A method for forming silicon powder, silicon blocks and their applications
The problem of low loading density of native polycrystalline silicon powder was solved by pressure forming method. The prepared silicon blocks are easy to handle and crush, and efficient Czochralski single crystal production is realized.
Patent Information
- Application Number
- CN202311132123.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-09-04
- Publication Date
- 2026-11-10
- Estimated Expiration
- 2043-09-04
AI Technical Summary
The small particle size and low loading density of native polycrystalline silicon powder make it unsuitable for direct use in CZ Czochralski single crystal furnaces, affecting the amount of material loaded and production efficiency.
Silicon blocks are prepared by placing silicon powder under pressure P1 for a duration T1, satisfying 50MPa≤P1≤600MPa and 7min≤T1≤15min. The dry pressure technology is used to avoid pollution and improve production efficiency.
The prepared silicon blocks are easy to remove from the mold without breaking and generating dust. After breaking, the particle size distribution is controllable, and the density is increased to 0.18 g/cm3 to 0.25 g/cm3, which is suitable for Czochralski single crystal production.
Smart Images

Figure CN117067663B_ABST
Abstract
Description
Technical Field
[0001] This application belongs to the field of single crystal growth technology, specifically relating to a silicon powder forming method, silicon block and its application. Background Technology
[0002] Because the native polycrystalline silicon powder has a small particle size (0.1μm to 1000μm), its loading density is low, meaning that less weight is loaded in the same space. This directly affects the weight of the crucible before use in the CZ Czochralski single crystal furnace and makes it unusable in the CZ Czochralski single crystal furnace re-feeding (continuous feeding crystal pulling technology) process. Summary of the Invention
[0003] The purpose of this application is to provide a silicon powder forming method, silicon block and its application, which can solve the above-mentioned technical problems.
[0004] This application provides a method for forming silicon powder, including the following steps:
[0005] The mold containing silicon powder is placed under the first pressure P1 and maintained under the first pressure for a time T1, satisfying 50MPa≤P1≤600MPa and 7min≤T1≤15min, to obtain a silicon block.
[0006] In some embodiments, the first pressure P1 condition is achieved by increasing the pressure, and the pressure increasing step includes increasing the pressure to the first pressure P1 at a first pressure increasing rate v1, satisfying 20MPa / s≤v1≤30MPa / s.
[0007] In some embodiments, the mold containing silicon powder is placed before the first pressure condition P1, and the mold containing silicon powder is placed in a closed environment.
[0008] In some embodiments, the first pressure P1 condition is applied by a pressurizing medium, the pressurizing medium being a fluid, the mold containing silicon powder is placed before the first pressure P1 condition, and the mold containing silicon powder is placed in a cavity;
[0009] The mold and the pressurizing medium are separated by the cavity; or, the pressurizing medium is filled in the cavity and the mold is in contact with the pressurizing medium.
[0010] In some embodiments, when the mold and the pressurizing medium are separated by the cavity, the pressurizing medium is a liquid; when the pressurizing medium fills the cavity and the mold is in contact with the pressurizing medium, the pressurizing medium is a gas.
[0011] In some embodiments, when the mold and the pressurizing medium are separated by the cavity, the interior of the cavity is kept in a dry environment with a temperature range of 20–25°C and a humidity range of 40–50% RH.
[0012] In some embodiments, the particle size of the silicon powder is from 0.1 to 1000 μm.
[0013] In some embodiments, the mold includes a first surface and a second surface disposed opposite to each other, the first surface and the second surface being connected by a third surface, the first surface and the third surface receiving the first pressure P1.
[0014] In some embodiments, the first surface, the second surface, and the third surface receive the first pressure P1, and the pressure deviation PD of the first pressure P1 applied to the first surface, the second surface, and the third surface satisfies: -5MPa≤PD≤5MPa.
[0015] In some embodiments, the mold includes a cover and a cylinder, the cover sealing the cylinder, and the silicon powder being filled into the cylinder.
[0016] In some embodiments, a protective sleeve is provided on the outer periphery of the cover, the protective sleeve covering at least a portion of the cover.
[0017] In some embodiments, the edge of the cover includes a step that surrounds the cover.
