.g., 20%, 21%, 22%, 23%, 24%, 25%, 26%, 27%, 28%, 29%, 30%, 31%, or 32%), with the atomic percentage of P or S being 0.3% to 2% (e.g., 0.3%, 0.4%, 0.5%, 0.6%, 0.7%, 0.8%, 0.9%, 1%, 1.1%, 1.2%, 1.3%, 1.4%, 1.5%, 1.6%, 1.7%, 1.8%, 1.9%, or 2%).

[0035] In this invention, the preferred values ​​are 30% ≤ x ≤ 35%, 5% ≤ y ≤ 15%, and 0.2% ≤ w ≤ 10%. This invention has found that if the value of x is too low and the value of y is too high, the hydrogen evolution catalytic performance of the cathode electrode will be significantly reduced. Further preferably, the atomic percentage ratio of Mo to Co is (0.8–1.8):1 (e.g., 0.8:1, 0.9:1, 1.0:1, 1.1:1, 1.2:1, 1.3:1). 1.4:1, 1.5:1, 1.6:1, 1.7:1 or 1.8:1), or the ratio of the atomic percentage of Mo to the atomic percentage of Ce is (0.8 to 1.8):1 (e.g. 0.8:1, 0.9:1, 1.0:1, 1.1:1, 1.2:1, 1.3:1, 1.4:1, 1.5:1, 1.6:1, 1.7:1 or 1.8:1), which is beneficial to ensuring that the cathode electrode has better hydrogen evolution catalytic performance.

[0036] According to some preferred embodiments, the high-entropy alloy formed on the metal matrix has a composition of Ni. 0.35 Cr 0.08 Mo 0.30 Co 0.20 Al 0.07 Ni 0.33 Cr 0.10 Mo 0.31 Co 0.20 Al (6-x)% High entropy alloys or Ni 0.33 Cr 0.08 Mo 0.28 Ce 0.22 Al 0.07 P 0.02 These high-entropy alloys exhibit superior hydrogen evolution catalytic performance; in Ni 0.33 Cr 0.10 Mo 0.31 Co 0.20 Al (6-x)% In high-entropy alloys, 0 < x ≤ 6, derived from Ni 0.33 Cr 0.10 Mo 0.31 Co 0.20 Al 0.06 High-entropy alloys are obtained through dealloying processes, in which Ni 0.33 Cr 0.10 Mo 0.31 Co 0.20 Al (6-x)% In high-entropy alloys, due to dealloying treatment, Al (6-x)% This refers to the aluminum remaining after the dealloying process. Before the dealloying process, the resulting high-entropy alloy is Ni. 0.33 Cr 0.10 Mo 0.31 Co 0.20 Al 0.06 .

[0037] According to some preferred embodiments, the high-entropy alloy is prepared by magnetron sputtering; preferably, the magnetron sputtering is magnetron co-sputtering.

[0038] According to some preferred embodiments, the high-entropy alloy is a porous high-entropy alloy, and the porous high-entropy alloy is prepared by: firstly, a high-entropy alloy is prepared on the surface of a metal substrate by magnetron sputtering, and then the high-entropy alloy formed on the surface of the metal substrate is subjected to dealloying treatment to obtain a porous high-entropy alloy.

[0039] According to some preferred embodiments, the process parameters for magnetron sputtering are: a base vacuum of no more than 5 × 10⁻⁶. -4 The process gas pressure is 0.4–0.7 Pa, and magnetron sputtering is performed using a DC power supply with a power of 40–140 W (e.g., 40, 50, 60, 70, 80, 90, 100, 110, 120, 130, or 140 W). The magnetron sputtering time is 30–100 min (e.g., 30, 40, 50, 60, 70, 80, 90, or 100 min). In this invention, during magnetron sputtering, the sputtering angle of the sputtering gun is at an angle of 65–90° to the horizontal direction. Changing the sputtering angle directly alters the distance between the target and the metal substrate, affecting the concentration range of element deposition and resulting in different concentration ranges of deposited elements, exhibiting compositional gradient characteristics. This is a conventional technique in the art, and those skilled in the art can understand it. The selection is made according to needs; preferably, the target is subjected to ion bombardment glow discharge cleaning before the high-entropy alloy is prepared on the surface of the metal substrate; preferably, in this invention, when the high-entropy alloy does not contain P or S, the magnetron sputtering temperature is room temperature, for example, room temperature 15-35°C; when the high-entropy alloy contains P and / or S elements, the magnetron sputtering temperature is 180-200°C; in this invention, when the high-entropy alloy contains P, the sputtering target is NiP (nickel phosphide); when the high-entropy alloy contains S, the sputtering target is NiS (nickel sulfide); when the high-entropy alloy contains each metal element, the sputtering target is a pure metal target of the single element corresponding to the metal component, that is, the sputtering target used is an elemental metal target corresponding to each metal element; of course, for the metal elements Ni and Cr, an alloy target can also be used.

[0040] According to some preferred embodiments, the dealloying treatment is as follows: immersing the high-entropy alloy formed on the surface of the metal substrate in a sodium hydroxide solution with a concentration of 0.05–0.15 mol / L for 1–3 hours; preferably, immersing the high-entropy alloy formed on the surface of the metal substrate in a sodium hydroxide solution (aqueous sodium hydroxide solution) with a concentration of 0.1 mol / L for 2 hours; the thickness of the high-entropy alloy is 0.6–8 μm (e.g., 0.6, 0.7, 0.8, 0.9, 1, 2, 3, 4, 5, 6, 7, or 8 μm); the metal substrate is nickel or stainless steel; and / or preferably, the nickel is nickel plate, nickel mesh, or nickel foam, and the stainless steel is 304L stainless steel, 316 stainless steel, or 316L stainless steel. In this invention, the main purpose of choosing nickel foam as the metal substrate is to further improve the hydrogen evolution catalytic performance of the cathode electrode, and the main purpose of choosing stainless steel as the metal substrate is to further improve the corrosion resistance of the cathode electrode in high COD wastewater. Both nickel foam and stainless steel are good conductors, which is beneficial to the magnetron sputtering deposition of high-entropy alloys. Preferably, the thickness of the metal substrate is 1 to 3 mm, more preferably 2 mm.

[0041] In a second aspect, the present invention provides a method for preparing the cathode electrode for hydrogen production from wastewater as described in the first aspect, the method comprising the following steps:

[0042] (1) Surface pretreatment of the metal substrate;

[0043] (2) A high-entropy alloy is prepared on the surface of the metal substrate after step (1) by magnetron sputtering; optionally, the high-entropy alloy formed on the surface of the metal substrate is subjected to dealloying treatment.

[0044] According to some specific embodiments, the cathode electrode for hydrogen production by wastewater electrolysis is prepared as follows:

[0045] ① Perform surface pretreatment on the metal substrate (pre-coated workpiece). When using nickel foam as the metal substrate, only acetone is used to remove surface oil. When using stainless steel as the metal substrate, it needs to be sanded before using acetone for degreasing. Based on the composition of the high-entropy alloy, use elemental metal targets, phosphide and / or sulfide targets as sputtering targets. Use a DC power supply, and after closing the vacuum chamber, evacuate to 5×10⁻⁶. -4 Below Pa (baseline vacuum), high-purity argon gas is introduced and adjusted to the required negative pressure (i.e., reaching the process gas pressure of 0.4-0.7 Pa). Pre-sputtering for 10-20 minutes is performed to conduct ion bombardment glow discharge cleaning of the target material, which can clean the target surface, mainly removing oxides or contaminants, and is conducive to forming a target sputtering environment. The elemental metal target contains five or more elements from Ni, Zr, Ti, Cr, Mo, Co, Ce, and Al (Ni and Al must be included). When phosphating or sulfidation treatment is required, NiS or NiP is selected as one of the sputtering targets. The purity of the argon gas is 99.99%, and the purity of the sputtering target is not less than 99.99%.

[0046] ② After ion bombardment glow discharge cleaning, when the selected sputtering targets are all elemental metal targets, the pre-coated workpiece is not heated, and the sputtering temperature is room temperature; when the selected sputtering targets contain NiS or NiP, the pre-coated workpiece needs to be heated to 180-200℃, and the sputtering temperature is 180-200℃; after reaching the required temperature, high-purity argon is introduced as the process gas, and the process gas pressure in the vacuum chamber is maintained at 0.4-0.7 Pa, the DC power supply power is 40-140 W, and the deposition time is 30-100 min; in this invention, when the selected sputtering targets contain NiS or NiP, heating the pre-coated workpiece is beneficial to film crystallization and optimizes the conductivity and crystal structure of the high-entropy alloy.

