A permanent magnet and a method for preparing the same, and a permanent magnet drive motor
By adopting a shell-core structure and tin/zinc-plated graphene distribution in rare earth permanent magnets, the problem of insufficient performance of rare earth permanent magnets is solved, and high coercivity, durability and bending strength are improved, which is suitable for long-life and high-voltage applications. Performance permanent magnet drive motor.
Patent Information
- Application Number
- CN202210520131.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-05-13
- Publication Date
- 2024-10-11
- Estimated Expiration
- 2042-05-13
AI Technical Summary
It is difficult for existing rare earth permanent magnets to have high coercivity, high durability and high bending strength at the same time, and increasing the content of precious rare earths will affect their overall performance.
A permanent magnet with a shell-core structure is used, including a main phase and a grain boundary phase isolated between them, and tin-plated and/or zinc-plated graphene is evenly distributed in the shell layer and grain boundary phase, and is pressed and formed through magnetic field orientation and hot pressing treatment. Improve its mechanical properties and magnetic properties.
The low-cost permanent magnet is realized with excellent mechanical properties, good magnetic properties and high-temperature external field durability, extending the service life and improving the overall performance.
Smart Images

Figure CN117095901B_ABST
Abstract
Description
Technical Field
[0001] The present application relates to the technical field of permanent magnet materials, and in particular to a permanent magnet and a preparation method thereof, and a permanent magnet drive motor. Background Art
[0002] Rare earth permanent magnets have been widely used in many fields such as new energy vehicles, wind power generation, and household appliances due to their small size, light weight, and high energy conversion efficiency. However, it is difficult for current rare earth permanent magnets to have high coercivity, high durability, and high bending strength without special treatment. At present, the industry often increases the content of precious rare earths to improve the magnetic properties of rare earth permanent magnets, but this does not improve the mechanical properties of rare earth permanent magnets, and may even affect the comprehensive performance of rare earth permanent magnets. Summary of the invention
[0003] In view of this, the present application provides a permanent magnet and a preparation method thereof and a permanent magnet drive motor, wherein the permanent magnet comprises a main phase having a core-shell structure, a grain boundary phase isolated between the main phases, and tin-plated and / or zinc-plated graphene uniformly distributed in the main phase shell and the grain boundary phase. The permanent magnet has low cost, excellent mechanical properties, good magnetic properties and high-temperature external field durability, and can be used to provide a permanent magnet drive motor with a long service life and excellent comprehensive performance.
[0004] Specifically, the first aspect of the present application provides a permanent magnet, which includes a main phase and a grain boundary phase, wherein the grain boundary phase isolates and / or covers the adjacent main phase; the main phase includes a shell layer and a core layer, and tin-plated and / or zinc-plated graphene is dispersed in the grain boundary phase and the shell layer;
[0005] The core consists of RL1 a RH1 b Fe c Co d B e , RL1 includes at least one of Pr and Nd, RH1 includes at least one of La, Ce, Sm, Gd, Ho and Y, wherein a, b, c, d, e represent weight percentages, 10.2≤a≤16.2, 12.4≤b≤18.9, 59.99≤c≤76.18, 0≤d≤2.6, 0.72≤e≤1.41;
[0006] The shell layer comprises RL2 f RH2 g RH3 h Fe i Co j B k M1 l, RL2 includes at least one of Pr and Nd, RH2 includes at least one of La, Ce, Sm, Gd, Ho and Y, RH3 includes at least one of Dy and Tb, and M1 includes at least one of Zr, Ga, Cu, Sn, Al, Zn, Bi, Ta, In, Pb, Cd, Tl, Sb and Ge, wherein f, g, h, i, j, k, l represent weight percentages, 23.71≤f+g+h≤59.2, 3.7≤g≤7.72, 9≤h≤17.07, f>0, 18.33≤i≤68.17, 0≤j≤2, 0.22≤k≤0.57, 7.4≤l≤19;
[0007] The composition of the grain boundary phase includes RL3 m RH4 n Fe o Co p M2 q , RL3 includes at least one of La, Ce, Sm, Pr and Nd, RH4 includes at least one of Dy and Tb, and M2 includes at least one of Zr, Ga, Cu, Sn, Al, Zn, Bi, Ta, In, Pb, Cd, Tl, Sb and Ge, wherein m, n, o, p, q represent weight percentages, and 34≤m+n≤57.8, 15.2≤n≤24.55, 12.56≤o≤53.19, 0≤p≤1.43, and 12.31≤q≤27.31.
[0008] The permanent magnet comprises a main phase with a core-shell structure, a grain boundary phase isolated between the main phases, and tinned and / or zinc-plated graphene uniformly distributed in the main phase shell and the grain boundary phase. The shell can increase the magnetocrystalline anisotropy field of the main phase, reduce the magnetic exchange coupling between the main phases, and increase the coercive force of the permanent magnet. In addition, the graphene can improve the bending performance of the permanent magnet. The permanent magnet has excellent comprehensive performance and low cost.
[0009] Optionally, the mass percentage of the main phase in the permanent magnet is in the range of 60%-80%; the mass percentage of the grain boundary phase in the permanent magnet is in the range of 20%-40%.
[0010] Optionally, the mass percentage of the tin-plated and / or zinc-plated graphene in the grain boundary phase is in the range of 0.07%-2.25%, and the mass percentage of the tin-plated and / or zinc-plated graphene in the shell layer is in the range of 0.04%-1.58%.
[0011] Optionally, the mass percentage A of the tinned and / or galvanized graphene in the permanent magnet satisfies: 0%<A<0.9%. Preferably, the mass percentage A of the tinned and / or galvanized graphene in the permanent magnet satisfies: 0.1%<A<0.9%.
[0012] Optionally, in the composition of the kernel, 10.3≤a≤16, 12.5≤b≤18.7, 60.64≤c≤75.65, 0.2≤d≤2.5, and 0.75≤e≤1.36.
[0013] Optionally, in the composition of the shell layer, 24≤f+g+h≤58, 4≤g≤7, 10≤h≤16, 21.2≤i≤66.6, 0.5≤j≤1.5, 0.3≤k≤0.5, and 8≤l≤18.
[0014] Optionally, in the composition of the grain boundary phase, 36≤m+n≤55, 16≤n≤23, 15.46≤o≤51.09, 0≤p≤1.43, and 12.31≤q≤27.31.
[0015] Optionally, the thickness of the shell layer is in the range of 0.1 μm-8.5 μm. Preferably, the thickness of the shell layer is in the range of 0.8 μm-7.4 μm. More preferably, the thickness of the shell layer is in the range of 1.2 μm-6.5 μm.
[0016] Optionally, the ratio of the sum of the masses of the RL2 and the RH2 to the sum of the masses of the RL1 and the RH1 is 1:(1.01-2.62).
[0017] Optionally, the average particle size of the tin-plated and / or galvanized graphene is in the range of 10nm-25nm. Preferably, the average particle size of the tin-plated and / or galvanized graphene is in the range of 15nm-23nm.
[0018] Optionally, the permanent magnet is a sheet material, and the thickness of the permanent magnet is in the range of 1 mm to 10 mm. Preferably, the thickness of the permanent magnet is in the range of 2 mm to 7 mm.
[0019] Optionally, the permanent magnet further comprises a diffusion alloy enriched layer located on the surface of the permanent magnet, and the thickness of the diffusion alloy enriched layer is in the range of 5 μm-15 μm. Preferably, the thickness of the diffusion alloy enriched layer is in the range of 7 μm-15 μm.
[0020] Optionally, the composition of the diffusion alloy layer includes R4xR5yFezNt, R4 includes at least one of Pr and Nd, R5 includes at least one of Dy and Tb, N includes at least one of Ga, Cu, Sn, Al, Zn, Bi, Ta, In, Pb, Cd, Tl, Sb and Ge, x, y, z, t represent weight proportions, and 37.2≤x≤45.7, 23.8≤y≤32, 1.4≤z≤23, 15.5≤t≤20.