[0018] In some embodiments, the mold is made of polyurethane material, and the density ρ0 of the polyurethane material satisfies: 1.00 g / cm³. 3 ≤ρ0≤1.01g / cm 3 .
[0019] In some embodiments, the wear rate G of the mold satisfies: G < G0, where G0 is the material loss in g / cm³. 2 ;
[0020] The condition G0 satisfies: 0 < G0 ≤ 0.1.
[0021] In some embodiments, the mold containing silicon powder is placed under a second pressure P2 for a duration of T2, satisfying 50MPa≤P2≤200MPa and 3min≤T2≤7min;
[0022] The mold containing silicon powder is placed under the third pressure P3 and maintained under the third pressure for a time T3, satisfying 200MPa≤P3≤600MPa and 4min≤T3≤8min.
[0023] In some embodiments, the mold containing silicon powder is placed under a fourth pressure P4 for a duration of T4, satisfying 100MPa≤P4≤600MPa and 3min≤T4≤6min.
[0024] In some embodiments, after the pressurization process is completed, a first depressurization process is applied to the mold, the first depressurization process including: reducing the pressure to a fifth pressure P5, and maintaining this pressure for T. n Time, satisfying: 10 ≤ P5 ≤ 100 MPa, 1 min ≤ T n ≤2min.
[0025] Accordingly, this application also provides a silicon block prepared by the above-described preparation method.
[0026] In some embodiments, the silicon block is broken into first particles, and the first particles account for ≥97% of the mass of the silicon block, based on the mass of the silicon block, and the particle size D1 of the first particles satisfies: 10mm≤D1.
[0027] In some embodiments, the silicon block is broken into second particles, wherein the second particles account for ≤3% of the mass of the silicon block, and the particle size D2 of the second particles satisfies: D2 < 10 mm.
[0028] Accordingly, embodiments of this application provide the application of the silicon block obtained by the above-described silicon powder forming method in the production of Czochralski single crystals; or, the application of the above-described silicon block in the production of Czochralski single crystals.
[0029] Beneficial Effects: Compared with existing technologies, this application provides a silicon powder forming method, a silicon block, and its application. The silicon powder forming method of this application includes the following steps: placing a mold containing silicon powder under a first pressure P1, maintaining the first pressure for a first time T1, satisfying 50MPa≤P1≤600MPa, 7min≤T1≤15min, to obtain a silicon block. This application, through pressure control, makes the formed silicon block easy to remove from the mold without breakage and dust generation. The obtained silicon block is easy to break during filling, the particle size distribution after breakage is easy to control, and the dust generation during the breakage process is low. The silicon block obtained by this application can be directly used in Czochralski single crystal production, increasing the charge density to 0.18g / cm³. 3 ~0.25g / cm 3 . Attached Figure Description
[0030] To more clearly illustrate the technical solutions in the embodiments of this application, the accompanying drawings used in the description of the embodiments will be briefly introduced below. Obviously, the accompanying drawings described below are only some embodiments of this application. For those skilled in the art, other drawings can be obtained based on these drawings without creative effort.
[0031] Figure 1 This is a three-dimensional exploded view of the mold used in this application;
[0032] Figure 2 This is an exploded structural diagram of the mold used in this application;
[0033] Figure 3 This is the front view of the mold used in this application;
[0034] Figure 4 for Figure 3 A cross-sectional view of the BB plane.
[0035] In the diagram, 1-mold, 100-cylinder, 110-first side, 120-second side, 130-third side, 200-cover, 201-step, 300-protective sleeve. Detailed Implementation
[0036] The technical solutions in the embodiments of this application will be clearly and completely described below with reference to the accompanying drawings. Obviously, the described embodiments are only a part of the embodiments of this application, and not all of the embodiments. Based on the embodiments in this application, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of this application. In addition, in the description of this application, the term "comprising" means "including but not limited to". The terms first, second, third, etc. are used only as illustrative purposes and do not impose numerical requirements or establish an order. Various embodiments of this application may exist in the form of a range; it should be understood that the description in the form of a range is only for convenience and conciseness and should not be construed as a hard limitation on the scope of this application; therefore, it should be considered that the range description has specifically disclosed all possible sub-ranges and single values within that range. For example, it should be considered that the range description from 1 to 6 has specifically disclosed sub-ranges, such as from 1 to 3, from 1 to 4, from 1 to 5, from 2 to 4, from 2 to 6, from 3 to 6, etc., and single numbers within the range, such as 1, 2, 3, 4, 5 and 6, which applies regardless of the range. Additionally, whenever a range of numbers is specified in this document, it means including any referenced numbers (fractions or integers) within the range referred to.