[0047] ③ The high-entropy alloy sputtered on the metal substrate by magnetron sputtering is subjected to dealloying treatment to form a porous self-supporting electrode (porous high-entropy alloy); In this invention, dealloying refers to the preferential dissolution or precipitation of the active component of an alloy with different chemical potential components under certain corrosion conditions. The porous self-supporting electrode after dealloying treatment in this invention has a porous nanostructure catalytic interface with a high specific surface area and has excellent catalytic performance; Specifically, in this invention, the metal substrate and the high-entropy alloy formed on the surface of the metal substrate are immersed in a sodium hydroxide solution for dealloying treatment.

[0048] This invention does not specifically limit the equipment used for magnetron sputtering, as it is conventional technology in the field. The magnetron sputtering equipment used can be, for example, a continuous multi-chamber magnetron sputtering coating system. This system may consist of a vacuum system, a cathode system, a substrate heating and temperature control system, a water cooling system, a PLC control system, a gas flow control and distribution system, and a power supply system. The ultimate vacuum level of the vacuum system is 2.0 × 10⁻⁶. -4 Pa, meaning the background vacuum can be controlled at 2.0 × 10⁻⁶. -4 ~5.0×10 -4 Pa, the power supply system adopts a programmable DC pulse power supply with a rated power of 15kW, which can independently control multiple target positions; in this invention, the target material used can be, for example, a circular target material with a diameter of 50mm, and the target material utilization rate is greater than 35%.

[0049] In a third aspect, the present invention provides a method for designing the composition of a cathode electrode for hydrogen production by wastewater electrolysis. Preferably, the cathode electrode for hydrogen production by wastewater electrolysis described in the first aspect of the present invention is determined by the composition design method described in the present invention, the composition design method comprising the following steps:

[0050] S1. A high-entropy alloy with a compositional gradient distribution is prepared on the surface of a metal substrate by magnetron sputtering. The high-entropy alloy is then cut into multiple samples. The microstructure of each cut sample is observed by scanning electron microscopy, and the elemental composition of each cut sample is recorded by energy dispersive X-ray spectroscopy (EDS) or X-ray photoelectron spectroscopy (XPS). The electrochemical characteristics of each cut sample are also tested using a three-electrode system. In this invention, a high-entropy alloy with a compositional gradient distribution is prepared on the surface of a metal substrate using magnetron sputtering at high throughput. In this invention, a high-entropy alloy with a compositional gradient distribution refers to an alloy with a gradient distribution in a planar direction. For example, in a square material, the Ni content can be controlled from left to right within the range of 5% to 30%, and the Co content can be controlled from the range of 10% to 20%. During magnetron sputtering, the sputtering gun is adjusted... The angle is adjusted to allow the deposited high-entropy alloy to exhibit a gradient distribution of component concentration, a conventional technique in the field that achieves high-throughput preparation. Those skilled in the art can select the appropriate angle based on the target range. In this invention, for example, the high-entropy alloy can be cut into multiple samples of 1cm (length) × 1cm (width). In this invention, the three-electrode system includes a working electrode, a reference electrode, a counter electrode, and an electrolyte. The working electrode is a cut high-entropy alloy sample formed on the surface of a metal substrate; the reference electrode is an Ag / AgCl electrode and / or a calomel electrode; the counter electrode is a Pt electrode, a graphite electrode, and / or a titanium electrode. The electrolyte is COD wastewater of all pH values, specifically, high-COD wastewater of all pH values ​​(pH 0–14). In this invention, the high-COD wastewater can, for example, be wastewater with a COD content of 1000–50000 mg / L.

[0051] S2. Collect known data on high-entropy alloys and establish a database. The data on high-entropy alloys includes the entropy value of the cut sample, elemental composition, physicochemical properties of the elements, surface microstructure characteristics, preparation information, electrochemical characteristics, and catalytic conditions for testing electrochemical characteristics. In this invention, the elemental composition includes the types of elements contained in the cut sample and the atomic ratio of each element.

[0052] S3. The collected data is filtered and normalized to construct a machine learning prediction model that uses the preparation information, elemental composition, physicochemical properties of elements, surface microstructure characteristics, entropy value, and catalytic conditions of the high-entropy alloy as input information and the electrochemical characteristics of the high-entropy alloy as output information. In this invention, the filtering involves deleting indistinguishable features and outliers, and the normalization process includes maximum and minimum value normalization and / or Z-score normalization. The algorithms involved include one or more of linear regression, logistic regression, random forest, support vector machine, and K-nearest neighbor algorithm, and the accuracy evaluation index is one or more of F1 score, PRC curve, and ROC curve.

[0053] S4. The machine learning prediction model is trained. When the training accuracy reaches the target, the target machine learning prediction model (i.e., the trained machine learning prediction model) is obtained. Then, the target machine learning prediction model is used to predict the electrochemical characteristics of the cut sample, thereby obtaining the composition of multiple high-entropy alloys with excellent catalytic performance formed on the surface of the metal matrix, that is, the composition of the cathode electrode with excellent catalytic performance for hydrogen production by wastewater electrolysis; In this invention, the database contains no less than 150 data points of high-entropy alloys; The database includes a training set and a test set, and the ratio of the number of data in the training set to the test set is 8:2; In this invention, the training accuracy is no less than 90%, that is, when the machine learning prediction model is trained and the correct prediction rate of the machine learning prediction model on the test set is above 90%, the training accuracy can be considered to have reached the target, and the target machine learning prediction model is obtained.

[0054] The purpose of this invention is to propose a cathode electrode for hydrogen production via wastewater electrolysis and its composition design method. The cathode electrode composition design method of this invention comprises two parts: high-throughput preparation of high-entropy alloys and machine learning, combining the development of cathode electrode materials for hydrogen production via wastewater electrolysis with the field of machine learning. High-throughput preparation of high-entropy alloys utilizes magnetron sputtering technology, which can prepare high-entropy alloys with compositional gradient distributions on the surface of a metal substrate and provide a large dataset for machine learning. Simultaneously, the high-entropy alloys prepared on the metal substrate surface using this technology exhibit high strength, high hardness, high catalytic activity, and excellent corrosion resistance, enabling them to operate stably in wastewater environments for extended periods. This invention fully leverages the advantages of high-throughput magnetron sputtering to deposit various multi-component high-entropy alloys on the surface of a metal substrate for hydrogen production via wastewater electrolysis. A database was constructed by collecting microstructure and catalytic performance information of the high-entropy alloys. Based on this database, machine learning techniques were applied to build a model. By inputting data including the surface microstructure characteristics of the high-entropy alloys, the model rapidly outputs the hydrogen evolution catalytic performance (electrochemical characteristics) of the high-entropy alloys, thereby enabling the design of high-entropy alloy composition and selection of element ratios in the cathode electrode. This invention innovatively establishes the relationship between the surface microstructure characteristics and electrochemical characteristics of high-entropy alloys through a machine learning prediction model.

[0055] This invention is of great significance. First, it provides an innovative method for designing and optimizing cathode electrode materials for hydrogen production by wastewater electrolysis. Second, by combining high-throughput preparation and machine learning, this method can efficiently screen for the optimal high-entropy alloy combination, thereby improving catalytic performance and corrosion resistance. This has a positive impact on promoting the development of hydrogen production technology by wastewater electrolysis, reducing preparation costs, improving energy conversion efficiency, and achieving sustainable energy production. The composition design method includes high-throughput preparation of high-entropy alloys and rapid screening of high-entropy alloy components with excellent performance using machine learning methods; the cathode electrode includes a metal substrate and a high-entropy alloy deposited on the surface of the metal substrate; the high-throughput preparation method is magnetron sputtering technology; the high-entropy alloy is prepared by magnetron sputtering using five or six or more of Ni-Zr-Ti-Cr-Mo-Co-Ce-Al-PS as raw materials, specifically, the high-entropy alloy contains Ni and Al, and also contains three or more other elements selected from Zr, Ti, Cr, Mo, Co, Ce, P, and S; the database source for the machine learning is the surface microstructure information and electrochemical performance data of the prepared high-entropy alloy.