[0021] A second aspect of the present application provides a method for preparing a permanent magnet, the method comprising the following steps:
[0022] (1) uniformly mixing a first main phase alloy powder raw material, a second main phase alloy powder raw material, and a grain boundary phase alloy powder raw material to obtain a first mixed material, and then performing magnetic field orientation pressing, sintering, and a first tempering treatment to obtain a permanent magnet blank;
[0023] Wherein, the composition of the first main phase powder raw material is: R1 a’ Fe b’ Co c’ B d’ , R1 includes at least one of Pr and Nd, a', b', c', d' represent weight percentages, and 25.5≤a'≤29.5, 66.4≤b'≤73.1, 0≤c'≤2, 0.9≤d'≤1.2; the composition of the second main phase alloy powder raw material is: R2 e’ Fe f’ Co g’ B h’ , R2 includes at least one of La, Ce, Sm, Gd, Ho and Y, e', f', g', h' represent weight percentages, and 27.5≤e'≤31.5, 0≤g'≤2.5, 63.85≤f'≤71.2, 0.8≤h'≤1.25; the composition of the grain boundary phase alloy powder raw material includes R3 i’ Fe j’ Co k’ M l’ , R3 includes at least one of La, Ce, Sm, Pr and Nd, M includes at least one of Zr, Ga, Cu, Sn, Al, Zn, Bi, Ta, In, Pb, Cd, Tl, Sb and Ge, i', j', k', l' represent weight percentages, and 40≤i'≤65, 5.1≤j'≤49.5, 0≤k'≤4, 10≤l'≤25;
[0024] (2) uniformly mixing the tin-plated and / or galvanized graphene and the diffusion alloy powder raw material to obtain a second mixture, and placing the second mixture on the surface of the permanent magnet blank;
[0025] (3) performing hot pressing and diffusion treatment on the permanent magnet blank with the second mixed material on the surface, or performing the hot pressing, diffusion and surface polishing treatments in sequence, to obtain the permanent magnet provided in the first aspect of the present application;
[0026] Wherein, the composition of the diffusion alloy powder raw material includes R4 x R5 y Fe z N t, R4 includes at least one of Pr and Nd, R5 includes at least one of Dy and Tb, N includes at least one of Ga, Cu, Sn, Al, Zn, Bi, Ta, In, Pb, Cd, Tl, Sb and Ge, x, y, z, t represent weight percentages, and 37.2≤x≤45.7, 23.8≤y≤32, 1.4≤z≤23, and 15.5≤t≤20.
[0027] The preparation method has simple steps, strong operability and high production efficiency, and can be applied to large-scale industrial preparation.
[0028] Optionally, in the diffusion alloy powder raw material, 38≤x≤45, 24≤y≤30, 5.1≤z≤21.5, and 16≤t≤19.
[0029] Optionally, the mass percentage of the grain boundary phase alloy powder raw material in the permanent magnet raw material is 3%-15%.
[0030] Optionally, the mass ratio of the first main phase alloy powder raw material to the second main phase alloy powder raw material is 1:(0.6-1.33).
[0031] Optionally, the mass percentage of the tinned and / or galvanized graphene in the second mixture is 0.1%-3%. Preferably, the mass percentage of the tinned and / or galvanized graphene in the second mixture is 0.5%-2.5%.
[0032] Optionally, the average particle size of the diffusion alloy powder raw material is 30nm-85nm. Preferably, the average particle size of the diffusion alloy powder raw material is 35nm-80nm.
[0033] Optionally, the heat pressing treatment conditions include: performing the treatment in a vacuum environment with an absolute vacuum degree of 10 -3 Pa-10 - 2 Pa, the pressing pressure is 80MPa-150MPa, the temperature is 550℃-800℃, and the holding time is 30min-150min; wherein the direction of the pressing pressure is parallel to the direction of the easy magnetization axis of the permanent magnet blank.
[0034] Optionally, the diffusion treatment conditions include: a temperature of 600°C-1000°C, a time of 2h-12h, an absolute vacuum of 10 -5 Pa-10 -2 Pa.
[0035] Optionally, the diffusion alloy powder raw material is obtained by a melt rapid quenching method.
[0036] Optionally, the speed of the rapid quenching is 18m / s-28m / s. Preferably, the speed of the rapid quenching is 19m / s-26m / s.
[0037] Optionally, the tin-plated and / or galvanized graphene is obtained by plating tin and / or galvanizing on the surface of graphene.
[0038] Optionally, the method further comprises dispersing the graphene in an ethanol solution before the tin plating and / or zinc plating treatment.
[0039] Optionally, the dispersion includes ultrasonic treatment, and the conditions of the ultrasonic treatment are: ultrasonic power is 1000w-1500w, time is 5min-30min, and after dispersion, the graphene is placed in an environment of 120℃-140℃ and dried for 20min-150min.
[0040] Optionally, after the diffusion treatment, a second tempering treatment is further included, and the conditions of the second tempering treatment include: a temperature of 400°C-600°C, a time of 2.5h-10h, an absolute pressure of 10 -5 Pa-10 -2 Pa.
[0041] The third aspect of the present application provides a permanent magnet drive motor, which has the permanent magnet provided by the first aspect of the present application. The permanent magnet drive motor has a long service life and better overall performance, and can be applied to new energy vehicles and other fields. BRIEF DESCRIPTION OF THE DRAWINGS
[0042] Figure 1 A schematic diagram of a partial cross section of a permanent magnet provided in one embodiment of the present application;
[0043] Figure 2 This is a scanning electron microscopy (SEM) photograph of the cross section of the permanent magnet provided in Example 1 of the present application.
[0044] Description of the drawings: 100 - permanent magnet; 10 - main phase; 101 - inner core; 102 - shell; 20 - grain boundary phase; 30 - tinned and / or galvanized graphene. DETAILED DESCRIPTION
[0045] The technical solution of the present application is described in detail below with reference to the accompanying drawings.
[0046] See also Figure 1 The embodiment of the present application provides a permanent magnet 100, which includes a main phase 10 and a grain boundary phase 20, wherein the grain boundary phase 20 isolates the main phase 10; the main phase 10 includes a core 101 and a shell 102, wherein tin-plated and / or zinc-plated graphene 30 is dispersed in the grain boundary phase 20 and the shell 102;
[0047] The core 101 consists of RL1 a RH1 b Fe c Co d B e , RL1 includes at least one of Pr and Nd, RH1 includes at least one of La, Ce, Sm, Gd, Ho and Y, wherein a, b, c, d, e represent weight percentages, 10.2≤a≤16.2, 12.4≤b≤18.9, 59.99≤c≤76.18, 0≤d≤2.6, 0.72≤e≤1.41;
[0048] The shell 102 comprises RL2 f RH2 g RH3 h Fe i Co j B k M1 l , RL2 includes at least one of Pr and Nd, RH2 includes at least one of La, Ce, Sm, Gd, Ho and Y, RH3 includes at least one of Dy and Tb, and M1 includes at least one of Zr, Ga, Cu, Sn, Al, Zn, Bi, Ta, In, Pb, Cd, Tl, Sb and Ge, wherein f, g, h, i, j, k, l represent weight percentages, 23.71≤f+g+h≤59.2, 3.7≤g≤7.72, 9≤h≤17.07, f>0, 18.33≤i≤68.17, 0≤j≤2, 0.22≤k≤0.57, 7.4≤l≤19;
[0049] The composition of the grain boundary phase 20 includes RL3 m RH4 n Fe o Co p M2 q , RL3 includes at least one of La, Ce, Sm, Pr and Nd, RH4 includes at least one of Dy and Tb, and M2 includes at least one of Zr, Ga, Cu, Sn, Al, Zn, Bi, Ta, In, Pb, Cd, Tl, Sb and Ge, wherein m, n, o, p, q represent weight percentages, and 34≤m+n≤57.8, 15.2≤n≤24.55, 12.56≤o≤53.19, 0≤p≤1.43, and 12.31≤q≤27.31.
[0050] The permanent magnet 100 includes a main phase 10 with a core-shell structure, a grain boundary phase 20 isolating the main phase 10, and tinned and / or galvanized graphene 30 is also dispersed in the grain boundary phase 20 and the shell layer 102. The tinned or galvanized graphene can significantly improve the mechanical properties of the permanent magnet 100, especially the bending resistance, thereby greatly broadening the processability and assemblability of the permanent magnet 100, and greatly improving the comprehensive performance of the permanent magnet 100. The tinned and / or galvanized layer on the surface of the graphene can increase the density of the graphene, and is converted into a molten state during the preparation process of the permanent magnet 100, so as to improve the wettability of the molten state grain boundary phase to the graphene during the preparation process of the permanent magnet, thereby smoothly preparing the permanent magnet 100, and increasing the interface bonding force between the graphene and the grain boundary phase material and the shell material, avoiding the agglomeration of the graphene, etc.
[0051] In addition, the permanent magnet 100 contains a large amount of high-abundance rare earth elements (such as Ce, Y, La, etc.), which can reduce the cost of the permanent magnet 100 while ensuring that the permanent magnet 100 has sufficient magnetism. Dy and / or Tb, Pr and / or Nd in the shell 102 can work together with Fe and B to generate a material that can enhance magnetic anisotropy (for example, Dy2Fe 14 B and / or Tb2Fe 14 B. Pr2Fe 14 B and / or Nd2Fe 14 B), and the coexistence of the shell 102 and the grain boundary phase 20 can better separate the adjacent core materials, avoid magnetic coupling exchange between the core materials, and inhibit the generation of reverse magnetization domains, thereby significantly enhancing the overall coercive force and high-temperature external field durability of the permanent magnet 100, and at the same time can ensure that the residual magnetic properties of the permanent magnet 100 are good to the greatest extent.
[0052] In summary, the permanent magnet 100 provided in the embodiment of the present application has excellent mechanical properties and good and stable magnetic properties, good machinability and good workpiece adaptability, and its cost is low. The permanent magnet 100 can also be used to provide a permanent magnet drive motor with a long service life and better comprehensive performance.
