A method for preparing sesquioxide ceramics

By designing the ABA structure during the sintering process of sesquioxide ceramics, the problem of difficult to eliminate micro-stomatal pores in the ceramics is solved, and the high transmittance and low scattering loss of the ceramics are achieved, which improves its performance.

CN117088680BActive Publication Date: 2025-05-13SHANGHAI INST OF OPTICS & FINE MECHANICS CHINESE ACAD OF SCI
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202310901367.X
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-07-21
Publication Date
2025-05-13
Estimated Expiration
2043-07-21

AI Technical Summary

Technical Problem

The micro-stomata in sesquioxide ceramics is difficult to completely eliminate, resulting in a degradation in the performance of laser ceramics, limiting its application.

Method used

The ceramic preparation method with ABA structure is used. During the sintering process, the ceramic surface cannot be completely dense, which promotes the elimination of micro-air pores inside the ceramic, improves transmittance and reduces scattering losses.

Benefits of technology

Effectively eliminate residual micro-air pores to the maximum extent, reduce scattering losses, and improve the transmittance and performance of ceramics.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN117088680B_ABST
    Figure CN117088680B_ABST
Patent Text Reader

Abstract

The invention discloses a method for preparing sesquioxide ceramics. An ABA laminated structure is adopted during green blank forming. A layer of mixed powder A prepared by ball milling sesquioxide and magnesium oxide in a certain proportion is respectively covered on the upper and lower layers of sesquioxide powder B. The ABA structure is pressed and formed. During the sintering process, the A layer which will become the upper and lower surfaces of sesquioxide B is ground and polished to obtain sesquioxide ceramics. The invention can eliminate residual micropores to the greatest extent possible and reduce the scattering loss caused by the existence of micropores.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of transparent ceramic materials, and relates to a sesquioxide ceramic, and in particular to a preparation method of the sesquioxide ceramic. Background Art

[0002] Solid-state lasers have shown extremely important development prospects in the fields of communications, remote sensing, environmental monitoring, biomedicine, infrared countermeasures, etc. As one of the most promising high-power solid-state laser materials, sesquioxide materials have gradually attracted widespread attention due to their advantages such as low phonon energy, low thermal expansion coefficient and high thermal conductivity. However, due to the extremely high melting point of sesquioxide (>2420℃), its single crystal growth technology is very complicated, so it is difficult to grow high optical quality and large-sized sesquioxide single crystals. With the development of ceramic preparation technology, the sintering of sesquioxide ceramics provides another solution to overcome the technical difficulties of its crystal growth. Since the sintering temperature of sesquioxide ceramics is relatively low (~60%-70% of the melting point), it is easier to prepare larger-sized green bodies. Combined with the reasonable regulation of the sintering system and the control of its microstructure, the transparency of sesquioxide ceramics can be fully achieved.

[0003] Compared with non-solid solution laser ceramics, pores in sesquioxide solid solution laser ceramics are extremely difficult to eliminate. Because the presence of pore scattering points causes the various properties of laser ceramics to drop drastically, the micropores inside the ceramics have always been the bottleneck that prevents the application of this type of laser ceramics. In order to solve the micropores in ceramics, the industry has tried a lot of methods. For example, controlling the heating rate, controlling the powder size to make it as uniform as possible, avoiding abnormal growth of grains, and preventing the pores from being wrapped inside the grains to form scattering points; or increasing the sintering activity of the powder, and removing gas during the densification of the ceramics. For example, the patents with publication numbers CN114163235A (patent document 1) and CN115557787A (patent document 2) directly press the sesquioxide powder with higher sintering activity and then sinter in two steps. However, the above methods can only eliminate some larger pores, and some mist-like micropores cannot be completely eliminated. This is because in the traditional sintering method, heat transfer will inevitably produce a temperature gradient inside and outside the ceramic blank, and because the surface of the blank is more active than the inside, this causes the ceramic surface to be heated first and then dense. Before the internal micropores are completely eliminated, the outermost layer has formed a very dense shell. Once this shell is formed, the internal pores cannot be further discharged and can only remain inside the ceramic, affecting the ceramic performance. The Y2O3 surface coated with Zr 4+ , and during vacuum sintering, yttria and zirconium oxide powders are embedded to perform double-layer embedding sintering. Summary of the invention

[0004] The purpose of the present invention is to provide a method for preparing sesquioxide ceramics, design a new ceramic structure, and make the ceramic surface unable to be completely dense during the sintering process, so as to promote the further elimination of micropores inside the ceramic, improve the ceramic transmittance, and reduce scattering loss.