[0056] According to some preferred embodiments, after the target machine learning prediction model obtains the composition of multiple cathode electrodes with excellent catalytic performance for wastewater electrolysis hydrogen production, multiple cathode electrodes with excellent catalytic performance (i.e., multiple high-entropy alloys with excellent catalytic performance formed on the surface of a metal substrate) with the same composition are prepared. These cathode electrodes are then used in long-term experiments for wastewater electrolysis hydrogen production. The relevant experimental data from the long-term experiments are input into the database of step S2, and the target machine learning prediction model is used for active learning to further enhance the accuracy of the predictions. The wastewater is, for example, industrial wastewater. Specifically, after the target machine learning prediction model obtains the composition of multiple cathode electrodes with excellent catalytic performance for wastewater electrolysis hydrogen production, multiple cathode electrodes with the same composition and excellent catalytic performance for wastewater electrolysis hydrogen production are prepared using vacuum arc melting, thermal spraying, ball milling, or magnetron sputtering methods. The cathode electrodes prepared by different methods are simultaneously subjected to long-term tests to evaluate catalytic performance, corrosion resistance, preparation cost, and service performance, screening out a long-life high-entropy alloy composition and preparation method more suitable for industrial applications. Preferably, the current density of the long-term test is not less than 250 mA / cm². 2 The long-term test duration is not less than 1000 hours; preferably, the long-term test is conducted in high COD wastewater, such as high COD wastewater containing chlorine or organic matter; preferably, the relevant experimental data of the long-term test include the measured catalytic performance of the cathode electrode (i.e., hydrogen evolution catalytic performance) and the recorded surface microstructure and physicochemical characteristics of the cathode electrode sample; the hydrogen evolution catalytic performance mainly includes the measured overpotential of the cathode electrode.

[0057] According to some preferred embodiments, the electrochemical features include active surface area and overpotential; and / or, when constructing a machine learning prediction model, the surface micromorphology features are digitized through machine learning to obtain information on lattice spacing, number of defects, number of pores, and specific surface area.

[0058] The present invention provides, in a fourth aspect, the application of the cathode electrode for hydrogen production by wastewater electrolysis as described in the first aspect of the present invention, or the cathode electrode for hydrogen production by wastewater electrolysis obtained by the composition design method described in the third aspect of the present invention, in hydrogen production by wastewater electrolysis.

[0059] The present invention will be further described below by way of examples, but the scope of protection of the present invention is not limited to these embodiments.

[0060] Example 1

[0061] ① The nickel foam substrate (metal matrix) is pretreated by degreasing; elemental metal targets corresponding to Ni, Cr, Mo, Co, and Al are used as sputtering cathodes, and DC power is used for sputtering. The atomic percentage distribution range of Ni, Cr, Mo, Co, and Al is controlled by adjusting the sputtering angle of the sputtering gun as follows: Ni 5-35%, Cr 5-30%, Mo 10-30%, Co 10-30%, and Al 0.2-10%; vacuum is then applied to a background vacuum of 5×10⁻⁶. -4 Below Pa, high-purity argon gas was introduced to adjust to the required negative pressure of 0.5 Pa, and pre-sputtering was performed at room temperature (25°C) for 10 min to perform ion bombardment glow cleaning on each target material. High-purity argon gas was continued to be introduced as the process gas, maintaining the process gas pressure in the vacuum chamber at 0.5 Pa, the DC power supply power (i.e., the target sputtering power) at 40–140 W, the sputtering angle of the sputtering gun at an angle of 65–90° to the horizontal direction, and the magnetron sputtering deposition time at room temperature (25°C) for 40 min, resulting in a high-entropy alloy with a compositional gradient distribution and a thickness of 2 μm on the metal substrate. This metal substrate and the high-entropy alloy deposited on the metal substrate together serve as the cathode electrode material.

[0062] ② The obtained cathode electrode material was cut into multiple samples of 1cm (length) × 1cm (width) (referred to as cut samples); the microstructure of each cut sample was observed by scanning electron microscopy, the elemental composition of each cut sample was recorded by X-ray energy dispersive spectroscopy (EDS), and the electrochemical characteristics of each cut sample were tested by a three-electrode system; the electrochemical characteristics included overpotential and active surface area; in the three-electrode system, Pt electrode was used as counter electrode, Ag / AgCl as reference electrode, cut sample as working electrode, and electrolyte was high COD wastewater at full pH (oilfield wastewater with COD content of 4000mg / L), and the overpotential and active surface area were recorded.

[0063] ③ Collect known data on high-entropy alloys and establish a database. This data includes the entropy value, elemental composition, physicochemical properties of the elements, surface microstructure characteristics, preparation information (magnetron sputtering (PVD) preparation conditions), electrochemical characteristics, and catalytic conditions for testing electrochemical characteristics of the cut samples. The collected data is screened and normalized to construct a machine learning prediction model. This model uses the high-entropy alloy's preparation information, elemental composition, physicochemical properties of the elements, surface microstructure characteristics, entropy value, and catalytic conditions as input information, and the high-entropy alloy's electrochemical characteristics as output information. During the construction of the machine learning prediction model, the surface microstructure characteristics are digitized using machine learning to obtain the high-entropy alloy's lattice spacing, number of defects, number of pores, and specific surface area. The machine learning prediction model is trained, and when the training accuracy reaches the target, a target machine learning prediction model is obtained. This target model is then used to predict the electrochemical characteristics of the cut samples, combining the digitized information with catalytic conditions to predict the electrochemical characteristics. The Ni value is then obtained through machine learning comparison. 0.35 Cr 0.08 Mo 0.30 Co 0.20 Al 0.07 High-entropy alloys exhibit optimal catalytic performance.

[0064] ④ After obtaining the high-entropy alloy of the cathode electrode for hydrogen production from wastewater with the best catalytic performance in step ③, a Ni alloy is precisely formed on the nickel foam substrate by magnetron sputtering. 0.35 Cr 0.08 Mo 0.30 Co 0.20 Al 0.07 A high-entropy alloy was used to obtain a cathode electrode for hydrogen production by wastewater electrolysis. Specifically, the nickel foam substrate (metal matrix) was pretreated by degreasing, and Ni, Cr, Mo, Co and Al targets with a purity of 99.99% were used as target materials. The vacuum was evacuated to a base vacuum of 5 × 10⁻⁶. -4 Below Pa, high-purity argon gas was introduced to adjust to the required negative pressure of 0.5 Pa. Each target was pre-sputtered at room temperature (25°C) for 10 minutes to perform ion bombardment glow discharge cleaning. High-purity argon gas was then introduced as the process gas, maintaining the process gas pressure in the vacuum chamber at 0.5 Pa. The sputtering power was then adjusted to 75 W for the Ni target, 85 W for the Cr target, 74 W for the Mo target, 57 W for the Co target, and 68 W for the Al target. The sputtering angle of the sputtering gun was 90° to the horizontal direction. Sputtering was performed at room temperature (25°C) for 40 minutes, forming a Ni-containing substrate (metal matrix) on the pre-treated foamed nickel substrate (metal matrix). 0.35 Cr 0.08 Mo 0.30 Co 0.20Al 0.07 High-entropy alloys.

[0065] This embodiment uses the cathode electrode (foamed nickel matrix + Ni) obtained in step ④ for hydrogen production from wastewater electrolysis. 0.35 Cr 0.08 Mo 0.30 Co 0.20 Al 0.07 The catalytic performance of the cathode electrode (high-entropy alloy electrode layer) was tested in a three-electrode system: In the three-electrode system, a Pt electrode was used as the counter electrode, Ag / AgCl was used as the reference electrode, and the cathode electrode obtained in step ④ for hydrogen production by wastewater electrolysis was used as the working electrode. The electrolyte was oilfield wastewater (high COD wastewater) with a pH of 8 and a COD content of 4000 mg / L; the current density in the wastewater was 10 mA / cm². 2 Under the specified conditions, the overpotential of the cathode electrode was measured to be 47 mV, and the active surface area was 51 m². 2 / g, and the current density in the wastewater is 250mA / cm. 2 After a long-term experiment of 1000 hours under the specified conditions, the overpotential decay was measured to be 9.4%, and the results are shown in Table 1.

[0066] Example 2

[0067] ① The nickel foam substrate (metal matrix) is pretreated by degreasing; elemental metal targets of Ni, Cr, Mo, Co, and Al are used as sputtering cathodes, and DC power is used for sputtering. The atomic percentage distribution range of Ni, Cr, Mo, Co, and Al is controlled by adjusting the sputtering angle of the sputtering gun as follows: Ni 5-35%, Cr 5-30%, Mo 10-35%, Co 10-30%, and Al 0.2-10%; vacuum is then applied to a background vacuum of 5×10⁻⁶. -4 Below Pa, high-purity argon gas was introduced to adjust to the required negative pressure of 0.5 Pa, and pre-sputtering was performed at room temperature (25°C) for 10 min to perform ion bombardment glow discharge cleaning on each target material. High-purity argon gas was continued to be introduced as the process gas, maintaining the process gas pressure in the vacuum chamber at 0.5 Pa, the DC power supply power at 40-140 W, the sputtering angle of the sputtering gun at an angle of 65-90° to the horizontal direction, and the magnetron sputtering deposition time at room temperature (25°C) for 40 min, resulting in a high-entropy alloy with a compositional gradient distribution and a thickness of 2 μm on the metal substrate. The high-entropy alloy obtained on the metal substrate was immersed in a 0.1 mol / L NaOH aqueous solution for 2 h for dealloying treatment to obtain the cathode electrode material.

