An oily high-solid-content carbon nanotube conductive paste and a preparation method thereof

By preparing an oily, high-solids-content carbon nanotube conductive slurry and using a combination of dispersants and surfactants, the problem of carbon nanotube agglomeration was solved, achieving high energy density and good conductivity in lithium-ion batteries.

CN117079891BActive Publication Date: 2026-11-10SHENZHEN JINBAINA NANO TECH CO LTD
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202311173164.X
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-09-12
Publication Date
2026-11-10
Estimated Expiration
2043-09-12

AI Technical Summary

Technical Problem

Carbon nanotubes are prone to agglomeration during large-scale production, making it difficult for them to effectively exert their excellent performance in lithium-ion batteries. Furthermore, the excessive amount of traditional carbon-based conductive materials added cannot meet the requirements of high-energy-density batteries.

Method used

An oily, high-solids-content carbon nanotube conductive slurry was prepared by using a combination of dispersants and surfactants, followed by ultrasonic dispersion and grinding to form a small-sized conductive network, thereby improving the dispersion performance and connection efficiency of carbon nanotubes in the positive electrode active material.

Benefits of technology

It improves the energy density and capacity of lithium-ion batteries, reduces the increase in resistance during charging and discharging, and enhances the battery's lifespan and conductivity.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004444571070000071
    Figure BDA0004444571070000071
  • Figure BDA0004444571070000091
    Figure BDA0004444571070000091
Patent Text Reader

Abstract

This invention discloses an oily high-solids-content carbon nanotube conductive slurry and its preparation method, belonging to the field of conductive slurry technology. The key technical point is a preparation method of an oily high-solids-content carbon nanotube conductive slurry, including the following steps: (1) adding a dispersant to a solvent and stirring and dispersing for 30-50 min; (2) adding a conductive agent and a surfactant to the mixture obtained in step (1) and performing ultrasonic dispersion treatment for 50-70 min; (3) grinding the dispersion obtained in step (2) using a sand mill at a ball-to-material mass ratio of 10:1 and a rotation speed of 1200-1500 rpm for 1-3 h, then sieving and performing a second ultrasonic dispersion treatment for 40-60 min to obtain a conductive slurry; wherein the conductive slurry, by mass percentage, is: 10-12% conductive agent, 1.0-2.5% dispersant, 1.0-2.0% surfactant, and the remainder is solvent; the conductive agent includes carbon nanotubes, thereby improving the dispersion performance of carbon nanotubes.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of conductive paste technology, and in particular to an oily, high-solids-content carbon nanotube conductive paste and its preparation method. Background Technology

[0002] Lithium-ion batteries are considered one of the most promising energy storage technologies due to their high energy density, energy conversion efficiency, and output voltage. However, the positive and negative electrode materials of lithium-ion batteries (such as lithium iron phosphate and silicon suboxide) generally suffer from poor conductivity. During charging and discharging, electrode polarization can easily occur, leading to incomplete charging and discharging reactions and preventing the effective energy of the electrode materials from being fully utilized. To improve the conductivity of the electrodes, carbon-based conductive agents need to be added. However, traditional carbon-based conductive materials, such as carbon black and graphite, are difficult to meet the high energy density requirements of current electric vehicle batteries due to their high addition amounts. Carbon nanotube conductive agents, on the other hand, have excellent conductivity, and adding a small amount can ensure the battery's energy density while also improving its electrochemical performance.

[0003] However, carbon nanotubes currently exhibit severe aggregation during large-scale production. If directly applied to batteries, their excellent performance cannot be effectively utilized at the microscale, which also reduces battery performance. Summary of the Invention

[0004] To improve the dispersion performance of carbon nanotubes, this invention provides an oily, high-solids-content carbon nanotube conductive slurry and its preparation method.