[0005] To achieve the above purpose, the technical solution adopted by the present invention is as follows:

[0006] A method for preparing sesquioxide ceramics adopts an ABA structure during molding, that is, a layer of mixed powder A prepared by ball-milling sesquioxide and magnesium oxide in a certain proportion is respectively covered on the upper and lower layers of sesquioxide powder B, and the mixture is pressed into shape with an ABA structure. During the sintering process, the A layer becomes the upper and lower surfaces of the ceramic. During the processing, the A layer is completely ground off, and then polished to obtain the sesquioxide ceramics.

[0007] The method for preparing sesquioxide ceramic by forming and sintering is characterized in that it comprises the following steps:

[0008] Step 1, weighing sesquioxide powder and magnesium oxide powder according to a mass ratio of 2:3-3:2, and adding alcohol as a solvent;

[0009] Step 2, placing the raw material powder weighed in step 1 into a ball mill, and adding grinding balls for ball milling and mixing while performing planetary ball milling, the ball milling speed is 120-180r / min, and the ball milling time is 12-24h;

[0010] Step 3, drying the slurry after ball milling in step 2 at a temperature of 40-60° C. for 10-24 hours, and then crushing the dried slurry and passing it through a 100-200 mesh sieve to obtain a mixed powder;

[0011] Step 4, weighing a certain amount of sesquioxide powder, and adding alcohol as a solvent;

[0012] Step 5, placing the raw material powder weighed in step 4 into a ball mill, and adding grinding balls to perform ball milling and mixing while performing planetary ball milling, the ball milling speed is 120-180r / min, and the ball milling time is 12-24h;

[0013] Step 6, drying the slurry after ball milling in step 5 at a temperature of 40-60° C. for 10-24 hours, and then crushing the dried slurry and passing it through a 100-200 mesh sieve to obtain sesquioxide powder;

[0014] Step 7, according to the blank forming schematic diagram, the powder is pressed into the required ceramic block. Then, cold isostatic pressing is performed at a pressure of 200-300 MPa and a holding time of 200-400 seconds to obtain a ceramic blank;

[0015] Step 8, sintering and annealing the ceramic blank, and then double-sided grinding and polishing to obtain sesquioxide ceramics.

[0016] The sesquioxide powder is selected from Lu, Sc and a rare earth element oxide powder and mixed by ball milling, and then the pressed body is sintered to produce transparent Re: (Lu 1-x Sc x )2O3 type sesquioxide sintered body.

[0017] Preferably, the sintering method described in step 8 is vacuum sintering and heated isostatic pressing sintering, the vacuum sintering temperature is 1600-1700°C, and the insulation time is 5-24h; the hot isostatic pressing sintering temperature is 1700-1800°C, and the insulation time is 3-7h, and the pressure is 120-200Mpa.

[0018] Beneficial effects:

[0019] In the traditional ceramic sintering method, the surface of the ceramic is heated first due to the existence of temperature gradient during the sintering process. After heating, the grains grow and become dense. After the surface is dense, the micro-gas inside the ceramic cannot be discharged smoothly, resulting in scattering during use, which affects the performance of the ceramic. To solve this problem, during molding, a new surface of sesquioxide ceramic is made by mixing sesquioxide and magnesium oxide powder. Since the densification temperature of the sesquioxide and magnesium oxide coating layers is higher than that of the sesquioxide middle layer, it cannot be completely dense during the sintering process, leaving a large number of pore channels on the surface. The gas inside the sesquioxide middle layer has the opportunity to be discharged, making the ceramic further dense and the transmittance further improved. In summary, it has the following advantages:

[0020] 1. When using this structure, residual micropores can be eliminated to the greatest extent possible.

[0021] 2. Reduce the scattering loss caused by the presence of micropores. BRIEF DESCRIPTION OF THE DRAWINGS

[0022] Figure 1 This is a transmittance diagram of the sesquioxide ceramic material prepared in Example 1, where the abscissa is wavelength and the ordinate is transmittance;

[0023] Figure 2 This is a scanning electron microscope image of the sesquioxide ceramic material prepared in Example 1.