[0068] ② The obtained cathode electrode material was cut into multiple samples of 1cm (length) × 1cm (width) (referred to as cut samples); the microstructure of each cut sample was observed by scanning electron microscopy, the elemental composition of each cut sample was recorded by X-ray energy dispersive spectroscopy, and the electrochemical characteristics of each cut sample were tested by a three-electrode system; the electrochemical characteristics included overpotential and active surface area; in the three-electrode system, Pt electrode was used as counter electrode, Ag / AgCl as reference electrode, cut sample as working electrode, and electrolyte was high COD wastewater at full pH (oilfield wastewater with COD content of 4000mg / L), and the overpotential and active surface area were recorded.

[0069] ③ Collect known data on high-entropy alloys and establish a database. This data includes the entropy value, elemental composition, physicochemical properties of the elements, surface microstructure characteristics, preparation information (magnetron sputtering (PVD) preparation conditions), electrochemical characteristics, and catalytic conditions for testing electrochemical characteristics of the cut samples. The collected data is screened and normalized to construct a machine learning prediction model. This model uses the high-entropy alloy's preparation information, elemental composition, physicochemical properties of the elements, surface microstructure characteristics, entropy value, and catalytic conditions as input information, and the high-entropy alloy's electrochemical characteristics as output information. During the construction of the machine learning prediction model, the surface microstructure characteristics are digitized using machine learning to obtain the high-entropy alloy's lattice spacing, number of defects, number of pores, and specific surface area. The machine learning prediction model is trained, and when the training accuracy reaches the target, a target machine learning prediction model is obtained. This target model is then used to predict the electrochemical characteristics of the cut samples, combining the digitized information with catalytic conditions to predict the electrochemical characteristics. The Ni value is then obtained through machine learning comparison. 0.33 Cr 0.10 Mo 0.31 Co 0.20 Al (6-x)% High-entropy alloys with (0 < x ≤ 6) exhibit optimal catalytic performance in this Ni 0.33 Cr 0.10 Mo 0.31 Co 0.20 Al (6-x)% In high-entropy alloys, due to dealloying treatment, Al (6-x)% This refers to the aluminum remaining after the dealloying process. Before the dealloying process, the resulting high-entropy alloy is Ni. 0.33 Cr 0.10 Mo 0.31 Co 0.20 Al 0.06 .

[0070] ④ After obtaining the high-entropy alloy of the cathode electrode for hydrogen production from wastewater with the best catalytic performance in step ③, a Ni alloy is precisely formed on the nickel foam substrate by magnetron sputtering. 0.33 Cr 0.10 Mo 0.31 Co 0.20 Al 0.06 A high-entropy alloy, then Ni formed on a nickel foam substrate. 0.33 Cr 0.10 Mo 0.31 Co 0.20 Al 0.06 The high-entropy alloy was immersed in a 0.1 mol / L NaOH aqueous solution for 2 hours to undergo dealloying treatment to obtain Ni. 0.33 Cr 0.10 Mo 0.31 Co 0.20 Al (6-x)% (0<x≤6) High-entropy alloy, used as the cathode electrode for hydrogen production by wastewater electrolysis; the specific magnetron sputtering process is as follows: The foamed nickel substrate (metal matrix) undergoes degreasing pretreatment, and each target material is pre-sputtered at room temperature (25℃) for 10 minutes to perform ion bombardment glow discharge cleaning. The foamed nickel substrate (metal matrix) undergoes degreasing pretreatment, using Ni, Cr, Mo, Co, and Al targets with a purity of 99.99% as the target materials. The vacuum is evacuated to a base vacuum of 5×10⁻⁶. -4 Below Pa, high-purity argon gas was introduced to adjust to the required negative pressure of 0.5 Pa. Each target was pre-sputtered at room temperature (25°C) for 10 minutes to perform ion bombardment glow discharge cleaning. High-purity argon gas was then introduced as the process gas, maintaining the process gas pressure in the vacuum chamber at 0.5 Pa. The sputtering power was then adjusted to 72 W for the Ni target, 85 W for the Cr target, 77 W for the Mo target, 50 W for the Co target, and 65 W for the Al target. The sputtering angle of the sputtering gun was 90° to the horizontal direction. Sputtering was performed at room temperature (25°C) for 40 minutes, forming a Ni-containing substrate (metal matrix) on the pre-treated foamed nickel substrate (metal matrix). 0.33 Cr 0.10 Mo 0.31 Co 0.20 Al 0.06 High-entropy alloys.

[0071] This embodiment uses the cathode electrode (foamed nickel matrix + Ni) obtained in step ④ for hydrogen production from wastewater electrolysis. 0.33 Cr 0.10 Mo 0.31 Co 0.20 Al (6-x)%The catalytic performance of the cathode electrode (high-entropy alloy electrode layer) was tested in a three-electrode system: In the three-electrode system, a Pt electrode was used as the counter electrode, Ag / AgCl was used as the reference electrode, and the cathode electrode obtained in step ④ for hydrogen production by wastewater electrolysis was used as the working electrode. The electrolyte was oilfield wastewater (high COD wastewater) with a pH of 8 and a COD content of 4000 mg / L; the current density in the wastewater was 10 mA / cm². 2 Under the specified conditions, the overpotential of the cathode electrode was measured to be 39 mV, and the active surface area was 57 m². 2 / g, and the current density in the wastewater is 250mA / cm. 2 After a long-term experiment of 1000 hours under the specified conditions, the overpotential decay was measured to be 12.3%, and the results are shown in Table 1.

[0072] Example 3

[0073] ① The nickel foam substrate (metal matrix) is pretreated by degreasing; elemental metal targets of Ni, Cr, Mo, Co, and Al, and NiP targets are used as sputtering cathodes, and DC power is used for sputtering. The composition gradient distribution range of the atomic percentages of Ni, Cr, Mo, Ce, and Al is controlled by adjusting the sputtering angle of the sputtering gun as follows: Ni 5-35%, Cr 5-30%, Mo 10-30%, Ce 10-30%, Al 0.2-10%, and P 0.3-2%; vacuum is evacuated to a background vacuum of 5×10⁻⁶. -4 Below Pa, high-purity argon gas was introduced to adjust to the required negative pressure of 0.5 Pa, and then pre-sputtered at room temperature (25°C) for 10 min to perform ion bombardment glow discharge cleaning on each target material. The degreasing pre-treated foamed nickel substrate was heated to 200°C, and high-purity argon gas was continued to be introduced as the process gas, maintaining the process gas pressure in the vacuum chamber at 0.5 Pa, the DC power supply power at 40-140 W, and the sputtering angle of the sputtering gun at an angle of 65-90° to the horizontal direction. Magnetron sputtering deposition was performed at 200°C for 40 min to obtain a high-entropy alloy with a compositional gradient distribution and a thickness of 2 μm on the metal substrate. This metal substrate and the high-entropy alloy deposited on the metal substrate together served as the cathode electrode material.

[0074] ② The obtained cathode electrode material was cut into multiple samples of 1cm (length) × 1cm (width) (referred to as cut samples); the microstructure of each cut sample was observed by scanning electron microscopy, the elemental composition of each cut sample was recorded by X-ray energy dispersive spectroscopy, and the electrochemical characteristics of each cut sample were tested by a three-electrode system; the electrochemical characteristics included overpotential and active surface area; in the three-electrode system, Pt electrode was used as counter electrode, Ag / AgCl as reference electrode, cut sample as working electrode, and electrolyte was high COD wastewater at full pH (oilfield wastewater with COD content of 4000mg / L), and the overpotential and active surface area were recorded.