[0053] In the present application, the permanent magnet 100 may contain trace impurities in the core 101, the shell 102, and the grain boundary phase 20. The impurities are brought from the metal raw materials, such as Y, Er, Si, W, Mo, C, Ca, N, O, S, P, etc.
[0054] In this application, the core 101 comprises RL1 a RH1 b Fe c Co d B e. Exemplarily, the value of a can be 10.2, 10.3, 10.5, 11, 11.5, 12, 12.5, 13, 14, 15, 16, 16.2, etc. Exemplarily, the value of b can be 12.4, 12.5, 13, 14, 15, 16, 17, 18, 18.7, 18.9, etc. Exemplarily, the value of c can be 59.99, 60.64, 61, 62, 63, 64, 65, 66, 67, 68, 69, 70, 71, 72, 73, 74, 75, 75.65, 76, 76.18. Exemplarily, the value of d can be 0, 0.2, 0.5, 1, 1.5, 2, 2.5, 2.6, etc. Illustratively, the value of e may be 0.72, 0.75, 0.8, 0.9, 1, 1.2, 1.3, 1.36, 1.41, etc.
[0055] The shell 102 comprises RL2 f RH2 g RH3 h Fe i Co j B k M1 l . Exemplarily, the value of f+g+h can be 23.71, 24, 24.5, 25, 26, 27, 28, 29, 30, 35, 40, 45, 50, 55, 58, 59.2, etc. Exemplarily, the value of g can be 3.7, 4, 4.5, 5, 5.5, 6, 6.5, 7, 7.5, 7.72, etc. Exemplarily, the value of h can be 9, 10, 11, 12, 13, 14, 15, 16, 17, 17.07, etc. Exemplarily, the value of j can be 0, 0.5, 1, 1.5, 2, etc. Exemplarily, the value of i can be 18.33, 20, 21.2, 25, 30, 35, 40, 45, 50, 55, 60, 65, 66.6, 68, 68.17, etc. Exemplarily, the value of k can be 0.22, 0.3, 0.35, 0.4, 0.45, 0.5, 0.57, etc. Exemplarily, the value of l can be 7.4, 8, 9, 10, 11, 12, 13, 14, 15, 16, 17, 18, 19, etc.
[0056] The composition of the grain boundary phase 20 includes RL3 m RH4 n Fe o Co p M2 q. Exemplarily, the value of m+n can be 34, 35, 36, 40, 45, 50, 55, 57.8, etc. Exemplarily, the value of n can be 15.2, 16, 18, 20, 21, 22, 23, 24, 24.55, etc. Exemplarily, the value of o can be 12.56, 13, 15, 15.46, 20, 25, 30, 35, 40, 45, 50, 51.09, 53, 53.19, etc. Exemplarily, the value of p can be 0, 0.5, 1, 1.43, etc. Exemplarily, the value of q can be 12.31, 13, 14, 15, 20, 25, 26, 27, 27.31, etc.
[0057] In some embodiments of the present application, the average particle size of the tinned and / or galvanized graphene 30 is 10nm-25nm. Exemplarily, the average particle size of the tinned and / or galvanized graphene 30 can be 10nm, 12.5nm, 15nm, 17.5nm, 20nm, 22.5nm, 23nm, 25nm, etc. In some specific embodiments, the average particle size of the tinned and / or galvanized graphene 30 is 15nm-23nm. The size of the galvanized and / or galvanized graphene 30 is within the above range to effectively improve the mechanical properties of the permanent magnet 100, and can reduce its uniform dispersion in the permanent magnet 100, reducing the preparation cost and process difficulty.
[0058] In some embodiments of the present application, the mass percentage of tinned and / or galvanized graphene 30 in the shell layer 102 is 0.04%-1.58%, and the mass percentage of tinned and / or galvanized graphene 30 in the grain boundary phase 20 is 0.07%-2.25%. Exemplarily, the mass percentage of tinned and / or galvanized graphene 30 in the shell layer 102 can be 0.04%, 0.1%, 0.2%, 0.3%, 0.4%, 0.5%, 0.6%, 0.7%, 0.8%, 0.9%, 1.0%, 1.1%, 1.2%, 1.3%, 1.4%, 1.5%, 1.58%, etc. For example, the mass percentage of the tinned and / or galvanized graphene 30 in the grain boundary phase 20 may be 0.07%, 0.1%, 0.25%, 0.5%, 0.75%, 1.0%, 1.25%, 1.5%, 1.75%, 2.0%, 2.25%, etc. In combination with the mass percentages of the main phase 10 and the grain boundary phase 20 in the permanent magnet 100, in some specific embodiments, the mass percentage A of the tinned and / or galvanized graphene 30 in the permanent magnet 100 satisfies: 0%<A<0.9%. In other specific embodiments, the mass percentage A of the tinned and / or galvanized graphene 30 in the permanent magnet 100 satisfies: 0.1%<A<0.9%. For example, the value of A can be 0.05%, 0.11%, 0.15%, 0.2%, 0.3%, 0.4%, 0.5%, 0.6%, 0.7%, 0.8%, 0.85%, 0.89%, etc. Controlling the content of tin-plated and / or galvanized graphene 30 within the above range is conducive to ensuring that the mechanical properties (especially bending resistance) of the permanent magnet 100 are good.
[0059] In some embodiments of the present application, the mass percentage B of the main phase 10 in the permanent magnet 100 satisfies 60%≤B≤80%, and the mass percentage C of the grain boundary phase 20 in the permanent magnet 100 satisfies 20%≤C≤40%. For example, the value of B can be 60%, 62.5%, 65%, 67.5%, 70%, 72.5%, 75%, 77.5%, 80%, etc. For example, the value of C can be 20%, 22.5%, 25%, 27.5%, 30%, 32.5%, 35%, 37.5%, 40%, etc. Controlling the mass percentages of the above two structures within the above range is conducive to ensuring that the microstructure of the permanent magnet 100 is within the range defined in the present application, thereby ensuring that the overall performance of the permanent magnet 100 is better.
[0060] In some embodiments of the present application, the thickness of the shell 102 is 0.1 μm-8.5 μm. For example, the thickness of the shell 102 can be 0.1 μm, 0.5 μm, 1 μm, 1.5 μm, 2 μm, 2.5 μm, 3 μm, 3.5 μm, 4 μm, 4.5 μm, 5 μm, 5.5 μm, 6 μm, 6.5 μm, 7 μm, 7.5 μm, 8 μm, 8.5 μm, etc. In some specific embodiments, the thickness of the shell 102 is in the range of 0.8 μm-7.4 μm. In other specific embodiments, the thickness of the shell 102 is in the range of 1.2 μm-6.5 μm. Controlling the thickness of the shell 102 within the above range is conducive to ensuring that the coercive force and residual magnetic properties of the permanent magnet 100 are high.
[0061] In some embodiments of the present application, in the main phase 10, the ratio of the sum of the masses of the RL2, the RH2 and the RH3 to the sum of the masses of the RL1 and the RH1 is 1:(1.01-2.62). Exemplarily, the ratio of the sum of the masses of the RL2, the RH2 and the RH3 to the sum of the masses of the RL1 and the RH1 can be 1:1.01, 1:1.1, 1:1.5, 1:2, 1:2.5, 1:2.62, etc. In this way, during the preparation process, Dy and Tb can more easily undergo substitution reactions with other rare earth elements in the main phase alloy raw material to form a shell 102 with a certain thickness, thereby improving the coercive force and high-temperature external field durability of the permanent magnet 100.
[0062] In some implementations of the present application, in the composition of the core 101, 10.3≤a≤16, 12.5≤b≤18.7, 60.64≤c≤75.65, 0.2≤d≤2.5, and 0.75≤e≤1.36.
[0063] In some embodiments of the present application, in the composition of the shell 102, 24≤f+g+h≤58, 4≤g≤7, 10≤h≤16, 21.2≤i≤66.6, 0.5≤j≤1.5, 0.3≤k≤0.5, and 8≤l≤18.
[0064] In some embodiments of the present application, in the composition of the grain boundary phase 20, 36≤m+n≤55, 16≤n≤23, 15.46≤o≤51.09, 0≤p≤1.43, and 12.31≤q≤27.31.
[0065] By controlling the above parameters within the above ranges, a permanent magnet 100 having higher coercivity and better high temperature external field durability can be obtained. In addition, the Co element can increase the Curie temperature of the permanent magnet 100, reduce the coercivity temperature coefficient, and improve the temperature stability of the permanent magnet 100.
[0066] In some embodiments of the present application, in the permanent magnet 100, the M1 includes at least one of Bi, Ta, In, Pb, Cd, Tl, Sb and Ge.
[0067] In some embodiments of the present application, in the permanent magnet 100, the M2 includes at least one of Bi, Ta, In, Pb, Cd, Tl, Sb and Ge.
[0068] In some embodiments of the present application, the permanent magnet 100 is a sheet material, and the thickness of the permanent magnet 100 is in the range of 1 mm to 10 mm. Controlling the shape and size of the permanent magnet 100 is conducive to the performance of the magnetic and mechanical properties of the permanent magnet 100.