[0024] Figure 3 This is a transmittance diagram of the sesquioxide ceramic material prepared in Example 2, where the abscissa is wavelength and the ordinate is transmittance;

[0025] Figure 4 This is a scanning electron microscope image of the sesquioxide ceramic material prepared in Example 2.

[0026] Figure 5 This is a transmittance diagram of the sesquioxide ceramic material prepared in Example 3, where the abscissa is wavelength and the ordinate is transmittance;

[0027] Figure 6 This is a scanning electron microscope image of the sesquioxide ceramic material prepared in Example 3.

[0028] Figure 7 This is a transmittance diagram of the sesquioxide ceramic material prepared in Example 4, where the abscissa is wavelength and the ordinate is transmittance;

[0029] Figure 8 This is a scanning electron microscope image of the sesquioxide ceramic material prepared in Example 4.

[0030] Fig. 9 This is a transmittance diagram of the sesquioxide ceramic material prepared in Example 5, where the abscissa is wavelength and the ordinate is transmittance;

[0031] Fig.10 This is a scanning electron microscope image of the sesquioxide ceramic material prepared in Example 5. DETAILED DESCRIPTION

[0032] The present invention is further described in detail below with reference to the accompanying drawings and specific embodiments.

[0033] Prepare 50g of mixed powder A and 50g of sesquioxide powder B, and weigh the raw powder ingredients separately. See Table 1. The measurement methods involved in the following examples are all conventional technical means in the art, and the materials are all commercial products, which will not be repeated here.

[0034] Table 1 Ingredients of Example

[0035]

[0036]

[0037] Example 1

[0038] A sesquioxide ceramic material has a surface layer mixed with powder A, and the mass ratio of the sesquioxide powder to the magnesium oxide powder is 1:1.

[0039] The method for preparing the above-mentioned sesquioxide ceramic material comprises the following steps:

[0040] Step 1, weigh 0.5g Yb2O3, 24.5g Lu2O3 and 25.00g MgO, and add 90ml alcohol as solvent;

[0041] Step 2, placing the raw material powder weighed in step 1 into a ball mill, and adding grinding balls for ball milling and mixing while performing planetary ball milling, the ball milling speed is 120r / min, and the ball milling time is 24h;

[0042] Step 3, drying the slurry after ball milling in step 2 at a temperature of 60° C. for 10 hours, and then crushing the dried slurry and passing it through a 100-mesh sieve to obtain a mixed powder;

[0043] Step 4, weigh 1.00 g Yb2O3, 49.00 g Lu2O3, and add 90 ml alcohol as solvent;

[0044] Step 5, placing the raw material powder weighed in step 4 into a ball mill, and adding grinding balls to perform ball milling and mixing while performing planetary ball milling, the ball milling speed is 120 r / min, and the ball milling time is 24 h;

[0045] Step 6, drying the slurry after ball milling in step 5 at a temperature of 60° C. for 10 hours, and then crushing the dried slurry and passing it through a 100-mesh sieve to obtain sesquioxide powder;

[0046] Step 7, according to the blank forming schematic diagram, the powder is pressed into the required ceramic block. Then, cold isostatic pressing is performed at a pressure of 200 MPa and a holding time of 200 seconds to obtain a ceramic blank;

[0047] Step 8, sinter the ceramic blank at 1600°C in vacuum for 5 hours, and hot isostatically press the blank at 1700°C for 7 hours at a pressure of 120 MPa. Anneal, double-sided grinding, and polishing are performed to obtain sesquioxide ceramics.

[0048] See attached Figure 1 This embodiment is a transmittance diagram of a sample of a sesquioxide ceramic material prepared from a mixed powder A with a mass ratio of 1:1. The test results of the spectrophotometer show that the transmittance of the prepared sesquioxide ceramic at 1200nm is 81.32%

[0049] See attached Figure 2 , This embodiment is a scanning electron microscope image of the surface of the sesquioxide ceramic prepared from the mixed powder A with a mass ratio of 1:1. The SEM test results show that there are almost no pores.

[0050] Example 2

[0051] A sesquioxide ceramic material has a surface layer mixed with powder A, and the mass ratio of sesquioxide powder to magnesium oxide powder is 2:3.