[0037] In the process of crystal rod preparation, silicon powder cannot be directly fed in and needs to be transformed into silicon rods or silicon blocks. To improve the filling rate, this application provides a silicon powder forming method, including the following steps: placing a mold 1 containing silicon powder under a first pressure P1 and maintaining the first pressure for a first time T1, satisfying 50MPa≤P1≤600MPa and 7min≤T1≤15min, to obtain a silicon block. The first pressure P1 (MPa) can be any value or a range of any two values from 50, 100, 150, 200, 250, 300, 350, 400, 450, 500, 550, and 600. The first pressure time T1 (min) can be any value or a range of any two values from 7, 8, 9, 10, 11, 12, 13, 14, and 15. If the pressure is too low, it will affect the compaction density and waste time. Excessive pressure, while not affecting the compaction density of the product, can shorten the lifespan of the equipment and make it more difficult to break the silicon block after molding.
[0038] In some embodiments, the first pressure P1 condition is achieved by increasing the pressure. The pressure increase step includes increasing the pressure to the first pressure P1 at a first pressure increase rate v1, satisfying 20 MPa / s ≤ v1 ≤ 30 MPa / s. The first pressure increase rate v1 (MPa / s) can be any value among 20, 25, and 30, or a range of any two values.
[0039] In some embodiments, the mold 1 containing silicon powder is placed before the first pressure condition P1, and the mold 1 containing silicon powder is placed in a closed environment.
[0040] This application places a mold 1 containing silicon powder in a sealed environment. In some embodiments, the mold 1 is sealed by a cover around its periphery, and then pressurized. This application overcomes the problem of low production efficiency caused by the need for manual bagging and unbagging operations each time wet pressing is performed. Furthermore, wet pressing uses liquid to pressurize the preform; if the mold 1 breaks during the pressing process, the liquid can easily seep into the pressed product, causing contamination and affecting quality. This application reduces the risk of silicon powder contamination by further providing a sealed space around the periphery of the mold 1.
[0041] In some embodiments, the first pressure P1 condition is applied by a pressurizing medium, which is a fluid. The mold 1 containing silicon powder is placed before the first pressure P1 condition and is placed in the cavity.
[0042] The mold 1 and the pressurizing medium are separated by a cavity; or, the pressurizing medium is filled in the cavity and the mold 1 is in contact with the pressurizing medium.
[0043] In some embodiments, when the mold 1 and the pressurizing medium are separated by a cavity, the pressurizing medium is a liquid; when the pressurizing medium fills the cavity and the mold 1 is in contact with the pressurizing medium, the pressurizing medium is a gas.
[0044] In some embodiments, the mold 1 and the pressurizing medium are separated by a cavity, and the interior of the cavity maintains a dry environment. The temperature range of the dry environment is 20–25°C, and the humidity range is 40–50% RH. For example, the temperature of the dry environment can be any value or a range of any two of the following: 20°C, 21°C, 22°C, 23°C, 24°C, and 25°C. Similarly, the humidity (% RH) can be any value or a range of any two of the following: 40, 41, 42, 43, 44, 45, 46, 47, 48, 49, and 50.
[0045] In some embodiments, the particle size range of the silicon powder is 0.1 μm to 1000 μm. The particle size (μm) of the silicon powder can be any value or a range of any two values from 0.1, 10, 50, 100, 150, 200, 250, 300, 350, 400, 450, 500, 550, 600, 650, 700, 750, 800, 850, 900, 950, and 1000.
[0046] In some embodiments, the mold 1 includes a first surface 110 and a second surface 120 disposed opposite to each other, the first surface 110 and the second surface 120 being connected by a third surface 130, and the first surface 110 and the third surface 130 receiving a first pressure P1.