[0005] The first aspect of the present invention provides a method for preparing an oily, high-solids-content carbon nanotube conductive paste, using the following technical solution: A method for preparing an oily, high-solids-content carbon nanotube conductive paste includes the following steps: (1) Add the dispersant to the solvent and stir to disperse for 30-50 minutes; (2) Add conductive agent and surfactant to the mixture obtained in step (1) and perform ultrasonic dispersion treatment for 50-70 min; (3) The dispersion obtained in step (2) is ground in a sand mill at a ball-to-material mass ratio of 10:1 and a rotation speed of 1200-1500 rpm for 1-3 hours, then sieved and subjected to a second ultrasonic dispersion treatment for 40-60 minutes to obtain a conductive slurry. The conductive paste, by mass percentage, comprises: 10-12% conductive agent, 1.0-2.5% dispersant, 1.0-2.0% surfactant, with the balance being solvent; the conductive agent includes carbon nanotubes.

[0006] By adopting the above technical solution, after adding the conductive agent and surfactant to the solvent containing the dispersant, the dispersion performance of the conductive agent in the solvent can be improved under the action of ultrasound. After further treatment by grinding and ultrasonic dispersion, not only can the conductive agents overcome van der Waals forces to achieve separation, but the conductive agents can also be broken into smaller sizes. The small-sized structure formed is conducive to the formation of a highly efficient conductive network in the positive electrode active material, thereby improving the energy density of the battery. At the same time, the small-sized structure formed by the breakage can not only effectively connect more active materials to increase the battery capacity, but also reduce the increase in resistance caused by the volume shrinkage and expansion of positive electrode particles during the charging and discharging process.

[0007] When the proportions of conductive agent, dispersant, and surfactant in the conductive paste are within this range, not only can the conductive paste maintain a high solids content, but the conductive agent is also less likely to settle in the positive electrode active material, reducing solvent usage and thus shortening the subsequent coating and drying time of the conductive paste, thereby improving battery manufacturing efficiency. Furthermore, the combined use of dispersant and surfactant contributes to the uniformity of the conductive paste, effectively extending battery life.

[0008] Preferably, the conductive paste contains, by mass percentage, 10-12% conductive agent, 1.5-2.0% dispersant, 1.5-2.0% surfactant, and the balance being solvent.

[0009] By adopting the above technical solution, experiments have shown that when the contents of conductive agent, dispersant and surfactant are within this range, the dispersion performance of the conductive agent is further improved, resulting in good stability and low volume resistivity of the conductive slurry.

[0010] Preferably, the conductive agent further includes graphene, and the weight ratio of graphene to carbon nanotubes is 1:(2-4).

[0011] Preferably, the carbon nanotubes have an average diameter of 20-50 nm and a specific surface area of ​​70-110 m². 2 / g.

[0012] By adopting the above technical solution, when the average diameter of carbon nanotubes is within this range, the conductivity of the electrode material can be improved, thereby enhancing the overall conductivity of the electrode and improving the rate performance of the battery. When the diameter of carbon nanotubes is too small, the specific surface area of ​​carbon nanotubes will be relatively large, which will consume electrolyte. At the same time, due to Brownian motion, the particles will collide violently, causing flocculation of the slurry and making it easier for the conductive slurry to separate.

[0013] Preferably, the dispersant comprises sodium salt of 2-naphthalenesulfonic acid formaldehyde polymer and polyvinylpyrrolidone in a weight ratio of 1:(0.4-0.8).

[0014] Preferably, the surfactant includes one or two of fatty alcohol polyoxyethylene ether phosphate and sodium dodecyl sulfate.

[0015] Preferably, the weight ratio of the fatty alcohol polyoxyethylene ether phosphate to sodium dodecyl sulfate is 1:(0.8-1.2).

[0016] Preferably, the viscosity of the conductive paste is between 1000 and 3000 mPa·s.

[0017] A second aspect of the present invention is to provide a conductive paste obtained by the preparation method of the above-described oily high-solids-content carbon nanotube conductive paste.