[0052] The method for preparing the above-mentioned sesquioxide ceramic material comprises the following steps:

[0053] Step 1, weigh 0.46g Yb2O3, 18.04g Lu2O3, 1.50g Sc2O3 and 30.00g MgO, and add 95ml alcohol as solvent;

[0054] Step 2, placing the raw material powder weighed in step 1 into a ball mill, and adding grinding balls for ball milling and mixing while performing planetary ball milling, the ball milling speed is 130r / min, and the ball milling time is 20h;

[0055] Step 3, drying the slurry after ball milling in step 2 at a temperature of 55° C. for 12 hours, and then crushing the dried slurry and passing it through a 120-mesh sieve to obtain a mixed powder;

[0056] Step 4, weigh 1.13 g Yb2O3, 45.11 g Lu2O3 and 3.76 g Sc2O3, and add 95 ml alcohol as solvent;

[0057] Step 5, placing the raw material powder weighed in step 4 into a ball mill, and adding grinding balls to perform ball milling and mixing while performing planetary ball milling, the ball milling speed is 130r / min, and the ball milling time is 20h;

[0058] Step 6, drying the slurry after ball milling in step 5 at a temperature of 55° C. for 12 hours, and then crushing the dried slurry and passing it through a 120-mesh sieve to obtain sesquioxide powder;

[0059] Step 7, according to the blank forming schematic diagram, the powder is pressed into the required ceramic block. Then, cold isostatic pressing is performed at a pressure of 220 MPa and a holding time of 240 seconds to obtain a ceramic blank;

[0060] Step 8, sinter the ceramic blank at 1640°C in vacuum for 10 hours, and hot isostatically press the sintering temperature at 1720°C for 6 hours at a pressure of 140 MPa. Anneal, double-sided grinding, and polishing are performed to obtain sesquioxide ceramics.

[0061] See attached Figure 3 This embodiment is a transmittance diagram of a sample of a sesquioxide ceramic material prepared from a mixed powder A with a mass ratio of 2:3. The test results of the spectrophotometer show that the transmittance of the prepared sesquioxide ceramic is 81.59%.

[0062] See attached Figure 4 , This embodiment is a scanning electron microscope image of the surface of the sesquioxide ceramic prepared from the mixed powder A with a mass ratio of 2:3. The SEM test results show that there are almost no pores.

[0063] Example 3

[0064] A sesquioxide ceramic material has a surface layer mixed with powder A, and the mass ratio of sesquioxide powder to magnesium oxide powder is 3:2.

[0065] The method for preparing the above-mentioned sesquioxide ceramic material comprises the following steps:

[0066] Step 1, weigh 0.80g Yb2O3, 23.76g Lu2O3, 5.44g Sc2O3 and 20.00g MgO, and add 100ml alcohol as solvent;

[0067] Step 2, placing the raw material powder weighed in step 1 into a ball mill, and adding grinding balls for ball milling and mixing while performing planetary ball milling, the ball milling speed is 150r / min, and the ball milling time is 18h;

[0068] Step 3, drying the slurry after ball milling in step 2 at a temperature of 50° C. for 14 hours, and then crushing the dried slurry and passing it through a 150-mesh sieve to obtain a mixed powder;

[0069] Step 4, weigh 1.33 g Yb2O3, 39.60 g Lu2O3 and 9.07 g Sc2O3, and add 100 ml alcohol as solvent;

[0070] Step 5, placing the raw material powder weighed in step 4 into a ball mill, performing planetary ball milling while adding grinding balls for ball milling mixing, the ball milling speed is 150r / min, and the ball milling time is 18h;

[0071] Step 6, drying the slurry after ball milling in step 5 at a temperature of 50° C. for 18 hours, and then crushing the dried slurry and passing it through a 150-mesh sieve to obtain sesquioxide powder;

[0072] Step 7, according to the blank forming schematic diagram, the powder is pressed into the required ceramic block. Then, cold isostatic pressing is performed at a pressure of 260 MPa and a holding time of 280 seconds to obtain a ceramic blank;

[0073] Step 8, sinter the ceramic blank at 1660°C in vacuum for 14 hours, and hot isostatically press the sintering temperature at 1740°C for 5 hours at a pressure of 160 MPa. Anneal, double-sided grinding, and polishing are performed to obtain sesquioxide ceramics.

[0074] See attached Figure 5 This embodiment is a transmittance diagram of a sample of a sesquioxide ceramic material prepared from a mixed powder A with a mass ratio of 3:2. The test results of the spectrophotometer show that the transmittance of the prepared sesquioxide ceramic is 81.76%.