[0047] In some embodiments, the pressure deviation PD MPa of the first pressure P1 satisfies: -5≤PD≤5, such that the value of PD (MPa) is any value among -5, -3, -2, 0, 1, 3, 5 or any range of two values.
[0048] In some embodiments, the mold 1 containing silicon powder is placed under a second pressure P2 for a duration T2, satisfying 50MPa≤P2≤200MPa and 3min≤T2≤7min. The second pressure P2 (MPa) can be any value from 50, 100, 150, and 200, or a range of any two values. The second pressure time T2 (min) can be any value from 3, 4, 5, 6, and 7, or a range of any two values.
[0049] In some embodiments, the mold 1 containing silicon powder is placed under a third pressure P3 for a duration T3, satisfying 200MPa≤P3≤600MPa and 4min≤T3≤8min. The third pressure P3 (MPa) can be any value or a range of any two values from 200, 250, 300, 350, 400, 450, 500, 550, and 600. The third pressure duration T3 (min) can be any value or a range of any two values from 4, 5, 6, 7, and 8.
[0050] In some embodiments, the mold 1 containing silicon powder is placed under a fourth pressure P4 for a duration T4, satisfying 100MPa≤P4≤600MPa and 3min≤T4≤6min. The fourth pressure P4 (MPa) can be any value or a range of any two values from 100, 150, 200, 250, 300, 350, 400, 450, 500, 550, and 600. The fourth pressure time T4 (min) can be any value or a range of any two values from 3, 4, 5, and 6.
[0051] In some embodiments, after the pressurization process is completed, a first depressurization process is applied to the mold 1. The first depressurization process includes: reducing the pressure to a fifth pressure P5 and maintaining it for T. n Time, satisfying: 10MPa≤P5≤100MPa, 1min≤T n ≤2min. For example, the fifth pressure P5 (MPa) can take any value or a range of any two values from 10, 20, 30, 40, 50, 60, 70, 80, 90, 100. For example, T... n The value of (min) can be any value from 1, 1.5, and 2, or a range of any two values. This application maintains a fifth pressure P5 after pressurization, which can further reduce the amount of dust generated when the shaped silicon block is broken.
[0052] In some embodiments, the pressure relief rate v2 satisfies 20 MPa / s ≤ v2 ≤ 30 MPa / s. For example, the pressure relief rate v2 can take any value from 20, 25, and 30, or a range of any two values.
[0053] In some embodiments, this application controls the pressure range of the pressurization process by selecting a first pressurization rate or a depressurization rate.
[0054] In some embodiments, the pressurization time of this application does not include the time for the pressurization or depressurization process.
[0055] like Figures 1 to 4 As shown, in some embodiments, mold 1 is made of polyurethane material, and the density ρ0 of the polyurethane material satisfies: 1.00 g / cm³.3 ≤ρ0≤1.01g / cm 3 .
[0056] In some embodiments, the mold 1 includes a cover 200 and a cylinder 100, the cover 200 covering the cylinder 100, and silicon powder being filled inside the cylinder 100.
[0057] In some embodiments, the inner diameter of the cylinder 100 is 137 mm to 141 mm.
[0058] In some embodiments, the outer diameter of the cylinder 100 is 154 mm to 160 mm.
[0059] In some embodiments, the height of the cylinder 100 is 691 mm to 697 mm.
[0060] In some embodiments, a protective sleeve 300 is provided on the outer periphery of the cover 200, and the protective sleeve 300 covers at least a portion of the cover 200.
[0061] In some embodiments, the protective sleeve 300 is disposed over the outer periphery of the cover 200 to compact the cover 200.
[0062] In some embodiments, the pressurization method used in this application is isostatic pressing. During operation, the cover 200 of the mold 1 is opened, the material is loaded, and then the cover 200 is closed and pressurized to form the material. When discharging, the cover 200 of the mold 1 is opened, and the silicon block formed in the mold 1 is pushed out by applying pressure to the bottom of the cylinder 100. The operation cycle is short and suitable for batch production.
[0063] In some embodiments, the edge of the cover 200 includes a step 201, which surrounds the cover 200 and further increases the sealing of the cover 200 to prevent silicon powder from leaking out.