[0018] In summary, the present invention has the following beneficial effects: The combined use of dispersants and surfactants in this application enables the conductive agent to have good dispersion performance in the solvent, thereby obtaining a conductive slurry with high solid content. Moreover, the solid content of the conductive slurry changes little and the rate of change is small after storage at room temperature, indicating that the conductive slurry obtained in this application has good storage stability and effectively reduces the sedimentation of the conductive agent. In addition, when the conductive slurry obtained in this application is applied to lithium-ion batteries, it has good conductivity. Detailed Implementation

[0019] The present invention will be further described in detail below with reference to the embodiments.

[0020] All raw materials used in this application are commercially available.

[0021] Example 1 A method for preparing an oily, high-solids-content carbon nanotube conductive paste includes the following steps: (1) Add 1 kg of dispersant to 88 kg of N-methylpyrrolidone and stir to disperse for 30 min; (2) Add 10 kg of carbon nanotubes and 1 kg of fatty alcohol polyoxyethylene ether phosphate to the mixture obtained in step (1) and perform ultrasonic dispersion treatment for 50 min; (3) The dispersion obtained in step (2) is ground in a sand mill for 3 hours at a ball-to-material mass ratio of 10:1 and a rotation speed of 1200 rpm, then sieved and subjected to a second ultrasonic dispersion treatment for 40 minutes to obtain a conductive slurry. The dispersant includes sodium salt of 2-naphthalenesulfonic acid formaldehyde polymer and polyvinylpyrrolidone in a weight ratio of 1:0.4, specifically, the content of sodium salt of 2-naphthalenesulfonic acid formaldehyde polymer is 0.71 kg and the content of polyvinylpyrrolidone is 0.29 kg.

[0022] Example 2 A method for preparing an oily, high-solids-content carbon nanotube conductive paste includes the following steps: (1) Add 2.5 kg of dispersant to 83.5 kg of N-methylpyrrolidone and stir to disperse for 30 min; (2) Add 12 kg of carbon nanotubes and 2 kg of fatty alcohol polyoxyethylene ether phosphate to the mixture obtained in step (1) and perform ultrasonic dispersion treatment for 50 min; (3) The dispersion obtained in step (2) is ground in a sand mill for 3 hours at a ball-to-material mass ratio of 10:1 and a rotation speed of 1200 rpm, then sieved and subjected to a second ultrasonic dispersion treatment for 40 minutes to obtain a conductive slurry. The dispersant includes sodium salt of 2-naphthalenesulfonic acid formaldehyde polymer and polyvinylpyrrolidone in a weight ratio of 1:0.4, specifically, the content of sodium salt of 2-naphthalenesulfonic acid formaldehyde polymer is 1.79 kg and the content of polyvinylpyrrolidone is 0.71 kg.

[0023] Example 3 A method for preparing an oily, high-solids-content carbon nanotube conductive paste includes the following steps: (1) Add 1.5 kg of dispersant to 87 kg of N-methylpyrrolidone and stir to disperse for 30 min; (2) Add 10 kg of carbon nanotubes and 1.5 kg of fatty alcohol polyoxyethylene ether phosphate to the mixture obtained in step (1) and perform ultrasonic dispersion treatment for 50 min; (3) The dispersion obtained in step (2) is ground in a sand mill for 3 hours at a ball-to-material mass ratio of 10:1 and a rotation speed of 1200 rpm, then sieved and subjected to a second ultrasonic dispersion treatment for 40 minutes to obtain a conductive slurry. The dispersant includes sodium salt of 2-naphthalenesulfonic acid formaldehyde polymer and polyvinylpyrrolidone in a weight ratio of 1:0.4, specifically, the content of sodium salt of 2-naphthalenesulfonic acid formaldehyde polymer is 1.07 kg and the content of polyvinylpyrrolidone is 0.43 kg.