[0069] In some embodiments of the present application, the permanent magnet 100 also includes a diffusion alloy enriched layer located on its surface, and the thickness of the diffusion alloy enriched layer is in the range of 5μm-15μm. Exemplarily, the thickness of the diffusion alloy enriched layer can be 5μm, 6μm, 7μm, 8μm, 9μm, 10μm, 11μm, 12μm, 13μm, 14μm, 15μm, etc. Among them, the diffusion alloy enriched layer can be provided on one side of the upper surface or lower surface of the permanent magnet 100, or the diffusion alloy enriched layer can be provided on both sides of the upper and lower surfaces of the permanent magnet 100. In some specific embodiments, the thickness of the diffusion alloy enriched layer is in the range of 7μm-15μm. The composition of the diffusion alloy layer is the second mixture, which is formed during the preparation process of the permanent magnet 100. Whether to retain the diffusion alloy layer and the retained thickness can be selected according to actual production needs, but the appropriate thickness can ensure that the magnetic properties of the permanent magnet 100 are not affected. The removed diffusion alloy enriched layer can be reprocessed and reused as a second mixed material, further reducing the manufacturing cost.
[0070] Accordingly, the embodiment of the present application also provides a method for preparing a permanent magnet, which is suitable for preparing the above-mentioned permanent magnet 100. The preparation method comprises the following steps:
[0071] (1) uniformly mixing a first main phase alloy powder raw material, a second main phase alloy powder raw material, and a grain boundary phase alloy powder raw material to obtain a first mixed material, and then performing magnetic field orientation pressing, sintering, and a first tempering treatment to obtain a permanent magnet blank;
[0072] Wherein, the composition of the first main phase powder raw material includes R1 a’ Fe b’ Co c’ B d’, R1 includes at least one of Pr and Nd, a', b', c', d' represent weight percentages, and 25.5≤a'≤29.5, 66.4≤b'≤73.1, 0≤c'≤2, 0.9≤d'≤1.2; the composition of the second main phase alloy powder raw material is: R2 e’ Fe f’ Co g’ B h’ , R2 includes at least one of La, Ce, Sm, Gd, Ho and Y, e', f', g', h' represent weight percentages, and 27.5≤e'≤31.5, 0≤g'≤2.5, 63.85≤f'≤71.2, 0.8≤h'≤1.25; the composition of the grain boundary phase alloy powder raw material is: R3 i’ Fe j’ Co k’ M l’ , R3 includes at least one of La, Ce, Sm, Pr and Nd, M includes at least one of Zr, Ga, Cu, Sn, Al, Zn, Bi, Ta, In, Pb, Cd, Tl, Sb and Ge, i', j', k', l' represent weight percentages, and 40≤i'≤65, 5.1≤j'≤49.5, 0≤k'≤4, 10≤l'≤25;
[0073] (2) uniformly mixing the tin-plated and / or galvanized graphene and the diffusion alloy powder raw material to obtain a second mixture, and placing the second mixture on the surface of the permanent magnet blank;
[0074] (3) performing hot pressing and diffusion treatment on the permanent magnet blank with the second mixed material on the surface, or performing the hot pressing, diffusion and surface polishing treatments in sequence, to obtain the permanent magnet provided in the embodiment of the present application;
[0075] Wherein, the composition of the diffusion alloy powder raw material includes R4 x R5 y Fe z N t , R4 includes at least one of Pr and Nd, R5 includes at least one of Dy and Tb, N includes at least one of Ga, Cu, Sn, Al, Zn, Bi, Ta, In, Pb, Cd, Tl, Sb and Ge, x, y, z, t represent weight percentages, and 37.2≤x≤45.7, 23.8≤y≤32, 1.4≤z≤23, and 15.5≤t≤20.
[0076] In the above-mentioned preparation process, the first main phase alloy powder raw material and the second main phase alloy powder raw material are melted and formed under the action of high temperature to generate a main phase precursor, and at this time, the grain boundary phase alloy powder raw material is formed on the surface of the main phase precursor in whole or in part, thereby isolating and / or coating the above-mentioned main phase precursor to form a permanent magnet blank with a specific microstructure. Then, the second mixed material is placed on the surface of the permanent magnet blank, and the high-temperature treatment causes the diffusion alloy powder raw material with a relatively low melting point, the tin layer on the surface of the graphene, and the grain boundary phase alloy in the permanent magnet blank to be transformed into a molten state, so that the molten diffusion alloy raw material carries the graphene wrapped with molten tin and / or zinc along the diffusion channel provided by the molten grain boundary phase alloy, and diffuses into the permanent magnet blank together under the synergistic action of pressure and high temperature, and mixes with the grain boundary phase alloy to form a grain boundary phase precursor (that is, a mixed phase obtained by combining the grain boundary alloy and the diffusion alloy). At this time, the B element in the main phase precursor will diffuse into the grain boundary phase precursor close to the main phase precursor, and the light rare earth elements (such as La, Ce, Sm, Gd, Y, Pr, Nd) in the main phase precursor will undergo a substitution reaction with the heavy rare earth elements Tb and / or Dy in the grain boundary phase precursor, generating Dy2Fe in the grain boundary phase precursor close to the surface of the main phase precursor. 14 B and / or Tb2Fe 14 B material, thereby generating the aforementioned shell layer with a certain thickness, and finally forming a permanent magnet with relatively excellent mechanical properties, good magnetic properties and high temperature external field durability. The preparation method provided in the embodiment of the present application has simple steps, strong operability, high production efficiency, and can be applied to large-scale industrial production.
[0077] In addition, the diffusion alloy powder raw material of the above composition is selected in the present application, so that its melting point can be controlled within the range of 600°C-850°C. At the same diffusion temperature, the molten diffusion alloy of the above composition has a higher superheat and a greater diffusion potential energy than the diffusion alloy material in the prior art, thereby achieving a greater diffusion depth during the diffusion process. In addition, the diffusion alloy is completely in a molten state during the diffusion process, which can enhance its interfacial bonding force with tin-plated and / or galvanized graphene, as well as its surface bonding force with the substrate, thereby eliminating the process of adding an organic binder and debinding in the traditional process, and avoiding the degradation of the permanent magnet performance caused by residual carbon.
[0078] In some embodiments of the present application, the main phase precursor contains La and / or Ce. At this time, Pr and / or Nd in the grain boundary phase precursor will also react with it to replace the La and / or Ce elements in the main phase precursor, thereby generating Pr2Fe 14 B and / or Nd2Fe 14 B material further improves the magnetic anisotropy of the shell layer 102.
[0079] In some embodiments of the present application, the mass percentage of the grain boundary phase alloy powder raw material in the permanent magnet raw material is 3%-15%. The mass ratio of the first main phase alloy powder raw material to the second main phase alloy powder raw material is 1:(0.6-1.33). By controlling the mass ratio of the above raw materials within the above range, it can be ensured that the final permanent magnet forms a predetermined microstructure and has better performance.
[0080] In some embodiments of the present application, the mass percentage of the tinned and / or galvanized graphene in the second mixture is 0.1%-3%. In some specific embodiments, the mass percentage of the tinned and / or galvanized graphene in the second mixture is 0.1%-2.5%. Exemplarily, the mass percentage of the tinned and / or galvanized graphene in the second mixture can be 0.1%, 0.15%, 0.2%, 0.25%, 0.3%, etc. Only by controlling the content of tinned and / or galvanized graphene in the raw material can the final permanent magnet contain an appropriate amount of graphene, thereby improving the mechanical properties of the permanent magnet.
[0081] In some embodiments of the present application, in the diffusion alloy powder raw material, 38≤x≤45, 24≤y≤30, 5.1≤z≤21.5, 16≤t≤19. Controlling the above parameters within this range is conducive to obtaining a permanent magnet with better magnetic properties.
[0082] In some embodiments of the present application, in step (1), the first main phase alloy powder raw material, the second main phase alloy powder raw material and the grain boundary phase alloy powder raw material are mixed. The first and second main phase alloy raw materials and the grain boundary phase alloy raw material that have been proportioned are melted separately to obtain ingots or quick-solidified sheets of the first and second main phase alloy raw materials and ingots or quick-solidified sheets of the grain boundary phase alloy raw material, and then the ingots or quick-solidified sheets of the first and second main phase alloy raw materials and the ingots or quick-solidified sheets of the grain boundary phase alloy raw material are mixed. In some specific embodiments, after the above-mentioned ingots or quick-solidified sheets are mixed, the above-mentioned ingots or quick-solidified sheets are crushed and powdered; then a first mixture consisting of the first and second main phase alloy powder raw materials and the grain boundary phase alloy powder raw materials is obtained. In other embodiments, the first and second main phase alloy powder raw materials and the grain boundary phase alloy powder raw material can also be obtained separately, and then the above three are mixed to obtain the first mixture.
[0083] In the present application, in step (1), the above smelting method is a method well known to those skilled in the art, and the alloy obtained is a quick-setting sheet. The quick-setting thin strip is made by a quick-setting strip spinning process, and the strip spinning speed, i.e., the copper rod surface linear speed, is 1 m / s-2.5 m / s.