[0064] In some embodiments, the wear rate G of mold 1 satisfies: G < G0, where G0 is the material loss in g / cm³. 2 G0 satisfies: 0 < G0 ≤ 0.1.
[0065] In some embodiments, G0 represents the material loss measured by an abrasion testing machine under specified conditions, and the unit of material loss is g / cm³. 2 .
[0066] This application further provides a silicon block prepared by the above method.
[0067] In some embodiments, the silicon block is broken to form a first particle, wherein the first particle accounts for ≥97% of the mass of the silicon block, and the particle size D1 of the first particle satisfies: 10mm≤D1.
[0068] In some embodiments, the particle size D1 of the first particle satisfies: 10mm ≤ D1 ≤ 150mm, such that the particle size of the first particle takes any value or a range of any two values from 10, 20, 30, 40, 50, 60, 70, 80, 90, 100, 110, 120, 130, 140, 150. In other embodiments, the particle size D1 of the first particle satisfies: 10mm ≤ D1 ≤ 70mm.
[0069] In some embodiments, the silicon block is crushed to form second particles. The second particles, based on the mass of the silicon block, account for ≤3% of the silicon block's mass, and the particle size D2 of the second particles satisfies: D2 < 10 mm. For example, if the particle size of the second particles is 3 mm ≤ D2 < 10 mm, the proportion is 2-3%; if the particle size of the second particles is 0 mm ≤ D2 < 3 mm, the proportion is ≤1%. The silicon block formed in this application has a reasonable particle size distribution after crushing, resulting in a reasonable particle distribution during the feeding process in Czochralski single crystal production, facilitating the feeding operation.
[0070] The crushing method in this application can be manual crushing or mechanical vibration crushing. In some embodiments, manual crushing is used.
[0071] This application employs dry pressure technology to avoid contaminating raw materials, and enables large-scale and rapid production, thereby improving production efficiency and enabling the application of the prepared silicon blocks in Czochralski single crystal production.
[0072] Example 1: Native polycrystalline silicon powder is loaded into mold 1, as follows: Figures 1-4 As shown, the mold 1 of this application is made of polyurethane material. After loading, a scraper is used to level or flatten the silicon powder at the loading port. The cover 200 and protective sleeve 300 are then sealed. After sealing, a diaphragm is wound around the outer layer to form an isolation cavity, separating the mold 1 from the pressurized environment. The mold containing virgin polycrystalline silicon powder is placed into the equipment, and liquid is injected to the set height. The equipment starts running, and the pressure is set as follows: pressurization rate is increased from 20 MPa / s to 100 MPa, and the pressurization time is 15 minutes. After pressurization, the pressure is released at 30 MPa / s, and after returning to normal pressure, the furnace is opened and the liquid is extracted, and the mold 1 is removed. During the pressurization process, the liquid evenly transmits pressure to all surfaces of the mold 1, and the pressure deviation between any two surfaces of the mold 1 is within ±5 MPa. The surface of the mold 1 is rinsed with pure water, and after rinsing, the residual pure water on the surface of the mold 1 is wiped clean before unpacking and demolding; then it is sealed and packaged.
[0073] Examples 2-4: The pressurization method is the same as in Example 1, except that the pressure value and pressurization time are adjusted. For specific parameters, please refer to Table 1.
[0074] Comparative Example 1: The pressurization method is the same as in Example 1, except that the pressure value and pressurization time are adjusted. For specific parameters, please refer to Table 1.
[0075] Comparative Example 2: Silicon powder was not pressurized.
[0076] Calculation method:
[0077] The charge ratio is (B+C) / A*100%, where A is the theoretical charge amount of the crucible in kg, B is the mass of the crushed silicon powder block in kg, and C is the mass of other materials such as dopant elements in kg.
[0078] Table 1. Preparation parameters and results of Examples 1-4 and Comparative Examples 1-2
[0079]
[0080]
[0081] Data from Examples 1-4 and Comparative Examples 1-2 show that the method of this application increases the charge ratio from 6% in the silicon powder state to 100%. Data from Example 4 shows that when the pressure is too low, although the charge ratio is increased, it affects the compaction density of the silicon block and wastes time. Data from Comparative Example 1 shows that increasing the pressure does not affect the compaction density of the product, but excessive pressure will affect the equipment lifespan and make it difficult to break the silicon block after molding.