[0024] Example 4 A method for preparing an oily, high-solids-content carbon nanotube conductive paste includes the following steps: (1) Add 2 kg of dispersant to 86 kg of N-methylpyrrolidone and stir to disperse for 30 min; (2) Add 10 kg of carbon nanotubes and 2 kg of fatty alcohol polyoxyethylene ether phosphate to the mixture obtained in step (1) and perform ultrasonic dispersion treatment for 50 min; (3) The dispersion obtained in step (2) is ground in a sand mill for 3 hours at a ball-to-material mass ratio of 10:1 and a rotation speed of 1200 rpm, then sieved and subjected to a second ultrasonic dispersion treatment for 40 minutes to obtain a conductive slurry. The dispersant includes sodium salt of 2-naphthalenesulfonic acid formaldehyde polymer and polyvinylpyrrolidone in a weight ratio of 1:0.4, specifically, the content of sodium salt of 2-naphthalenesulfonic acid formaldehyde polymer is 1.43 kg and the content of polyvinylpyrrolidone is 0.57 kg.

[0025] Example 5 A method for preparing an oily, high-solids-content carbon nanotube conductive paste includes the following steps: (1) Add 1.5 kg of dispersant to 87 kg of N-methylpyrrolidone and stir to disperse for 30 min; (2) Add 10 kg of carbon nanotubes and 1.5 kg of fatty alcohol polyoxyethylene ether phosphate to the mixture obtained in step (1) and perform ultrasonic dispersion treatment for 70 min; (3) The dispersion obtained in step (2) is ground in a sand mill at a ball-to-material mass ratio of 10:1 and a rotation speed of 1500 rpm for 1 hour, then sieved and subjected to a second ultrasonic dispersion treatment for 60 minutes to obtain a conductive slurry. The dispersant includes sodium salt of 2-naphthalenesulfonic acid formaldehyde polymer and polyvinylpyrrolidone in a weight ratio of 1:0.4, specifically, the content of sodium salt of 2-naphthalenesulfonic acid formaldehyde polymer is 1.07 kg and the content of polyvinylpyrrolidone is 0.43 kg.

[0026] Example 6 A method for preparing an oily high-solids-content carbon nanotube conductive slurry differs from Example 3 in that the conductive agent is a mixture of graphene and carbon nanotubes, and the weight ratio of graphene to carbon nanotubes is 1:2. Specifically, the content of graphene is 3.33 kg and the content of carbon nanotubes is 6.67 kg, while the rest remain unchanged.

[0027] Example 7 A method for preparing an oily high-solids-content carbon nanotube conductive slurry differs from Example 3 in that the conductive agent is a mixture of graphene and carbon nanotubes, and the weight ratio of graphene to carbon nanotubes is 1:4. Specifically, the content of graphene is 2 kg and the content of carbon nanotubes is 8 kg, while the rest remain unchanged.

[0028] Example 8 A method for preparing an oily, high-solids-content carbon nanotube conductive slurry differs from Example 7 in that the dispersant comprises sodium salt of 2-naphthalenesulfonic acid formaldehyde polymer and polyvinylpyrrolidone in a weight ratio of 1:0.8, specifically, the content of sodium salt of 2-naphthalenesulfonic acid formaldehyde polymer is 0.83 kg and the content of polyvinylpyrrolidone is 0.67 kg.

[0029] Example 9 A method for preparing an oily, high-solids-content carbon nanotube conductive slurry differs from Example 7 in that the dispersant comprises sodium salt of 2-naphthalenesulfonic acid formaldehyde polymer and polyvinylpyrrolidone in a weight ratio of 1:1, specifically, the content of sodium salt of 2-naphthalenesulfonic acid formaldehyde polymer is 0.75 kg and the content of polyvinylpyrrolidone is 0.75 kg.

[0030] Example 10 A method for preparing an oily, high-solids-content carbon nanotube conductive slurry differs from Example 7 in that only polyvinylpyrrolidone is used as the dispersant.

[0031] Example 11 A method for preparing an oily, high-solids-content carbon nanotube conductive slurry differs from Example 7 in that the dispersant used is only sodium salt of 2-naphthalenesulfonic acid formaldehyde polymer.

[0032] Example 12 A method for preparing an oily high-solids-content carbon nanotube conductive paste differs from Example 7 in that, in step (2), an equal amount of sodium dodecyl sulfate is used instead of fatty alcohol polyoxyethylene ether phosphate.