[0084] The above-mentioned crushing method can adopt a method well known to those skilled in the art, as long as the obtained ingot or strip can be fully crushed to obtain crushed powder. Specifically, a hydrogen crushing method can be adopted. In some specific embodiments, the conditions of the hydrogen crushing include: absorbing hydrogen at room temperature (20±5°C) for 1h-3h under a hydrogen pressure of 0.1MPa-1.5MPa, and dehydrogenating at 500°C-650°C for 4h-8h.
[0085] In some embodiments of the present application, the permanent magnet blank is a sheet with a thickness of 1-10 nm. In some specific embodiments, the thickness of the permanent magnet blank is 2 nm-7 nm. The appropriate thickness allows the second mixture to diffuse to the full depth of the permanent magnet blank, thereby ensuring that the performance of the permanent magnet obtained is good.
[0086] In some embodiments of the present application, the above-mentioned magnetic field oriented pressing molding process can adopt a process familiar to ordinary technicians in the field. Specifically, the method of magnetic field oriented pressing molding can be: orienting and pressing the first mixture in a constant magnetic field or a pulsed magnetic field of 1.5T-3.5T, and maintaining it at a static pressure of 170MPa-210MPa for 60s-150s.
[0087] The specific process of the sintering and the first tempering treatment can adopt the process well known to ordinary technicians in the field. Specifically, the conditions of the sintering can be: the sintering temperature is 1030℃-1090℃, and the sintering time is 4h-5.5h. The conditions of the first tempering treatment can be: firstly perform the primary tempering at 890℃-950℃ and keep it for 2.5h-5h, then cool it to 480℃-520℃ for secondary tempering and keep it for 3.5h-8h. Then, the block after sintering and the first tempering is machined into the required shape block to obtain the permanent magnet blank.
[0088] In some embodiments of the present application, a lubricant may be added to the alloy powder prepared above, and the lubricant may be gasoline, oleic acid, stearic acid, polyethylene glycol, sorbitan, glyceryl stearate, etc. In some specific embodiments, the amount of the lubricant added is 0.02wt.%-0.2wt.% of the total weight of the alloy powder.
[0089] The above-mentioned powder making method can be a method well known to those of ordinary skill in the art, as long as the above-mentioned crushed powder can be made into an alloy powder of the target particle size. The airflow milling method can be adopted, and an antioxidant needs to be added before the airflow milling. The antioxidant can be any special antioxidant for NdFeB, for example, it can be a special antioxidant for NdFeB purchased from Beijing Juncefeng Technology Development Co., Ltd. with a brand name of KM-01. In the present application, preferably, the amount of antioxidant added is 0.03wt.%-0.15wt.% based on the total weight of the crushed powder of the permanent magnet alloy raw material obtained by the above process. In addition, it is preferred that the hydrogen crushed powder is made into an alloy powder with an average particle size of 2μm-4.5μm by airflow milling.
[0090] In some embodiments of the present application, in step (2), the diffusion alloy powder raw material is obtained by melt quenching, which may specifically include the following steps: after the ingredients are prepared according to the definition of the present application, the resulting mixture is smelted to obtain a diffusion alloy thin strip raw material, and then subjected to hydrogen embrittlement, air flow milling and other process treatments to obtain a diffusion alloy powder raw material. In some specific embodiments, the quenching speed is 18m / s-28m / s. In other specific embodiments, the quenching speed is 19m / s-26m / s. The subsequent processing steps are similar to the processing of the first, second or grain boundary phase alloy raw materials in step (1), and will not be repeated here.
[0091] In the present application, in step (2), the method for mixing the diffusion alloy powder raw material and the tin-plated and / or galvanized graphene is a method well known to those skilled in the art, and can be achieved by mechanical stirring, ball milling and the like.
[0092] In some embodiments of the present application, the conditions for the hot pressing treatment in step (2) include: treating in a vacuum environment, with an absolute vacuum degree of 10 -3 Pa-10 -2 Pa, hot pressing temperature is 550℃-800℃, pressing pressure is 80MPa-150MPa, and holding time is 30min-150min. Among them, the direction of pressing pressure is parallel to the easy magnetization axis direction of permanent magnet blank. It should be noted that for the main phase precursor (i.e., the main phase precursor grain), the A surface perpendicular to the c-axis of the grain is a surface that is difficult to attach foreign matter, and foreign matter is more likely to be enriched on the surface parallel to the c-axis direction (i.e., the c-axis is widened). The appropriate hot pressing conditions can increase the bonding force between tinned and / or galvanized graphene and molten diffusion alloy, thereby increasing the diffusion kinetic energy of tinned and / or galvanized galvanized graphene, controlling the pressing pressure direction to be parallel to the easy magnetization direction of the permanent magnet blank, which is conducive to the subsequent diffusion process, and enables the tinned and / or galvanized graphene and diffusion alloy to be evenly distributed in the aforementioned grain boundary phase alloy to form a preset grain boundary phase precursor.
[0093] Based on the above diffusion characteristics, in some specific embodiments of the present application, the second mixed material only needs to be placed on the upper and lower surfaces of the permanent magnet blank (i.e., the surface perpendicular to the magnetic orientation direction of the permanent magnet). This can ensure that the permanent magnet can be successfully manufactured while reducing the consumption of raw materials, the difficulty of implementing the process, and the time consumption.
[0094] In the present application, the above-mentioned method of placing the second mixed material on the surface of the permanent magnet is a process well known to those skilled in the art. The process can specifically be placing the second mixed material on the surface of the permanent magnet by coating, spraying, coating, dipping, suspension adhesion, roller plating electrophoresis and the like. In some specific embodiments of the present application, the second mixed material is directly coated on the upper and lower surfaces of the permanent magnet blank, in which case the process operation is simpler and the production cost is lower.
[0095] In the present application, the second mixture is placed in sufficient quantity during the preparation process, so that a diffusion alloy-enriched layer is formed on the surface of the permanent magnet blank after diffusion treatment, and the diffusion alloy-enriched layer can be removed or thinned according to actual production needs to obtain the final permanent magnet.
[0096] In some embodiments of the present application, the average particle size of the diffusion alloy powder raw material is 30nm-85nm. In some specific embodiments, the average particle size of the diffusion alloy powder raw material is 35nm-80nm. Controlling the particle size of the diffusion alloy powder raw material within the above range can weaken the difference in particle size between it and the tin-plated and / or galvanized graphene, thereby significantly improving the uniformity of the dispersion of the tin-plated and / or galvanized graphene in the second mixture, which is beneficial to the uniform dispersion of graphene in the permanent magnet blank, thereby ensuring that the mechanical properties of the final permanent magnet are good. In addition, the diffusion alloy powder raw material has a suitable particle size, which is also beneficial to the precise control of the degree of oxidation during the preparation process.
[0097] In some embodiments of the present application, in step (2), before the permanent magnet blank is subjected to hot pressing, the permanent magnet blank is subjected to surface treatment. The surface treatment may be performed by pickling or mechanical polishing. In some specific embodiments, the pickling is performed by a 0.3wt.% nitric acid aqueous solution.
[0098] In some embodiments of the present application, the diffusion treatment conditions in step (2) include: a temperature of 600°C-1000°C, a time of 2h-12h, an absolute vacuum of 10 -5 Pa-10 -2 Controlling the diffusion treatment conditions within the above range can ensure the melting of the diffusion alloy powder raw material and the grain boundary phase alloy powder raw material, and ensure that the properties of the main phase alloy are not affected, thereby successfully completing the preparation of the permanent magnet.
[0099] In some embodiments of the present application, step (2) further includes performing a second tempering treatment on the permanent magnet blank after the diffusion treatment. The conditions of the second tempering treatment include: a temperature of 400°C-600°C, a time of 2.5h-10h, an absolute pressure of 10 -5 -10 -2 The second tempering treatment can further optimize the microstructure of the permanent magnet and improve the intrinsic coercive force of the permanent magnet.
[0100] In the present application, the tinned and / or galvanized graphene is obtained by tinning and / or galvanizing the graphene surface. The tinning treatment comprises the following steps: placing the graphene in a tinning solution, treating it at 65°C-85°C for 5min-30min, allowing the tinning solution to be deposited on the graphene surface, and then taking it out, cleaning it, and drying it.
[0101] The galvanizing treatment comprises the following steps: placing the graphene in a galvanizing solution, treating it at 10°C-35°C for 20min-90min, allowing the galvanizing solution to be deposited on the surface of the graphene, and then taking it out, cleaning it, and drying it.
[0102] The chemical tin plating solution comprises: 45g / L-50g / L stannous chloride, 20g / L-25g / L thiourea, 32g / L-35g / L tartaric acid, 27g / L-30g / L citric acid, 23g / L-28g / L sodium hypophosphite, 2.5g / L-3g / L hydroquinone, 20mL / L-25mL / L polyethylene glycol, and 80mL / L-100mL / L hydrochloric acid; the pH value of the chemical tin plating and / or zinc plating solution is 0.6-1.2; wherein the molecular weight of the polyethylene glycol is 600.