[0075] ③ Collect known data on high-entropy alloys and establish a database. This data includes the entropy value, elemental composition, physicochemical properties of the elements, surface microstructure characteristics, preparation information (magnetron sputtering (PVD) preparation conditions), electrochemical characteristics, and catalytic conditions for testing electrochemical characteristics of the cut samples. The collected data is screened and normalized to construct a machine learning prediction model. This model uses the high-entropy alloy's preparation information, elemental composition, physicochemical properties of the elements, surface microstructure characteristics, entropy value, and catalytic conditions as input information, and the high-entropy alloy's electrochemical characteristics as output information. During the construction of the machine learning prediction model, the surface microstructure characteristics are digitized using machine learning to obtain the high-entropy alloy's lattice spacing, number of defects, number of pores, and specific surface area. The machine learning prediction model is trained, and when the training accuracy reaches the target, a target machine learning prediction model is obtained. This target model is then used to predict the electrochemical characteristics of the cut samples, combining the digitized information with catalytic conditions to predict the electrochemical characteristics. The Ni value is then obtained through machine learning comparison. 0.33 Cr 0.08 Mo 0.28 Ce 0.22 Al 0.07 P 0.02 High-entropy alloys exhibit optimal catalytic performance.

[0076] ④ After obtaining the high-entropy alloy of the cathode electrode for hydrogen production from wastewater with the best catalytic performance in step ③, a Ni alloy is precisely formed on the nickel foam substrate by magnetron sputtering. 0.33 Cr 0.08 Mo 0.28 Ce 0.22 Al 0.0 7P 0.02A high-entropy alloy was used to obtain a cathode electrode for hydrogen production by wastewater electrolysis. Specifically, the nickel foam substrate (metal matrix) was pretreated by degreasing, and Ni-Cr alloy targets (atomic percentage ratio of 4:1), Mo targets, Ce targets, Al targets, and NiP targets with a purity of 99.99% were used. The vacuum was evacuated to a base vacuum of 5 × 10⁻⁶. -4 Below Pa, high-purity argon gas was introduced to adjust to the required negative pressure of 0.5 Pa. Each target material was pre-sputtered at room temperature (25°C) for 10 minutes to perform ion bombardment glow discharge cleaning. The pre-treated foamed nickel substrate was heated to 200°C, and high-purity argon gas was continued to be introduced as the process gas, maintaining the process gas pressure in the vacuum chamber at 0.5 Pa. Then, the sputtering power of the Ni-Cr target was adjusted to 107 W, the Mo target to 71 W, the Ce target to 64 W, the Al target to 65 W, and the NiP target to 110 W. The sputtering angle of the sputtering gun was 90° to the horizontal direction, and sputtering was performed at 200°C for 40 minutes. This resulted in a Ni-based substrate (metal matrix) with a composition of Ni... 0.33 Cr 0.08 Mo 0.28 Ce 0.22 Al 0.0 7P 0.02 High-entropy alloys.

[0077] This embodiment uses the cathode electrode (foamed nickel matrix + Ni) obtained in step ④ for hydrogen production from wastewater electrolysis. 0.33 Cr 0.0 8Mo 0.28 Ce 0.22 Al 0.07 P 0.02 The catalytic performance of the cathode electrode (high-entropy alloy electrode layer) was tested in a three-electrode system: In the three-electrode system, a Pt electrode was used as the counter electrode, Ag / AgCl was used as the reference electrode, and the cathode electrode obtained in step ④ for hydrogen production by wastewater electrolysis was used as the working electrode. The electrolyte was oilfield wastewater (high COD wastewater) with a pH of 8 and a COD content of 4000 mg / L; the current density in the wastewater was 10 mA / cm². 2 Under the specified conditions, the overpotential of the cathode electrode was measured to be 42 mV, and the active surface area was 50 m². 2 / g, and the current density in the wastewater is 250mA / cm. 2 After a long-term experiment of 1000 hours under the specified conditions, the overpotential decay was measured to be 10.9%, and the results are shown in Table 1.

[0078] Example 4

[0079] ① First, the 316L stainless steel substrate (metal matrix) is sanded and then pre-treated with degreasing. Elemental metal targets containing Ni, Cr, Mo, Co, and Al are used as sputtering cathodes. DC power is used for sputtering. The atomic percentage distribution ranges of Ni, Cr, Mo, Co, and Al are controlled by adjusting the sputtering angle of the sputtering gun: Ni 5–35%, Cr 5–30%, Mo 10–30%, Co 10–30%, and Al 0.2–10%. The vacuum is then evacuated to a background vacuum of 5 × 10⁻⁶. -4 Below Pa, high-purity argon gas is introduced to adjust to the required negative pressure of 0.5 Pa, and then pre-sputtering is performed at room temperature (25°C) for 10 min to perform ion bombardment glow cleaning on each target material. High-purity argon gas is continued to be introduced as the process gas, maintaining the process gas pressure in the vacuum chamber at 0.5 Pa, the DC power supply power at 40-140 W, and the sputtering angle of the sputtering gun at an angle of 65-90° to the horizontal direction. Magnetron sputtering deposition is performed at room temperature (25°C) for 40 min to obtain a high-entropy alloy with a compositional gradient distribution and a thickness of 2 μm on the metal substrate. This metal substrate and the high-entropy alloy deposited on the metal substrate are used together as the cathode electrode material.

[0080] ② The obtained cathode electrode material was cut into multiple samples of 1cm (length) × 1cm (width) (referred to as cut samples); the microstructure of each cut sample was observed by scanning electron microscopy, the elemental composition of each cut sample was recorded by X-ray energy dispersive spectroscopy, and the electrochemical characteristics of each cut sample were tested by a three-electrode system; the electrochemical characteristics included overpotential and active surface area; in the three-electrode system, Pt electrode was used as counter electrode, Ag / AgCl as reference electrode, cut sample as working electrode, and electrolyte was high COD wastewater at full pH (oilfield wastewater with COD content of 4000mg / L), and the overpotential and active surface area were recorded.

[0081] ③ Collect known data on high-entropy alloys and establish a database. This data includes the entropy value, elemental composition, physicochemical properties of the elements, surface microstructure characteristics, preparation information (magnetron sputtering (PVD) preparation conditions), electrochemical characteristics, and catalytic conditions for testing electrochemical characteristics of the cut samples. The collected data is screened and normalized to construct a machine learning prediction model. This model uses the high-entropy alloy's preparation information, elemental composition, physicochemical properties of the elements, surface microstructure characteristics, entropy value, and catalytic conditions as input information, and the high-entropy alloy's electrochemical characteristics as output information. During the construction of the machine learning prediction model, the surface microstructure characteristics are digitized using machine learning to obtain the high-entropy alloy's lattice spacing, number of defects, number of pores, and specific surface area. The machine learning prediction model is trained, and when the training accuracy reaches the target, a target machine learning prediction model is obtained. This target model is then used to predict the electrochemical characteristics of the cut samples, combining the digitized information with catalytic conditions to predict the electrochemical characteristics. The Ni value is then obtained through machine learning comparison. 0.35 Cr 0.08 Mo 0.30 Co 0.20 Al 0.07 High-entropy alloys exhibit optimal catalytic performance.

[0082] ④ After obtaining the high-entropy alloy of the cathode electrode for hydrogen production from wastewater with the best catalytic performance in step ③, a Ni alloy is precisely formed on a 316L stainless steel substrate by magnetron sputtering. 0.35 Cr 0.08 Mo 0.30 Co 0.20 Al 0.07 A high-entropy alloy was used to obtain a cathode electrode for hydrogen production by wastewater electrolysis. Specifically, a 316L stainless steel substrate (metal matrix) was first polished with sandpaper, followed by degreasing pretreatment. Ni, Cr, Mo, Co, and Al targets, all with a purity of 99.99%, were used as target materials. The vacuum was evacuated to a base vacuum of 5 × 10⁻⁶. -4 Below Pa, high-purity argon gas was introduced to adjust to the required negative pressure of 0.5 Pa. Each target was pre-sputtered at room temperature (25°C) for 10 minutes to perform ion bombardment glow discharge cleaning. High-purity argon gas was then introduced as the process gas, maintaining the process gas pressure in the vacuum chamber at 0.5 Pa. The sputtering power was then adjusted to 75 W for Ni, 85 W for Cr, 74 W for Mo, 57 W for Co, and 68 W for Al. The sputtering angle of the sputtering gun was 90° to the horizontal direction. Sputtering was performed at room temperature (25°C) for 40 minutes, forming a Ni-containing matrix on the degreased 316L stainless steel substrate (metal matrix). 0.35 Cr 0.08 Mo0.30 Co 0.20 Al 0.07 High-entropy alloys.