[0075] See attached Figure 6, This embodiment is a scanning electron microscope image of the surface of the sesquioxide ceramic prepared from the mixed powder A with a mass ratio of 3:2. The SEM test results show that there are almost no pores.

[0076] Example 4

[0077] A sesquioxide ceramic material, wherein the mass ratio of the mixed powder sesquioxide powder / magnesium oxide powder in the surface layer is 4:5.

[0078] The method for preparing the above-mentioned sesquioxide ceramic material comprises the following steps:

[0079] Step 1, weigh 0.72g Yb2O3, 14.09g Lu2O3, 7.39g Sc2O3 and 27.80g MgO, and add 105ml alcohol as solvent;

[0080] Step 2, placing the raw material powder weighed in step 1 into a ball mill, performing planetary ball milling while adding grinding balls for ball milling mixing, the ball milling speed is 160r / min, and the ball milling time is 20h;

[0081] Step 3, drying the slurry after ball milling in step 2 at a temperature of 45° C. for 20 hours, and then crushing the dried slurry and passing it through a 180-mesh sieve to obtain a mixed powder;

[0082] Step 4, weigh 1.61 g Yb2O3, 31.75 g Lu2O3 and 16.64 g Sc2O3, and add 105 ml alcohol as solvent;

[0083] Step 5, placing the raw material powder weighed in step 4 into a ball mill, performing planetary ball milling while adding grinding balls for ball milling mixing, the ball milling speed is 160r / min, and the ball milling time is 20h;

[0084] Step 6, drying the slurry after ball milling in step 5 at a temperature of 45° C. for 20 hours, and then crushing the dried slurry and passing it through a 180-mesh sieve to obtain sesquioxide powder;

[0085] Step 7, according to the blank forming schematic diagram, the powder is pressed into the required ceramic block. Then, cold isostatic pressing is performed at a pressure of 280 MPa and a holding time of 380 seconds to obtain a ceramic blank;

[0086] Step 8, sinter the ceramic blank at 1680°C in vacuum for 20 hours, and hot isostatically press the sintering temperature at 1760°C for 4 hours at a pressure of 180 MPa. Anneal, double-sided grinding, and polishing are performed to obtain sesquioxide ceramics.

[0087] See attached Figure 7This embodiment is a transmittance diagram of a sample of a sesquioxide ceramic material prepared from a mixed powder A with a mass ratio of 4:5. The test results of the spectrophotometer show that the transmittance of the prepared sesquioxide ceramic is 82.26%.

[0088] See attached Figure 8 , This embodiment is a scanning electron microscope image of the surface of the sesquioxide ceramic prepared from the mixed powder A with a mass ratio of 4:5. The SEM test results show that there are almost no pores.

[0089] Example 5

[0090] A sesquioxide ceramic material, wherein the mass ratio of mixed powder sesquioxide powder / magnesium oxide powder in the surface layer is 5:4.

[0091] The method for preparing the above-mentioned sesquioxide ceramic material comprises the following steps:

[0092] Step 1, weigh 1.53g Yb2O3, 26.27g Sc2O3 and 22.20g MgO, and add 110ml alcohol as solvent;

[0093] Step 2, placing the raw material powder weighed in step 1 into a ball mill, and adding grinding balls for ball milling and mixing while performing planetary ball milling, the ball milling speed is 180r / min, and the ball milling time is 24h;

[0094] Step 3, drying the slurry after ball milling in step 2 at a temperature of 40° C. for 24 hours, and then crushing the dried slurry and passing it through a 200-mesh sieve to obtain a mixed powder;

[0095] Step 4, weigh 2.75g Yb2O3, 47.25g Sc2O3, and add 110ml alcohol as solvent;

[0096] Step 5, placing the raw material powder weighed in step 4 into a ball mill, performing planetary ball milling while adding grinding balls for ball milling mixing, the ball milling speed is 180r / min, and the ball milling time is 24h;

[0097] Step 6, drying the slurry after ball milling in step 5 at a temperature of 40° C. for 24 hours, and then crushing the dried slurry and passing it through a 200-mesh sieve to obtain sesquioxide powder;

[0098] Step 7, according to the blank forming schematic diagram, the ceramic is pressed into the required ceramic block. Then, cold isostatic pressing is performed at a pressure of 300 MPa and a holding time of 400 seconds to obtain a ceramic blank;

[0099] Step 8, sinter the ceramic blank at 1700°C in vacuum for 24 hours, and hot isostatically press the blank at 1800°C for 3 hours at a pressure of 200 MPa. Anneal, double-sided grinding, and polishing are performed to obtain sesquioxide ceramics.