[0103] The zinc plating solution comprises: 8g / L-15g / L zinc oxide, 100g / L-150g / L sodium hydroxide, 8g / L-15g / L sodium cyanide, 4mL / L-6mL / L DE-81 additive (electroplating grade), and 4mL / L-6mL / L ZBD-81 brightener (electroplating grade).
[0104] The embodiment of the present application also provides a permanent magnet drive motor, which has the permanent magnet provided by the embodiment of the present application. The permanent magnet drive motor has a long service life and better comprehensive performance, can be applied to new energy vehicles and other fields, and can be used to provide new energy vehicles with high power density, high torque density, high controllability and high efficiency.
[0105] The technical solution of the present application is described in detail below in conjunction with specific embodiments.
[0106] Example 1
[0107] The formula is Nd 26 Fe71.5 Co 1.5 The raw material of B1 was subjected to a belt spinning process at a copper roller surface linear speed of 1.1 m / s, and the resulting belt spinning sheet was subjected to hydrogen absorption for 1.5 h at 22° C. under a hydrogen pressure of 0.12 MPa, and then dehydrogenated at 510° C. for 4.2 h, thereby obtaining hydrogen powder. Then, 100 parts by weight of the hydrogen powder was mixed evenly with 0.035 parts by weight of a special antioxidant for NdFeB (purchased from Beijing Juncefeng Technology Development Co., Ltd., brand KM-01), and then ground by a jet mill to obtain a powder with an average particle size of 2.1 μm, thereby obtaining the first main phase alloy powder raw material.
[0108] The formula is La3Ce 25 Fe 69.1 Co2B 0.9 The raw material was subjected to belt spinning at a copper roller surface linear speed of 1.15 m / s, and the resulting belt spinning sheet was subjected to hydrogen absorption for 1.6 h at 23° C. under a hydrogen pressure of 0.13 MPa, and then dehydrogenated at 515° C. for 4.3 h, thereby obtaining hydrogen powder. Then, 100 parts by weight of the hydrogen powder was evenly mixed with 0.04 parts by weight of a special antioxidant for NdFeB (purchased from Beijing Juncefeng Technology Development Co., Ltd., brand KM-01), and then ground by a jet mill to obtain a powder with an average particle size of 2.2 μm, thereby obtaining a second main phase alloy powder raw material.
[0109] The formula is Pr 63 Fe 13 Co1Zr7Cu 10 The Al6 raw material was subjected to a belt-spinning treatment at a copper roller surface linear speed of 1.2 m / s, and the resulting belt-spinning sheet was subjected to hydrogen absorption for 1.7 h at 24° C. under a hydrogen pressure of 0.14 MPa, and then dehydrogenated at 520° C. for 4.4 h, thereby obtaining hydrogen powder. Then, 100 parts by weight of the hydrogen powder was mixed evenly with 0.045 parts by weight of a special antioxidant for NdFeB (purchased from Beijing Juncefeng Technology Development Co., Ltd., brand KM-01), and then ground by a jet mill to obtain a powder with an average particle size of 2.3 μm, thereby obtaining a grain boundary phase alloy powder raw material.
[0110] The first and second main phase alloy powder raw materials are uniformly mixed, and the weight of the first main phase alloy powder raw material is 1.22 times that of the second main phase alloy powder raw material. The first and second main phase alloy mixed powder raw materials and the grain boundary phase alloy powder raw material are uniformly mixed to obtain a first mixture. The mass percentage of the grain boundary phase alloy powder raw material in the first mixture is 10%. A certain amount of gasoline (YS-06 brand purchased from Haotian Chemical Company) is added to the first mixture, wherein the amount of gasoline is 0.03% of the first mixture.
[0111] The first mixture containing gasoline is molded in a constant magnetic field of 1.6T, and then kept at an isostatic pressure of 175MPa for 62s; then sintered at 1035℃ for 4.2h; and tempered at 855℃ for 2.5h; then tempered at 482℃ for 3.5h, and machined to finally obtain a permanent magnet blank with a size of 17mm long × 14mm wide × 2mm thick.
[0112] The formula is Pr 21 Dy 24 Fe 39 Ga 10 The Al2Zn4 raw material was melted at 600°C and quenched at a speed of 19 m / s to obtain a diffusion alloy ribbon, which was then ground by ball milling to obtain a diffusion alloy powder raw material with an average particle size of 35 nm.
[0113] The graphene was ultrasonically dispersed in an ethanol solution at a power of 1000w for 50min and dried in an environment of 125°C for 20min. The ultrasonically dispersed graphene was tinned in 45g / L stannous chloride, 20g / L thiourea, 32g / L tartaric acid, 27g / L citric acid, 23g / L sodium hypophosphite, 2.5g / L hydroquinone, 20mL / L polyethylene glycol molecular weight 600, 80mL / L hydrochloric acid chemical tin plating solution, the pH value was adjusted to 0.6, and the graphene was deposited at 65°C for 10min, then taken out, cleaned and dried. Tin-plated graphene with an average particle size of 15nm was obtained. Then it was evenly mixed with the diffusion alloy powder to obtain a second mixture. In the second mixture, the mass percentage of tin-plated graphene is 0.5%.
[0114] The permanent magnet blank was sandblasted, and then the second mixture was evenly coated on the upper and lower surfaces of the permanent magnet blank and placed in a hot pressing mold. The hot pressing mold was placed in a vacuum hot pressing furnace at a vacuum degree of 8×10 -2 Pa, the pressing temperature was 550 ° C, and the hot pressing was carried out under a pressing pressure of 80 MPa and the pressure was maintained for 30 minutes. The direction of the pressing pressure was parallel to the easy magnetization axis of the permanent magnet blank. -2 Pa, diffusion temperature was 850 ° C, diffusion treatment was carried out for 8 hours. Then the first tempering treatment was carried out. The conditions of the first tempering treatment included: temperature 410 ° C, time 2.5 hours, vacuum degree 4×10 -2 Pa. The samples obtained above are then polished.
[0115] The final size of the permanent magnet A1 is 17mm long, 14mm wide and 2mm thick, and the composition of its core is Nd 16 LqCy 7.5 Fe 70.55 Co 0.2B 0.75 , the shell composition is Nd 44 LqCy 10 Fe 33.2 Co 0.5 B 0.3 Zr3Cu1Al1Ga2Zn1, the composition of the grain boundary phase is Pr 20 Dy 16 Fe 51.1 Co 0.5 Zr3Cu2Al1Ga 4.2 Zn 2.2 The mass percentage of tin-coated graphene in the shell layer is 0.05%, and the mass percentage of tin-coated graphene in the grain boundary phase is 0.09%. The rare earth content in the shell layer is 2.04 times that in the core layer, the thickness of the shell layer is 1.2 μm-3.3 μm, and the mass percentage of the grain boundary phase in the permanent magnet is 20%.
[0116] Example 2
[0117] The difference from Example 1 is that the composition of the first main phase alloy powder raw material is Nd 27 Fe 71.05 Co1B 0.95 The composition of the second main phase alloy powder raw material is Sm5Ce 26 Fe 67.9 B 1.1 The composition of the grain boundary phase alloy powder raw material is Nd 41 Fe 45 Co3Ga3Bi2Zn6, the composition of the diffusion alloy powder raw material is Nd8Tb 30 Fe 39 Cu 13 Bi3In3, and the mass of the first main phase alloy is 0.66 times that of the second main phase alloy, the average particle size of the tin-plated graphene is 23nm, and the mass percentage of the tin-plated graphene in the second mixture is 2.5%.
[0118] The permanent magnet A2 with a length of 17 mm, a width of 14 mm, and a thickness of 7 mm was obtained, and the composition of its core was Nd 10.3 Sm 14 Ce 4.7 Fe 67.14 Co 2.5 B 1.36 , the shell composition is Nd 17.26 Sm 1.02 Ce 6.09 Tb 16.24 Fe 39.09 Co 1.52 B 0.51 Ga 7.1 Bi 2.03 Zn3.04 Cu 5.08 In 1.02 , the grain boundary phase composition is Nd 32.73 Tb 23.52 Fe 15.43 Co 1.23 Ga 5.11 Bi 2.05 Zn 10.22 Cu 5.11 In 4.6 The mass percentage of tin-coated graphene in the shell is 1.5%, and the mass percentage of tin-coated graphene in the grain boundary phase is 2.23%. The rare earth content in the shell is 1.38 times that in the core, and the thickness of the shell is 1.5-3.2 μm. The mass percentage of the grain boundary phase in the permanent magnet is 40%.