[0033] Example 13 A method for preparing an oily high-solids-content carbon nanotube conductive paste differs from Example 7 in that the surfactant in step (2) is a mixture of fatty alcohol polyoxyethylene ether phosphate and sodium dodecyl sulfate, wherein the weight ratio of fatty alcohol polyoxyethylene ether phosphate to sodium dodecyl sulfate is 1:0.8, specifically, the content of fatty alcohol polyoxyethylene ether phosphate is 0.83 kg and the content of sodium dodecyl sulfate is 0.67 kg.

[0034] Example 14 A method for preparing an oily high-solids-content carbon nanotube conductive paste differs from Example 7 in that the surfactant in step (2) is a mixture of fatty alcohol polyoxyethylene ether phosphate and sodium dodecyl sulfate, wherein the weight ratio of fatty alcohol polyoxyethylene ether phosphate to sodium dodecyl sulfate is 1:1.2, specifically, the content of fatty alcohol polyoxyethylene ether phosphate is 0.68 kg and the content of sodium dodecyl sulfate is 0.82 kg.

[0035] Example 15 A method for preparing an oily high-solids-content carbon nanotube conductive paste differs from Example 13 in that the surfactant in step (2) is a mixture of fatty alcohol polyoxyethylene ether phosphate and sodium alkylbenzene sulfonate, wherein the weight ratio of fatty alcohol polyoxyethylene ether phosphate to sodium alkylbenzene sulfonate is 1:0.8, specifically, the content of fatty alcohol polyoxyethylene ether phosphate is 0.83 kg and the content of sodium alkylbenzene sulfonate is 0.67 kg.

[0036] Example 16 A method for preparing an oily, high-solids-content carbon nanotube conductive paste differs from Example 13 in that an equal amount of sodium fatty alcohol polyoxyethylene ether sulfate is used instead of fatty alcohol polyoxyethylene ether phosphate, while all other aspects remain unchanged.

[0037] Example 17 A method for preparing an oily, high-solids-content carbon nanotube conductive paste differs from Example 13 in that an equal amount of hexadecyltrimethylammonium bromide is used instead of sodium dodecyl sulfate, while all other aspects remain unchanged.

[0038] Comparative Example 1 A method for preparing an oily, high-solids-content carbon nanotube conductive paste, which differs from Example 3 in that it includes the following steps: (1) Add 2.5 kg of dispersant to 83.5 kg of N-methylpyrrolidone and stir to disperse for 30 min; (2) Add 12 kg of carbon nanotubes and 2 kg of fatty alcohol polyoxyethylene ether phosphate to the mixture obtained in step (1). Grind the mixture for 3 hours using a sand mill at a ball-to-material mass ratio of 10:1 and a rotation speed of 1200 rpm. Then sieve the mixture and perform ultrasonic dispersion treatment for 40 minutes to obtain a conductive slurry. The dispersant includes sodium salt of 2-naphthalenesulfonic acid formaldehyde polymer and polyvinylpyrrolidone in a weight ratio of 1:0.4, specifically, the content of sodium salt of 2-naphthalenesulfonic acid formaldehyde polymer is 1.79 kg and the content of polyvinylpyrrolidone is 0.71 kg.

[0039] Comparative Example 2 A method for preparing an oily, high-solids-content carbon nanotube conductive paste, which differs from Example 3 in that it includes the following steps: (1) Add 2.5 kg of dispersant to 83.5 kg of N-methylpyrrolidone and stir to disperse for 30 min; (2) Add 12 kg of carbon nanotubes and 2 kg of fatty alcohol polyoxyethylene ether phosphate to the mixture obtained in step (1) and perform ultrasonic dispersion treatment for 50 min; (3) The dispersion obtained in step (2) is ground in a sand mill for 3 hours at a ball-to-material mass ratio of 10:1 and a rotation speed of 1200 rpm, and then sieved to obtain a conductive slurry. The dispersant includes sodium salt of 2-naphthalenesulfonic acid formaldehyde polymer and polyvinylpyrrolidone in a weight ratio of 1:0.4, specifically, the content of sodium salt of 2-naphthalenesulfonic acid formaldehyde polymer is 1.79 kg and the content of polyvinylpyrrolidone is 0.71 kg.