[0083] This embodiment uses the cathode electrode (316L stainless steel substrate + Ni) obtained in step ④ for hydrogen production from wastewater electrolysis. 0.35 Cr 0.08 Mo 0.30 Co 0.20 Al 0.07 The catalytic performance of the cathode electrode (high-entropy alloy electrode layer) was tested in a three-electrode system: In the three-electrode system, a Pt electrode was used as the counter electrode, Ag / AgCl was used as the reference electrode, and the cathode electrode obtained in step ④ for hydrogen production by wastewater electrolysis was used as the working electrode. The electrolyte was oilfield wastewater (high COD wastewater) with a pH of 8 and a COD content of 4000 mg / L; the current density in the wastewater was 10 mA / cm². 2 Under the specified conditions, the overpotential of the cathode electrode was measured to be 51 mV, and the active surface area was 46 m². 2 / g, and the current density in the wastewater is 250mA / cm. 2 After a long-term experiment of 1000 hours under the specified conditions, the overpotential decay was measured to be 7.6%, and the results are shown in Table 1.

[0084] Example 5

[0085] ① The nickel foam substrate (metal matrix) is pretreated by degreasing; elemental metal targets of Ni, Cr, Mo, Co, and Al are used as sputtering cathodes, and DC power is used for sputtering. The atomic percentage distribution range of Ni, Cr, Mo, Co, and Al is controlled by adjusting the sputtering angle of the sputtering gun as follows: Ni 5-10%, Cr 5-30%, Mo 10-30%, Co 10-30%, Al 10-20%; vacuum is evacuated to a background vacuum of 5×10⁻⁶. -4 Below Pa, high-purity argon gas is introduced to adjust to the required negative pressure of 0.5 Pa, and then pre-sputtering is performed at room temperature (25°C) for 10 min to perform ion bombardment glow cleaning on each target material. High-purity argon gas is continued to be introduced as the process gas, maintaining the process gas pressure in the vacuum chamber at 0.5 Pa, the DC power supply power at 40-140 W, and the sputtering angle of the sputtering gun at an angle of 65-90° to the horizontal direction. Magnetron sputtering deposition is performed at room temperature (25°C) for 40 min to obtain a high-entropy alloy with a compositional gradient distribution and a thickness of 2 μm on the metal substrate. This metal substrate and the high-entropy alloy deposited on the metal substrate are used together as the cathode electrode material.

[0086] ② The obtained cathode electrode material was cut into multiple samples of 1cm (length) × 1cm (width) (referred to as cut samples); the microstructure of each cut sample was observed by scanning electron microscopy, the elemental composition of each cut sample was recorded by X-ray energy dispersive spectroscopy, and the electrochemical characteristics of each cut sample were tested by a three-electrode system; the electrochemical characteristics included overpotential and active surface area; in the three-electrode system, Pt electrode was used as counter electrode, Ag / AgCl as reference electrode, cut sample as working electrode, and electrolyte was high COD wastewater at full pH (oilfield wastewater with COD content of 4000mg / L), and the overpotential and active surface area were recorded.

[0087] ③ Collect known data on high-entropy alloys and establish a database. This data includes the entropy value, elemental composition, physicochemical properties of the elements, surface microstructure characteristics, preparation information (magnetron sputtering (PVD) preparation conditions), electrochemical characteristics, and catalytic conditions for testing electrochemical characteristics of the cut samples. The collected data is screened and normalized to construct a machine learning prediction model. This model uses the high-entropy alloy's preparation information, elemental composition, physicochemical properties of the elements, surface microstructure characteristics, entropy value, and catalytic conditions as input information, and the high-entropy alloy's electrochemical characteristics as output information. During the construction of the machine learning prediction model, the surface microstructure characteristics are digitized using machine learning to obtain the high-entropy alloy's lattice spacing, number of defects, number of pores, and specific surface area. The machine learning prediction model is trained, and when the training accuracy reaches the target, a target machine learning prediction model is obtained. This target model is then used to predict the electrochemical characteristics of the cut samples, combining the digitized information with catalytic conditions to predict the electrochemical characteristics. The Ni value is then obtained through machine learning comparison. 0.10 Cr 0.17 Mo 0.30 Co 0.30 Al 0.13 High-entropy alloys exhibit optimal catalytic performance.

[0088] ④ After obtaining the high-entropy alloy of the cathode electrode for hydrogen production from wastewater with the best catalytic performance in step ③, a Ni alloy is precisely formed on the nickel foam substrate by magnetron sputtering. 0.10 Cr 0.17 Mo 0.30 Co 0.30 Al 0.13 A high-entropy alloy was used to obtain a cathode electrode for hydrogen production by wastewater electrolysis. Specifically, the nickel foam substrate (metal matrix) was pretreated by degreasing, and Ni, Cr, Mo, Co and Al targets with a purity of 99.99% were used as target materials. The vacuum was evacuated to a base vacuum of 5 × 10⁻⁶. -4Below Pa, high-purity argon gas was introduced to adjust to the required negative pressure of 0.5 Pa. Each target material was pre-sputtered at room temperature (25°C) for 10 minutes to perform ion bombardment glow discharge cleaning. High-purity argon gas was then introduced as the process gas, maintaining the process gas pressure in the vacuum chamber at 0.5 Pa. The Ni target power was then adjusted to 43 W, the Cr target power to 97 W, the Mo target power to 80 W, the Co target power to 63 W, and the Al target power to 78 W. The sputtering angle of the sputtering gun was 90° to the horizontal direction, and sputtering was performed at room temperature (25°C) for 40 minutes. This resulted in a Ni-containing substrate (metal matrix) formed on the pre-treated foamed nickel substrate (metal matrix). 0.10 Cr 0.17 Mo 0.30 Co 0.30 Al 0.13 High-entropy alloys.

[0089] This embodiment uses the cathode electrode (foamed nickel matrix + Ni) obtained in step ④ for hydrogen production from wastewater electrolysis. 0.10 Cr 0.17 Mo 0.30 Co 0.30 Al 0.13 The catalytic performance of the cathode electrode (high-entropy alloy electrode layer) was tested in a three-electrode system: In the three-electrode system, a Pt electrode was used as the counter electrode, Ag / AgCl was used as the reference electrode, and the cathode electrode obtained in step ④ for hydrogen production by wastewater electrolysis was used as the working electrode. The electrolyte was oilfield wastewater (high COD wastewater) with a pH of 8 and a COD content of 4000 mg / L; the current density in the wastewater was 10 mA / cm². 2 Under the specified conditions, the overpotential of the cathode electrode was measured to be 174 mV, and the active surface area was 26 m². 2 / g, and the current density in the wastewater is 250mA / cm. 2 After a long-term experiment of 1000 hours under the specified conditions, the overpotential decay was measured to be 8.0%, and the results are shown in Table 1.

[0090] Example 6

[0091] ① The foamed nickel substrate (metal matrix) is pretreated by degreasing; elemental metal targets of Cu, Cr, Mo, Co, and Al are used as sputtering cathodes, and DC power is used for sputtering. The atomic percentage distribution range of Cu, Cr, Mo, Co, and Al is controlled by adjusting the sputtering angle of the sputtering gun as follows: Cu 5-35%, Cr 5-30%, Mo 10-30%, Co 10-30%, and Al 0.2-10%; vacuum is evacuated to a background vacuum of 5×10⁻⁶. -4Below Pa, high-purity argon gas is introduced to adjust to the required negative pressure of 0.5 Pa, and then pre-sputtering is performed at room temperature (25°C) for 10 min to perform ion bombardment glow cleaning on each target material. High-purity argon gas is continued to be introduced as the process gas, maintaining the process gas pressure in the vacuum chamber at 0.5 Pa, the DC power supply power at 40-140 W, and the sputtering angle of the sputtering gun at an angle of 65-90° to the horizontal direction. Magnetron sputtering deposition is performed at room temperature (25°C) for 40 min to obtain a high-entropy alloy with a compositional gradient distribution and a thickness of 2 μm on the metal substrate. This metal substrate and the high-entropy alloy deposited on the metal substrate are used together as the cathode electrode material.

[0092] ② The obtained cathode electrode material was cut into multiple samples of 1cm (length) × 1cm (width) (referred to as cut samples); the microstructure of each cut sample was observed by scanning electron microscopy, the elemental composition of each cut sample was recorded by X-ray energy dispersive spectroscopy, and the electrochemical characteristics of each cut sample were tested by a three-electrode system; the electrochemical characteristics included overpotential and active surface area; in the three-electrode system, Pt electrode was used as counter electrode, Ag / AgCl as reference electrode, cut sample as working electrode, and electrolyte was high COD wastewater at full pH (oilfield wastewater with COD content of 4000mg / L), and the overpotential and active surface area were recorded.