[0119] Example 3
[0120] The difference from Example 2 is that the mass percentage of each element in the first main phase alloy and the second main phase alloy powder raw materials is finely adjusted, and the mass of the first main phase alloy powder raw materials is controlled to be 1.32 times the mass of the second main phase alloy powder. The permanent magnet A3 is obtained, and the composition of its core is Nd 14.89 Sm 13.15 Ce 0.28 Fe 67.85 Co 2.5 B 1.33 , the shell composition is Nd 22.03 Sm 0.15 Ce 5.99 Tb 11.75 Fe 39.74 Co 1.71 B 0.48 Ga 7.13 Bi 1.94 Zn 3.08 Cu 5.06 In 0.94 , the grain boundary phase composition is Nd 32.84 Tb 23.42 Fe 15.62 Co 1.25 Ga 5.13 Bi 1.95 Zn 10.26 Cu5In 4.53 The mass percentage of tin-coated graphene in the shell is 1.48%, and the mass percentage of tin-coated graphene in the grain boundary phase is 2.21%. The rare earth content in the shell is 1.39 times that in the core, and the thickness of the shell is 1.5-2.5 μm. The mass percentage of the grain boundary phase in the permanent magnet is 38%.
[0121] Example 4
[0122] The difference from Example 2 is that the mass percentage of each element in the first main phase alloy and the second main phase alloy powder raw materials is finely adjusted, and the mass of the first main phase alloy powder raw materials is controlled to be 1.32 times the mass of the second main phase alloy powder, and the mass percentage of the grain boundary phase alloy powder raw materials in the first mixed material is 5%. The permanent magnet A4 is obtained, and the composition of its core is Nd 14.62 Sm 13.2 Ce 0.54 Fe 67.7 Co 2.6 B 1.34 , the shell composition is Nd 13.12 Sm 0.2 Ce 6.29 Tb 12.02 Fe 47.51 Co 1.66 B 0.49 Ga7.0 78 Bi 2.19 Zn 2.99 Cu 5.32 In 1.14 , the grain boundary phase composition is Nd 32.49 Tb 23.72 Fe 15.04 Co 1.2 Ga 5.08 Bi 2.21 Zn 10.17 Cu 5.22 In 4.63 The mass percentage of tin-coated graphene in the shell is 1.52%, and the mass percentage of tin-coated graphene in the grain boundary phase is 2.25%. The rare earth content in the shell is 1.1 times that in the core, and the thickness of the shell is 1.1-2.3 μm. The mass percentage of the grain boundary phase in the permanent magnet is 36%.
[0123] Example 5
[0124] The difference from Example 1 is that the composition of the first main phase alloy powder raw material is Pr 29 Fe 69.85 B 1.15 The composition of the second main phase alloy powder raw material is Gd 10 Ce 20 Fe 68 Co1B1, the composition of the grain boundary phase alloy powder raw material is Ce 45 Fe 33.5 Co 1.5 Sn8Ta4Pb8, the composition of the diffusion alloy powder raw material is Pr 14 Tb 26 Fe 39Sn7Ta6Cd5. The mass of the first main phase alloy is 0.72 times the mass of the second main phase alloy, and the mass percentage of the grain boundary phase alloy in the first mixture is 10%. The average particle size of the tin-plated graphene is 16nm, and its mass percentage in the second mixture is 2%.
[0125] The permanent magnet A5 is obtained, and its core composition is Pr 12 oeLh 5.5 Fe 71.5 Co2B1, shell composition is Pr 25.25 G 4.04 Ce 1.01 Tb 12.12 Fe 41.02 Co 1.01 B 0.4 Sn 5.05 Ta 4.04 Pb 3.03 Cd 3.03 , the grain boundary phase composition is Pr 12.1 Tb 18.15 Ce 10.08 Fe 43.54 Co 1.01 Sn 3.02 Ta 7.06 Pb 2.02 Cd 3.02 The mass percentage of tin-coated graphene in the shell layer is 1%, and the mass percentage of tin-coated graphene in the grain boundary phase is 0.8%. The rare earth content in the shell layer is 1.65 times the rare earth content in the core of the main phase, and the thickness of the shell layer is 1.6μm-2.7μm. The mass percentage of the grain boundary phase in the permanent magnet is 36%.
[0126] Example 6
[0127] The difference from Example 1 is that the composition of the first main phase alloy powder raw material is Pr 25.5 Fe 71.3 Co2B 1.2 The composition of the second main phase alloy powder raw material is Ho 8.5 Ce 19 Fe 69.5 Co 2.2 B 0.8 The composition of the grain boundary phase alloy powder raw material is La 40 Fe 50 Sb7Ce3, the composition of the diffusion alloy powder raw material is Nd 13.4 Tb 23.8 Fe 38.8 Pb 10Tl2Ge5Sb3. The mass of the first main phase alloy is 0.613 times the mass of the second main phase alloy, and the mass percentage of the grain boundary phase alloy in the first mixture is 4%. The average particle size of the tin-plated graphene is 25nm, and its mass percentage in the second mixture is 0.2%.
[0128] The permanent magnet A6 is obtained, and its core composition is Pr 10.2 Ho 10 Ce 8.9 Fe 70.18 B 0.72 The shell composition is Pr 11 Ho 1.7 Ce2Dy9Fe 68.68 B 0.22 Sb2Ge3Pb1Tl 1.4 , the grain boundary phase composition is La4Nd6Tb 24.02 Fe 53.68 Sb4Ge2Pb3Tl 3.3 The mass percentage of tin-coated graphene in the shell layer is 0.04%, and the mass percentage of tin-coated graphene in the grain boundary phase is 0.07%. The rare earth content in the shell layer is 1.12 times the rare earth content in the core of the main phase, and the thickness of the shell layer is 0.1μm-0.8μm. The mass percentage of the grain boundary phase in the permanent magnet is 20%.
[0129] Example 7
[0130] The difference from Example 1 is that the composition of the first main phase alloy powder raw material is Pr 25.5 Fe 71.3 Co2B 1.2 The composition of the second main phase alloy powder raw material is Y 4.5 Ce 27 Fe 67.3 B 1.2 The composition of the grain boundary phase alloy powder raw material is Sm 64 Fe 8.5 Co 3.5 In 11 Cd9Tl4, the composition of the diffusion alloy powder raw material is Nd 13.7 Tb 32 Fe 38.8 Pb 8.5 Tl4Ge2Sb1. The mass of the first main phase alloy is 0.64 times the mass of the second main phase alloy, and the mass percentage of the grain boundary phase alloy in the first mixture is 15%. The average particle size of the tin-plated graphene is 26nm, and its mass percentage in the second mixture is 2.5%.
[0131] The permanent magnet A7 is obtained, and its core composition is Pr 16.2 Y6C6.4 Fe 67.39 Co 2.6 B 1.41 The shell composition is Pr 34.4 1Y 3.66 Ce 4.06 Tb 17.07 Fe 19.21 Co 2.03 B 0.57 In 5.79 Cd 4.06 Tl 2.03 Pb 3.05 Ge 2.03 Sb 2.03 , the grain boundary phase composition is Sm 21.48 Nd 20.97 Tb 15.34 Fe 13.47 Co 1.43 In 5.12 Cd 4.09 Tl 3.07 Pb 8.18 Ge 2.05 Sb 4.8 The mass percentage of tin-coated graphene in the shell is 1.58%, and the mass percentage of tin-coated graphene in the grain boundary phase is 2.25%. The rare earth content in the shell is 2.62 times that in the core of the main phase, and the thickness of the shell is 7.4μm-8.5μm. The mass percentage of the grain boundary phase in the permanent magnet is 21%.
[0132] Example 8
[0133] The difference from Example 7 is that the mass percentage of each element in the first main phase alloy and the second main phase alloy powder raw materials is finely adjusted, and the mass of the first main phase alloy is controlled to be 0.7 times the mass of the second main phase alloy, and the mass percentage of the grain boundary phase alloy in the first mixture is 15%. The permanent magnet A8 is obtained, and the composition of the core of A8 is Pr 10.3 Y 14 Ce 4.7 Fe 67.14 Co 2.5 B 1.36 The shell composition is Pr 34.41 Y 3.66 Ce 4.06 Tb 17.07 Fe 19.21 Co 2.03 B 0.57 In 5.79 Cd 4.06 Tl 2.03 Pb 3.05 Ge 2.03 Sb 2.03 , the grain boundary phase composition is Sm21.48 Nd 20.97 Tb 15.34 Fe 13.45 Co 1.43 In 5.12 Cd 4.09 Tl 3.07 Pb 8.18 Ge 2.05 Sb 4.8 .
[0134] Example 9
[0135] The difference from Example 7 is that the mass percentage of each element in the first main phase alloy and the second main phase alloy powder raw materials is slightly adjusted, and the mass of the first main phase alloy is controlled to be 0.64 times the mass of the second main phase alloy, and the mass percentage of the grain boundary phase alloy in the first mixture is 15%. The permanent magnet A9 is obtained, and the composition of the core of A9 is Pr 16.2 Y6C 6.4 Fe 67.39 Co 2.6 B 1.41 The shell composition is Pr 1.02 Y 1.02 Ce 6.09 Tb 16.24 Fe 55.32 Co 1.52 B 0.50 In 7.11 Cd 2.03 Tl 3.05 Pb 2.95 Ge 2.13 Sb 1.02 , the grain boundary phase composition is Sm 21.48 Nd 20.97 Tb 15.34 Fe 13.45 Co 1.43 In 5.12 Cd 4.09 Tl 3.07 Pb 8.18 Ge 2.05 Sb 4.8 .