[0040] Comparative Example 3 A method for preparing an oily high-solids-content carbon nanotube conductive paste differs from Example 3 in that step (2) does not contain fatty alcohol polyoxyethylene ether phosphate, and the content of dispersant in step (1) is 4.5 kg. The dispersant includes sodium salt of 2-naphthalenesulfonic acid formaldehyde polymer and polyvinylpyrrolidone in a weight ratio of 1:0.4. Specifically, the content of sodium salt of 2-naphthalenesulfonic acid formaldehyde polymer is 3.21 kg and the content of polyvinylpyrrolidone is 1.29 kg. The rest is the same as in Example 3.

[0041] Performance testing (1) The conductive pastes prepared in the above examples and comparative examples were subjected to conventional physical property tests for solid content, viscosity and metal content. The test results are shown in Table 1.

[0042] The metal content in conductive paste is the sum of impurity elements iron, copper, zinc, nickel, chromium, and cobalt.

[0043] The conductive pastes obtained in the above examples and comparative examples were sealed and placed at 55±1℃ for 7 days and then left to stand at room temperature (approximately 25±2℃) for 3 months. The change rate of solid content at the bottom 1 / 4 of the paste surface was then tested.

[0044] Table 1. Test Results of Physical Properties of Conductive Paste As can be seen from Table 1, the change rate of the solid content of the conductive slurry obtained in Examples 1-8 of this application after storage at room temperature and high temperature is within 0.8%, indicating that the conductive slurry obtained in Examples 1-8 has good dispersion performance, resulting in better stability of the conductive slurry during long-term storage.

[0045] Compared with Example 7, when the proportion of sodium 2-naphthalenesulfonic acid formaldehyde polymer and polyvinylpyrrolidone in the dispersant exceeds the limit of this application, the viscosity and storage stability of the conductive paste obtained in Example 9 are lower than those in Example 7. This indicates that exceeding the limit of this application in the proportion of sodium 2-naphthalenesulfonic acid formaldehyde polymer and polyvinylpyrrolidone in the dispersant will affect the stability of the conductive paste.

[0046] Compared with Example 7, when only polyvinylpyrrolidone or only sodium 2-naphthalenesulfonic acid formaldehyde polymer was used as the dispersant, the viscosity and storage stability of the conductive pastes obtained in Examples 10 and 11 were lower than those in Example 7. This further illustrates that the combined use of sodium 2-naphthalenesulfonic acid formaldehyde polymer and polyvinylpyrrolidone can effectively improve the dispersion performance of the conductive paste, thereby improving its stability.

[0047] Compared with Example 13, when sodium alkylbenzene sulfonate was used instead of sodium dodecyl sulfate or sodium fatty alcohol polyoxyethylene ether phosphate was used instead of fatty alcohol polyoxyethylene ether phosphate, the storage stability of the conductive pastes obtained in Examples 15 and 16 was reduced compared with Example 13. It can be seen that the combined use of sodium dodecyl sulfate and fatty alcohol polyoxyethylene ether phosphate can effectively ensure the dispersion performance of the conductive paste, thereby improving the storage stability of the conductive paste.

[0048] Compared with Example 13, when hexadecyltrimethylammonium bromide was used instead of sodium dodecyl sulfate, the storage stability of the conductive slurry obtained in Example 17 was greatly reduced. It can be seen that the use of cationic surfactants increases the probability of the conductive agent precipitating in the conductive slurry, which in turn affects the dispersion performance and storage stability of the conductive slurry.