[0082] Example 5: The preparation method is the same as in Example 1, except that the pressurization pressure and pressurization time are adjusted. The pressure is increased to 50 MPa at a pressurization rate of 20 MPa / s and the pressurization time is 3 min. After pressurization, the pressure is increased to 300 MPa at a pressurization rate of 20 MPa / s and the pressurization time is 6 min. For specific parameters, please refer to Table 2.
[0083] Examples 6-15: The preparation method is the same as that of Example 5, except that the pressurization pressure and pressurization time are adjusted. For specific parameters, please refer to Table 2.
[0084] Table 2 Preparation parameters and results of Examples 5-15
[0085]
[0086] As can be seen from the results in Table 2, this application improves the compaction density by controlling the pressure range and pressure time. The resulting molded silicon powder exhibits lower dust generation during the crushing process compared to the molded silicon blocks of Examples 1-4.
[0087] Example 16: The preparation method is the same as in Example 1, except that the pressurization pressure and pressurization time are adjusted. The pressure is increased to 50 MPa at a pressurization rate of 20 MPa / s for 3 min. After pressurization, the pressure is increased to 300 MPa at a pressurization rate of 20 MPa / s for 6 min. Then the pressure is maintained at 300 MPa and pressurization continues for 4 min. For specific parameters, please refer to Table 3.
[0088] Examples 17-31: The preparation method is the same as that in Example 16, except that the pressurization pressure and pressurization time are adjusted. For specific parameters, please refer to Table 3.
[0089] Table 3. Preparation parameters and results of Examples 16 to 31
[0090]
[0091] As can be seen from the results in Table 3, by controlling the pressure range and pressure time, this application improves the compaction density of silicon powder, and the resulting molded silicon block has a lower dust emission during the crushing process than the molded silicon blocks of Examples 5-15.
[0092] Example 32: The preparation method is the same as in Example 1, except that the pressurization pressure and pressurization time are adjusted. The pressure is increased to 50 MPa at a pressurization rate of 20 MPa / s for 3 min. After pressurization, the pressure is increased to 300 MPa at a pressurization rate of 20 MPa / s for 6 min. Then the pressure is maintained at 300 MPa and pressurization continues for 6 min. Then the pressure is reduced to 50 MPa at a depressurization rate of 20 MPa / s for 1.5 min. For specific parameters, please refer to Table 4.
[0093] Examples 33-50: The preparation method is the same as that of Example 32, except that the pressurization pressure and pressurization time are adjusted. For specific parameters, please refer to Table 4.
[0094] Table 4. Preparation parameters and results of Examples 32 to 50
[0095]
[0096]
[0097] As can be seen from the results in Table 4, applying pressure during the silicon powder forming process in this application can increase the compaction density of the silicon powder. From the results of silicon block crushing after forming, the pressure relief step has a relatively small impact on the compaction density, but the dust content is significantly reduced during crushing compared to silicon powder formed without a pressure relief step.
[0098] This application improves compaction density by controlling the pressure range and pressure time. Furthermore, the shaped silicon block prepared according to the embodiments of this application has a particle size distribution range after crushing that can be directly used for feeding, and there is no dust pollution during the crushing process.
[0099] In the above embodiments, the descriptions of each embodiment have different focuses. For parts not described in detail in a certain embodiment, please refer to the relevant descriptions in other embodiments.
[0100] The above provides a detailed description of a silicon powder forming method, silicon block, and application provided by the embodiments of this application. Specific examples have been used to illustrate the principles and implementation methods of this application. The description of the above embodiments is only for the purpose of helping to understand the method and core ideas of this application. At the same time, for those skilled in the art, there will be changes in the specific implementation methods and application scope based on the ideas of this application. Therefore, the content of this specification should not be construed as a limitation of this application.