[0100] See attached Fig. 9 This embodiment is a transmittance diagram of a sample of a sesquioxide ceramic material prepared from a mixed powder A with a mass ratio of 5:4. The test results of the spectrophotometer show that the transmittance of the prepared sesquioxide ceramic is 81.34%.

[0101] See attached Fig.10 , This embodiment is a scanning electron microscope image of the surface of the sesquioxide ceramic prepared from the mixed powder A with a mass ratio of 5:4. The SEM test results show that there are almost no pores.

[0102] In summary, the transmittance of sesquioxide ceramics is significantly improved, the porosity is significantly reduced, and the scattering loss is also reduced to a certain extent.

[0103] The above is only a preferred specific implementation manner of the present invention, and the protection scope of the present invention is not limited thereto. Any simple change or equivalent replacement of the technical solution that can be obviously obtained by any technician familiar with the technical field within the technical scope disclosed in the present invention falls within the protection scope of the present invention.

Claims

1. A method for preparing sesquioxide ceramics, characterized in that: The ABA laminated structure is adopted in the green billet molding, that is, a layer of mixed powder A prepared by ball-milling sesquioxide powder B and magnesium oxide is respectively covered on the upper and lower layers of sesquioxide powder B, and the mixture is pressed into the ABA structure; During the sintering process, the A layer, which will become the upper and lower surfaces of the sesquioxide B, is ground and polished to obtain a sesquioxide ceramic; The sesquioxide powder is selected from Lu, Sc and a rare earth element oxide powder and mixed by ball milling, and then the pressed body is sintered to produce transparent Re: (Lu 1-x Sc x )2O3 type sesquioxide sintered body.

2. The method for preparing sesquioxide ceramics according to claim 1, characterized in that: The following steps are involved: Step 1, weighing sesquioxide powder and magnesium oxide powder according to a mass ratio of 2:3-3:2, and adding alcohol as a solvent; Step 2, placing the raw material powder weighed in step 1 into a ball mill, performing planetary ball milling while adding grinding balls for ball milling mixing, the ball milling speed is 120-180 r / min, and the ball milling time is 12-24 h; Step 3, drying the slurry after ball milling in step 2 at a temperature of 40-60 ° C for 10-24 hours, and then crushing the dried slurry and passing it through a 100-200 mesh sieve to obtain a mixed powder; Step 4, weighing a certain amount of sesquioxide powder, and adding alcohol as a solvent; Step 5, placing the raw material powder weighed in step 4 into a ball mill, performing planetary ball milling while adding grinding balls for ball milling mixing, the ball milling speed is 120-180 r / min, and the ball milling time is 12-24 h; Step 6, drying the slurry after ball milling in step 5 at a temperature of 40-60 ° C for 10-24 hours, then crushing the dried slurry and passing it through a 100-200 mesh sieve to obtain sesquioxide powder; Step 7, pressing the powder into the desired ceramic block, and then performing cold isostatic pressing at a pressure of 200-300 MPa and a holding time of 200-400 s to obtain a ceramic green body; Step 8, sintering and annealing the ceramic blank, and then double-sided grinding and polishing to obtain sesquioxide ceramics.

3. The method for preparing sesquioxide ceramics according to claim 2, characterized in that: The sintering method described in step 8 is vacuum sintering and heated isostatic pressing sintering, the vacuum sintering temperature is 1600-1700° C., and the heat preservation time is 5-24 h; the hot isostatic pressing sintering temperature is 1700-1800° C., and the heat preservation time is 3-7 h.

Citation Information

Patent Citations

  • Preparation method of high-transmittance Dy: Y2O3 transparent ceramic

    CN114163235A

  • Sesquioxide transparent ceramic and preparation method thereof

    CN115557787A

  • Preparation method of transparent ceramic with high infrared transmittance

    CN115784742A

  • ABA type sandwich composite material and preparation method thereof

    CN111516314A

  • Preparation method and application of transparent ceramic with multi-layer composite structure

    CN112174668A