[0049] Compared with Example 3, the conductive slurries obtained in Comparative Examples 1-3 all showed sedimentation stability, which greatly reduced the storage stability of the conductive slurries. This indicates that the preparation process and the combined use of the components in this application can improve the dispersion performance of the conductive agent, thereby ensuring the storage stability of the conductive slurry.

[0050] (2) The conductive pastes obtained in the embodiments and comparative examples of this application were used in the positive electrode system to evaluate their conductivity. Taking the lithium iron phosphate (LFP) system as an example, PVDF (polyvinylidene fluoride) was used as a binder. By mass percentage, the content of LFP was 95%, the content of conductive paste was 2%, and the content of PVDF was 3%. The solid content of the positive electrode paste was controlled at 50-60% according to the viscosity requirements. After the paste was mixed, it was uniformly coated on the PET film. After drying, the resistivity of the electrode was tested using a four-probe tester. The test results are shown in Table 2.

[0051] (3) Using the above electrode sheet as the positive electrode and the lithium sheet as the negative electrode, a CR2032 coin cell was prepared. The CR2032 coin cell was tested in the Blue Electric Test System. The charging and discharging conditions were set as follows: charging to the cutoff voltage of 4.2V and discharging to the cutoff voltage of 2.5V. The discharge capacity at 0.1C and 5C was measured after 5 cycles of 0.1C, 0.5C, 1C, 3C and 5C. The test results are shown in Table 2.

[0052] Table 2. Results of Electrode and Battery Performance Testing As can be seen from Table 2, the conductive slurry obtained in the embodiments of this application has better conductivity when used in batteries, and its discharge capacity and initial efficiency are better than those in the comparative examples.

[0053] The embodiments described herein are preferred embodiments of the present invention and are not intended to limit the scope of protection of the present invention. Therefore, all equivalent changes made in accordance with the structure, shape, and principle of the present invention should be covered within the scope of protection of the present invention.

Claims

1. A method for preparing an oily, high-solids-content carbon nanotube conductive paste, characterized in that, Includes the following steps: (1) Add the dispersant to the solvent and stir to disperse for 30-50 minutes; (2) Add conductive agent and surfactant to the mixture obtained in step (1) and perform ultrasonic dispersion treatment for 50-70 min; (3) The dispersion obtained in step (2) is ground in a sand mill at a ball-to-material mass ratio of 10:1 and a rotation speed of 1200-1500 rpm for 1-3 hours, then sieved and subjected to a second ultrasonic dispersion treatment for 40-60 minutes to obtain a conductive slurry. The conductive paste, by mass percentage, comprises: 10-12% conductive agent, 1.0-2.5% dispersant, 1.0-2.0% surfactant, and the remainder is solvent; The conductive agent includes graphene and carbon nanotubes, and the weight ratio of graphene to carbon nanotubes is 1:(2-4). The carbon nanotubes have an average diameter of 20-50 nm and a specific surface area of ​​70-110 m². 2 / g; The dispersant comprises sodium salt of 2-naphthalenesulfonic acid formaldehyde polymer and polyvinylpyrrolidone in a weight ratio of 1:(0.4-0.8). The surfactant is fatty alcohol polyoxyethylene ether phosphate and sodium dodecyl sulfate, and their weight ratio is 1:(0.8-1.2).

2. The method for preparing an oily, high-solids-content carbon nanotube conductive paste according to claim 1, characterized in that: The conductive paste, by mass percentage, comprises 10-12% conductive agent, 1.5-2.0% dispersant, 1.5-2.0% surfactant, and the balance being solvent.

3. The method for preparing an oily, high-solids-content carbon nanotube conductive paste according to claim 1, characterized in that: The viscosity of the conductive paste is 1000-3000 mPa·s.

4. A conductive paste obtained by the preparation method of the oily high-solids-content carbon nanotube conductive paste according to any one of claims 1-3.

Citation Information

Patent Citations

  • Composite conductive paste as well as preparation method and application thereof

    CN112331380A

  • Electroconductive paste, substrate equipped with electroconductive film, and method for manufacturing substrate equipped with electroconductive film

    CN113348217A