[0093] ③ Collect known data on high-entropy alloys and establish a database. This data includes the entropy value, elemental composition, physicochemical properties of the elements, surface microstructure characteristics, preparation information (magnetron sputtering (PVD) preparation conditions), electrochemical characteristics, and catalytic conditions for testing electrochemical characteristics of the cut samples. The collected data is screened and normalized to construct a machine learning prediction model. This model uses the high-entropy alloy's preparation information, elemental composition, physicochemical properties of the elements, surface microstructure characteristics, entropy value, and catalytic conditions as input information, and the high-entropy alloy's electrochemical characteristics as output information. During the construction of the machine learning prediction model, the surface microstructure characteristics are digitized using machine learning to obtain the high-entropy alloy's lattice spacing, number of defects, number of pores, and specific surface area. The machine learning prediction model is trained, and when the training accuracy reaches the target, a target machine learning prediction model is obtained. This target model is then used to predict the electrochemical characteristics of the cut samples, combining the digitized information with catalytic conditions to predict the electrochemical characteristics. The results are compared using machine learning to obtain the Cu... 0.20 Cr 0.12 Mo 0.30 Co 0.30 Al 0.08 High-entropy alloys exhibit optimal catalytic performance.

[0094] ④ After obtaining the high-entropy alloy of the cathode electrode for hydrogen production from wastewater electrolysis with the best catalytic performance in step ③, a Cu alloy is precisely formed on the nickel foam substrate by magnetron sputtering. 0.20 Cr 0.12 Mo 0.30 Co 0.30 Al 0.08 A high-entropy alloy was used to obtain a cathode electrode for hydrogen production by wastewater electrolysis. Specifically, the nickel foam substrate (metal matrix) was pretreated by degreasing, and Cu, Cr, Mo, Co, and Al targets with a purity of 99.99% were used as target materials. The vacuum was evacuated to a base vacuum of 5 × 10⁻⁶. -4 Below Pa, high-purity argon gas was introduced to adjust to the required negative pressure of 0.5 Pa. Each target was pre-sputtered at room temperature (25°C) for 10 minutes to perform ion bombardment glow discharge cleaning. High-purity argon gas was then introduced as the process gas, maintaining the process gas pressure in the vacuum chamber at 0.5 Pa. The sputtering power was then adjusted to 63 W for Cu, 88 W for Cr, 80 W for Mo, 63 W for Co, and 70 W for Al. The sputtering angle of the sputtering gun was 90° to the horizontal direction. Sputtering was performed at room temperature (25°C) for 40 minutes, forming a Cu-containing substrate (metal matrix) on the pre-treated foamed nickel substrate (metal matrix). 0.20 Cr 0.12 Mo 0.30 Co 0.30 Al 0.08 High-entropy alloys.

[0095] This embodiment uses the cathode electrode (foamed nickel matrix + Cu) obtained in step ④ for hydrogen production from wastewater electrolysis. 0.20 Cr 0.12 Mo 0.30 Co 0.30 Al 0.08 The catalytic performance of the cathode electrode (high-entropy alloy electrode layer) was tested in a three-electrode system: In the three-electrode system, a Pt electrode was used as the counter electrode, Ag / AgCl was used as the reference electrode, and the cathode electrode obtained in step ④ for hydrogen production by wastewater electrolysis was used as the working electrode. The electrolyte was oilfield wastewater (high COD wastewater) with a pH of 8 and a COD content of 4000 mg / L; the current density in the wastewater was 10 mA / cm². 2 Under the specified conditions, the overpotential of the cathode electrode was measured to be 219 mV, and the active surface area was 19 m². 2 / g, and the current density in the wastewater is 250mA / cm. 2 After a long-term experiment of 1000 hours under the specified conditions, the overpotential decay was measured to be 9.0%, and the results are shown in Table 1.

[0096] Comparative Example 1

[0097] A Cr was prepared according to Example 1 of Chinese Patent CN112609213B. 14.33 Fe 22.42 Co 17.77 Ni 17.61 Cu 27.87 (Also written as Cr) 0.1433 Fe 0.2242 Co 0.1777 Ni 0.1761 Cu 0.2787 High-entropy alloy porous electrodes are used as cathode electrodes.

[0098] In this comparative example, the catalytic performance of the obtained cathode electrode was tested in a three-electrode system: In the three-electrode system, a Pt electrode was used as the counter electrode, Ag / AgCl as the reference electrode, and the cathode electrode obtained in this comparative example was used as the working electrode. The electrolyte was oilfield wastewater (high COD wastewater) with a pH of 8 and a COD content of 4000 mg / L; the current density in the wastewater was 10 mA / cm². 2 Under the conditions specified, the overpotential and active surface area of ​​the cathode electrode were measured, as shown in Table 1. The current density in the wastewater was 250 mA / cm². 2 After a long-term experiment of 1000 hours under the specified conditions, the overpotential decay data were measured, and the results are shown in Table 1.

[0099] Comparative Example 2

[0100] Ni composition was precisely formed on a nickel foam substrate using magnetron sputtering. 0.35 Cr 0.08 Fe 0.30 Nb 0.20 Al 0.07 A high-entropy alloy was used to obtain the cathode electrode; specifically, the nickel foam (metal matrix) was pretreated by degreasing, and Ni, Cr, Fe, Nb and Al targets with a purity of 99.99% were used as target materials, and the vacuum was evacuated to a base vacuum of 5×10⁻⁶. -4 Below Pa, high-purity argon gas was introduced to adjust to the required negative pressure of 0.5 Pa. Each target was pre-sputtered at room temperature (25°C) for 10 minutes to perform ion bombardment glow discharge cleaning. High-purity argon gas was then introduced as the process gas, maintaining the process gas pressure in the vacuum chamber at 0.5 Pa. The sputtering power was then adjusted to 75 W for the Ni target, 85 W for the Cr target, 94 W for the Fe target, 113 W for the Nb target, and 70 W for the Al target. The sputtering angle of the sputtering gun was 90° to the horizontal direction. Sputtering was performed at room temperature (25°C) for 40 minutes, forming a Ni-containing substrate (metal matrix) on the pre-treated foamed nickel substrate (metal matrix). 0.35 Cr 0.08 Fe 0.30 Nb 0.20 Al0.07 High-entropy alloys.

[0101] The cathode electrode obtained in this comparative example (nickel foam matrix + Ni) 0.35 Cr 0.08 Fe 0.30 Nb 0.20 Al 0.07 The catalytic performance of the cathode electrode (high-entropy alloy electrode layer) was tested in a three-electrode system: In the three-electrode system, a Pt electrode was used as the counter electrode, Ag / AgCl was used as the reference electrode, and the cathode electrode obtained in this comparative example was used as the working electrode. The electrolyte was oilfield wastewater (high COD wastewater) with a pH of 8 and a COD content of 4000 mg / L; the current density in the wastewater was 10 mA / cm². 2 Under the conditions specified, the overpotential and active surface area of ​​the cathode electrode were measured, as shown in Table 1. The current density in the wastewater was 250 mA / cm². 2 After a long-term experiment of 1000 hours under the specified conditions, the overpotential decay data were measured, and the results are shown in Table 1.

[0102] Comparative Example 3

[0103] Ni composition was precisely formed on a nickel foam substrate using magnetron sputtering. 0.35 Cu 0.08 Fe 0.30 Co 0.20 Al 0.07 A high-entropy alloy was used to obtain the cathode electrode; specifically, the nickel foam (metal matrix) was pretreated by degreasing, and Ni, Cu, Fe, Co and Al targets with a purity of 99.99% were used as target materials. The vacuum was evacuated to a base vacuum of 5×10⁻⁶. -4 Below Pa, high-purity argon gas was introduced to adjust to the required negative pressure of 0.5 Pa. Each target material was pre-sputtered at room temperature (25°C) for 10 minutes to perform ion bombardment glow discharge cleaning. High-purity argon gas was then introduced as the process gas, maintaining the process gas pressure in the vacuum chamber at 0.5 Pa. The Ni target power was then adjusted to 75 W, Cu target power to 53 W, Fe target power to 95 W, Co target power to 58 W, and Al target power to 66 W. The sputtering angle of the sputtering gun was 90° to the horizontal direction, and sputtering was performed at room temperature (25°C) for 40 minutes. This resulted in a Ni-containing substrate (metal matrix) formed on the pre-treated foamed nickel substrate (metal matrix). 0.35 Cu 0.08 Fe 0.30 Co 0.20 Al 0.07 High-entropy alloys.