Claims
1. A method for forming silicon powder, characterized in that, Includes the following steps: The mold (1) containing silicon powder is placed under the first pressure P1 and the first pressure is maintained for a time T1, satisfying 50 MPa≤P1≤600 MPa and 7min≤T1≤15min; The first pressure condition P1 is achieved by increasing the pressure. The pressure increasing step includes increasing the pressure to the first pressure P1 at a first pressure increasing rate v1, satisfying 20 MPa / s ≤ v1 ≤ 30 MPa / s. The mold (1) containing silicon powder is placed under the second pressure P2 and the second pressure is maintained for a time T2, satisfying 50 MPa≤P2≤200 MPa and 3min≤T2≤7min; The mold (1) containing silicon powder is placed under the third pressure P3 and the third pressure is maintained for a time T3, satisfying 200 MPa≤P3≤600 MPa, 4min≤T3≤8min; The mold (1) containing silicon powder is placed under the fourth pressure P4 and the fourth pressure is maintained for a time T4, satisfying 100 MPa≤P4≤600 MPa and 3min≤T4≤6min; After the pressurization process is completed, a first depressurization process is applied to the mold (1), the first depressurization process including: reducing the pressure to a fifth pressure P5 and maintaining it for T. n Time, satisfying: 10 ≤ P5 ≤ 100 MPa, 1 min ≤ T n ≤2min, silicon block is obtained.
2. The silicon powder forming method according to claim 1, characterized in that, Before the first pressure P1 condition, the mold (1) containing silicon powder is placed in a closed environment.
3. The silicon powder forming method according to claim 1, characterized in that, The first pressure P1 is applied by a pressurizing medium, which is a fluid. The mold (1) containing silicon powder is placed before the first pressure P1 condition and is placed in a cavity. The mold (1) and the pressurizing medium are separated by the cavity; or, the pressurizing medium is filled in the cavity and the mold (1) is in contact with the pressurizing medium.
4. The silicon powder forming method according to claim 3, characterized in that, When the mold (1) and the pressurizing medium are separated by the cavity, the pressurizing medium is a liquid; when the pressurizing medium fills the cavity and the mold (1) is in contact with the pressurizing medium, the pressurizing medium is a gas; and / or, When the mold (1) and the pressurizing medium are separated by the cavity, the inside of the cavity is kept in a dry environment with a temperature range of 20~25℃ and a humidity range of 40~50%rh.
5. The silicon powder forming method according to claim 1, characterized in that, The particle size of the silicon powder is from 0.1 μm to 1000 μm.
6. The silicon powder forming method according to claim 1, characterized in that, The mold (1) includes a first surface (110) and a second surface (120) disposed opposite to each other, the first surface (110) and the second surface (120) being connected by a third surface (130), the first surface (110) and the third surface (130) receiving the first pressure P1; and / or, The first surface (110), the second surface (120) and the third surface (130) receive the first pressure P1, and the pressure deviation PDMPa of the first pressure P1 applied to the first surface (110), the second surface (120) and the third surface (130) satisfies: -5≤PD≤5.
7. The silicon powder forming method according to claim 1, characterized in that, The mold (1) includes a cover (200) and a cylinder (100), the cover (200) covering the cylinder (100), and the silicon powder being filled inside the cylinder (100).
8. The silicon powder forming method according to claim 7, characterized in that, The cover (200) is provided with a protective sleeve (300) on its outer periphery, the protective sleeve (300) covering at least a portion of the cover (200).
9. The silicon powder forming method according to claim 7, characterized in that, The edge of the cover (200) includes a step (201) that surrounds the cover (200).
10. The silicon powder forming method according to claim 1, characterized in that, The mold (1) is made of polyurethane material, and the density ρ0 of the polyurethane material satisfies: 1.00 g / cm³. 3 ≤ρ0≤1.01g / cm 3 .
11. The silicon powder forming method according to claim 1, characterized in that, The wear rate G of the mold (1) satisfies: G < G0, where G0 is the material loss in g / cm³. 2 ; The condition G0 satisfies: 0 < G0 ≤ 0.1.
Citation Information
Patent Citations
Application of raw material silicon briquette with good packing performance in single crystal furnace or polycrystalline furnace
CN101613877A
Single crystal furnace and preparation method of single crystal silicon rod
CN110923806A