[0104] The cathode electrode obtained in this comparative example (nickel foam matrix + Ni) 0.35 Cu 0.08 Fe 0.30Co 0.20 Al 0.07 The catalytic performance of the cathode electrode (high-entropy alloy electrode layer) was tested in a three-electrode system: In the three-electrode system, a Pt electrode was used as the counter electrode, Ag / AgCl was used as the reference electrode, and the cathode electrode obtained in this comparative example was used as the working electrode. The electrolyte was oilfield wastewater (high COD wastewater) with a pH of 8 and a COD content of 4000 mg / L; the current density in the wastewater was 10 mA / cm². 2 Under the conditions specified, the potential and active surface area of ​​the cathode electrode were measured, as shown in Table 1. The current density in the wastewater was 250 mA / cm². 2 After a long-term experiment of 1000 hours under the specified conditions, the overpotential decay data were measured, and the results are shown in Table 1.

[0105] Table 1: Comparison of the effects of the cathode electrodes in Examples 1-6 and Comparative Examples 1-3 on hydrogen production from wastewater electrolysis.

[0106] Example Overpotential (mV) <![CDATA[active surface area (m 2 / g)]]> Potential decay (%) Example 1 47 51 9.4 Example 2 39 57 12.3 Example 3 42 50 10.9 Example 4 51 46 7.6 Example 5 174 26 8.0 Example 6 219 19 9.0 Comparative Example 1 117 33 16.4 Comparative Example 2 83 39 9.1 Comparative Example 3 63 44 18.8

[0107] The parts of this invention not described in detail are techniques known to those skilled in the art.

[0108] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, and are not intended to limit them. Although detailed descriptions have been made with reference to the foregoing embodiments, those skilled in the art should understand that modifications can still be made to the technical solutions described in the foregoing embodiments, or equivalent substitutions can be made to some of the technical features. Such modifications or substitutions do not cause the essence of the corresponding technical solutions to deviate from the spirit and scope of the technical solutions of the embodiments of the present invention.

Claims

1. A cathode electrode for hydrogen production by wastewater electrolysis, characterized in that: The cathode electrode for hydrogen production by wastewater electrolysis includes a metal substrate and a high-entropy alloy formed on the surface of the metal substrate. The high-entropy alloy contains Ni and Al, and the general formula for the composition of the high-entropy alloy is: Ni x A y B z Al w Where A is Cr, B is at least two of Mo, Co, Ce, P, and S; x, y, z, and w are atomic percentages, 5%≤x≤35%, 5%≤y≤35%, 10%≤z≤70%, 0.2%≤w≤10%, and x+y+z+w=100%.

2. The cathode electrode for hydrogen production by wastewater electrolysis according to claim 1, characterized in that: B represents Mo and Co, with 30%≤x≤35% and 5%≤y≤15%. In the high-entropy alloy, the atomic percentage of Mo is 25~35% and the atomic percentage of Co is 20~32%.

3. The cathode electrode for hydrogen production by wastewater electrolysis according to claim 1, characterized in that: B is Mo, Ce and P, or B is Mo, Ce and S, 30%≤x≤35%, 5%≤y≤15%, and in the high-entropy alloy, the atomic percentage of Mo is 25~35%, the atomic percentage of Ce is 20~32%, and the atomic percentage of P or S is 0.3~2%.

4. The cathode electrode for hydrogen production by wastewater electrolysis according to claim 1, characterized in that: The high-entropy alloy was prepared by magnetron sputtering.

5. The cathode electrode for hydrogen production by wastewater electrolysis according to claim 4, characterized in that: The magnetron sputtering is magnetron co-sputtering.

6. The cathode electrode for hydrogen production by wastewater electrolysis according to claim 5, characterized in that: The high-entropy alloy is a porous high-entropy alloy. The porous high-entropy alloy is prepared by first preparing a high-entropy alloy on the surface of a metal substrate by magnetron sputtering, and then performing a dealloying treatment on the high-entropy alloy formed on the surface of the metal substrate to obtain a porous high-entropy alloy.

7. The cathode electrode for hydrogen production by wastewater electrolysis according to claim 4, characterized in that: The process parameters for magnetron sputtering are: base vacuum not greater than 5 × 10⁻⁶. -4 The process gas pressure is 0.4~0.7Pa, and magnetron sputtering is performed using a DC power supply with a power of 40~140W. The magnetron sputtering time is 30~100min.

8. The cathode electrode for hydrogen production by wastewater electrolysis according to claim 7, characterized in that: When the high-entropy alloy contains P and / or S elements, the magnetron sputtering temperature is 180~200℃.

9. The cathode electrode for hydrogen production by wastewater electrolysis according to claim 6, characterized in that: The dealloying treatment is as follows: the high-entropy alloy formed on the surface of the metal substrate is immersed in a sodium hydroxide solution with a concentration of 0.05~0.15mol / L for 1~3 hours; The thickness of the high-entropy alloy is 0.6~8μm; The metal matrix is ​​nickel or stainless steel.

10. The cathode electrode for hydrogen production by wastewater electrolysis according to claim 9, characterized in that: The nickel is nickel plate, nickel mesh, or nickel foam, and the stainless steel is 304L stainless steel, 316 stainless steel, or 316L stainless steel.

11. A method for preparing a cathode electrode for hydrogen production by wastewater electrolysis according to any one of claims 1 to 10, characterized in that, The preparation method includes the following steps: (1) Surface pretreatment of the metal substrate; (2) A high-entropy alloy is prepared on the surface of the metal substrate after step (1) by magnetron sputtering.

12. The preparation method according to claim 11, characterized in that: The high-entropy alloy formed on the surface of the metal matrix is ​​subjected to a dealloying process.

13. A method for designing the composition of a cathode electrode for hydrogen production by wastewater electrolysis according to any one of claims 1 to 10, characterized in that, The component design method includes the following steps: S1. A high-entropy alloy with a compositional gradient distribution is prepared on the surface of a metal substrate by magnetron sputtering. The high-entropy alloy is then cut into multiple samples. The microstructure of each cut sample is observed by scanning electron microscopy. The elemental composition of each cut sample is recorded by X-ray energy dispersive spectroscopy or X-ray photoelectron spectroscopy. The electrochemical characteristics of each cut sample are tested by a three-electrode system. S2. Collect known data on high-entropy alloys and establish a database. The data on high-entropy alloys includes the entropy value of the cut sample, elemental composition, physicochemical properties of the elements, surface microstructure characteristics, preparation information, electrochemical characteristics, and catalytic conditions for testing electrochemical characteristics. S3. The collected data information is screened and normalized to construct a machine learning prediction model with the preparation information, elemental composition, physicochemical properties of elements, surface microstructure characteristics, entropy value and catalytic conditions of high-entropy alloy as input information and the electrochemical characteristics of high-entropy alloy as output information. S4. Train the machine learning prediction model. When the training accuracy reaches the target, obtain the target machine learning prediction model. Then, use the target machine learning prediction model to predict the electrochemical characteristics of the cut sample to obtain the composition of multiple cathode electrodes with excellent catalytic performance for hydrogen production by wastewater electrolysis.

14. The component design method according to claim 13, characterized in that: After obtaining the composition of multiple cathode electrodes with excellent catalytic performance for hydrogen production by wastewater electrolysis using the target machine learning prediction model, multiple cathode electrodes with the same composition and excellent catalytic performance are prepared. The cathode electrodes are then used in long-term experiments for hydrogen production by wastewater electrolysis. The relevant experimental data from the long-term experiments are input into the database of step S2, and the target machine learning prediction model is used for active learning to further enhance the accuracy of the predictions made by the target machine learning prediction model.

15. The component design method according to claim 14, characterized in that: The current density for long-term testing shall not be less than 250 mA / cm². 2 The long-term test duration shall not be less than 1000 hours.

16. The component design method according to claim 14, characterized in that: The relevant experimental data from the long-term test include the measured catalytic performance of the cathode electrode and the recorded surface microstructure and physicochemical characteristics of the cathode electrode sample.

17. The component design method according to claim 13, characterized in that: The electrochemical characteristics include active surface area and overpotential; and / or When constructing a machine learning prediction model, the surface micro-morphology features are digitized through machine learning to obtain information on lattice spacing, number of defects, number of pores, and specific surface area.

18. The application of the cathode electrode for hydrogen production by wastewater electrolysis according to any one of claims 1 to 10, or the cathode electrode for hydrogen production by wastewater electrolysis obtained by the composition design method according to any one of claims 13 to 17, in hydrogen production by wastewater electrolysis.

Citation Information

Patent Citations

  • High-entropy alloy porous electrode and its preparation method

    CN112609213B

  • Porous high-entropy alloy self-supporting electrode for electrolyzing water and preparation method thereof

    CN112725818A

  • FeCoNiBPt high-entropy amorphous alloy water electrolysis catalytic material and preparation method thereof

    CN115852390A