[0136] Example 10
[0137] The difference from Example 7 is that the mass percentage of each element in the grain boundary phase alloy powder raw material is finely adjusted, and the mass of the first main phase alloy is controlled to be 0.64 times the mass of the second main phase alloy, and the mass percentage of the grain boundary phase alloy in the first mixed material is 22.9%. The permanent magnet A10 is obtained, and the composition of the core of A10 is Pr 16.2 Y6C 6.4 Fe 67.39 Co 2.6 B1.41 The shell composition is Pr 34.41 Y 3.66 Ce 4.06 Tb 17.07 Fe 19.21 Co 2.03 B 0.57 In 5.79 Cd 4.06 Tl 2.03 Pb 3.05 Ge 2.03 Sb 2.03 , the composition of the grain boundary phase is Sm 32.73 Nd 15.08 Tb 8.44 Fe 15.43 Co 1.23 In 5.11 Cd 2.05 Tl 2.57 Pb 7.65 Ge 5.11 Sb 4.6 .
[0138] Embodiment 11
[0139] The difference from Example 1 is that the mass percentage of tin-plated graphene in the second mixture is controlled to be 0.08%, the mass percentage of tin-plated graphene in the shell layer is 0.02%, and the mass percentage of tin-plated graphene in the grain boundary phase is 0.05%.
[0140] Example 12
[0141] The difference from Example 1 is that in Example 12, galvanized graphene is added to obtain permanent magnet A12.
[0142] Example 13
[0143] The difference from Example 1 is that the upper surface of the permanent magnet A13 obtained further has a diffusion alloy enriched layer with a thickness of 5 μm.
[0144] Embodiment 14
[0145] The difference from Example 1 is that the length of the permanent magnet A14 obtained is 17 mm, the width is 14 mm, and the thickness is 10 mm.
[0146] Embodiment 15
[0147] The difference from Example 1 is that in the hot pressing process of step (2), the absolute vacuum degree is 10 -3 Pa, the pressing pressure is 150 MPa, the temperature is 800°C, and the holding time is 150 min. The permanent magnet A15 is obtained.
[0148] In order to highlight the beneficial effects of the embodiments of the present application, the following comparative examples are provided.
[0149] Comparative Example 1
[0150] The difference from Example 1 is that the formula is Pr 21 Dy 24 Fe 39 Ga 10 Al2Zn4 diffusion alloy powder is coated on the upper and lower surfaces of the rare earth permanent magnet blank (i.e., without zinc-plated and / or tin-plated graphene), and then subjected to diffusion heat treatment to obtain permanent magnet CA1, the core of which is composed of Nd 15.74 La 5.03 Ce 7.75 Fe 70.54 Co 0.2 B 0.74 , the shell composition is Nd 43.74 La 2.03 Ce 2.25 Dy 10 Fe 33.23 Co 0.5 B 0.2 Zr3Cu1Al1Ga2Zn1, the composition of the grain boundary phase is Pr 20 Dy 16 Fe 51.1 Co 0.5 Zr3Cu2Al1Ga 4.2 Zn 2.2 The rare earth content in the shell is 2.03 times that in the core, and the thickness of the shell is 1 μm-3 μm. The mass percentage of the grain boundary phase in the permanent magnet is 20%.
[0151] Comparative Example 2
[0152] The difference from Example 1 is that no diffusion alloy is added during the preparation process, and only a sufficient amount of tin-plated graphene is coated on the upper and lower surfaces of the permanent magnet blank.
[0153] The permanent magnet CA2 was obtained, and the main phase composition of the alloy was Nd 15.87 La 5.02 Ce 7.63 Fe 70.54 Co 0.2 B 0.74 , the composition of the main phase shell is Nd 10.79 Pr 20.16 La 3.41 Ce 5.19 Fe 52.13 Co 0.46 B 0.5 Zr 2.24 Cu 3.2 Al 1.92 C 0.0016 , the grain boundary phase composition is Pr63 Fe 13 Co1Zr7Cu 10 A l6 The mass percentage of tin-coated graphene in the grain boundary phase is 0.005%, and the mass percentage of tin-coated graphene in the shell layer is 0.0016%. The rare earth content in the shell layer of the main phase is 1.01 times the rare earth content in the core of the main phase, and the thickness of the shell layer is 1μm-2.5μm. Based on the total weight of the main phase and the grain boundary phase, the mass content of the grain boundary phase is 18%.
[0154] Comparative Example 3
[0155] The difference from Example 1 is that the permanent magnet blank prepared in Example 1 is directly used as the final permanent magnet product CA3. That is, the raw materials of CA3 do not include diffusion alloy and zinc / tin-plated graphene, and its preparation process does not involve the hot pressing treatment and diffusion treatment in step (3) of the above-mentioned permanent magnet preparation method.
[0156] Comparative Example 4
[0157] The difference from Example 1 is that a single alloy raw material is prepared into a permanent magnet blank, and its composition is Nd 12.58 La 1.19 Ce 9.9 Pr 7.56 Fe 63.53 Co 1.64 B 0.84 Zr 0.84 Cu 1.2 Al 0.72 , a permanent magnet CA4 is obtained. That is, the raw material of CA4 is only a single alloy, and is not divided into the first main phase alloy powder and the second main phase alloy powder for processing. The raw material does not include diffusion alloy and zinc / tin-plated graphene, and the preparation process does not involve the hot pressing treatment and diffusion treatment in step (3) of the above-mentioned permanent magnet preparation method.
[0158] Comparative Example 5
[0159] The difference from Example 1 is that the formula is Pr 9.6 Nd 29.3 Dy 10 Fe 15.5 Co 16.5 B 0.96 A l5.5 Cu 3.2 Zr 2.4 The alloy raw material of Ga7 is used as the raw material of grain boundary phase alloy powder to produce permanent magnet CA5. That is, the raw material of grain boundary phase alloy powder of CA5 also contains Dy element, and the content of Co element is too high. Other raw materials, quality and process conditions are consistent with those in Example 1.
[0160] The performance tests were performed on the permanent magnets obtained in the above embodiments and comparative examples:
[0161] (1) Remanence and coercivity test: The permanent magnets prepared in the above embodiments and comparative examples were tested according to the GB / T3217-1992 test standard. The remanence (Br) and intrinsic coercivity (Hcj) of the permanent magnets A1-A15 and CA1-CA5 were tested at 22°C using NIM-10000H of the China National Institute of Metrology. The test results are summarized in Table 1.
[0162] (2) High temperature external field durability test: Specifically, a 7kOe reverse magnetic field was applied to the permanent magnet, kept at 180°C for 100 h, and then cooled to 22°C. The irreversible loss of magnetic flux of each sample was tested using a fluxmeter. irr .
[0163] (3) Bending strength test: The bending strength of each permanent magnet was tested according to the national standard GBT228.1-2010. The test results are summarized in Table 1.
[0164] (4) Morphology test: The permanent magnet A1 prepared in Example 1 was subjected to SEM test. Specifically, the permanent magnet A1 was cut, and the cut surface was subjected to appropriate surface treatment, and its microstructure was observed under an electron scanning microscope.
[0165] Table 1 Summary of performance test results of permanent magnets prepared in various embodiments and comparative examples
[0166]
[0167] From the SEM photo of permanent magnet A1, it can be clearly seen that its main phase is divided into core ( Figure 2 1) and shell ( Figure 2 3) and the grain boundary phase is isolated ( Figure 2 2) and / or encapsulate the adjacent main phase.
[0168] In addition, it can be seen from the data in Table 1 that the permanent magnets A1-A15 obtained in the embodiment have excellent bending resistance, good magnetic properties and high-temperature external field durability. The coercive force, bending performance and high-temperature external field durability of the permanent magnets CA1-CA5 obtained in the comparative example are significantly worse than those of A1-A15. Among them, although CA2 contains tin-plated graphene, the tin-plated graphene is directly covered on the surface of the permanent magnet blank during its preparation process, which makes it difficult for the tin-plated graphene to enter the interior of the permanent magnet blank, thereby causing the tin-plated graphene content in CA2 to be too low, and the improvement of its bending performance is limited. CA3 and CA4 do not have a shell-core structure, nor do they contain tin-plated or zinc-plated graphene, resulting in poor performance. The Co element content in the grain boundary phase raw material used in comparative example 5 is too high and contains Dy elements, which affects the content of other elements, resulting in poor intrinsic coercive force, bending performance and high-temperature external field durability of CA5.
[0169] The above is an exemplary embodiment of the present application. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made thereto without departing from the principles of the present application. These improvements and modifications are also considered to be within the scope of protection of the present application.
Claims
1. A permanent magnet, characterized in that: The permanent magnet comprises a main phase and a grain boundary phase, wherein the grain boundary phase isolates and / or covers the adjacent main phase; the main phase comprises a shell layer and a core layer, and tin-plated and / or zinc-plated graphene is dispersed in the grain boundary phase and the shell layer; The core consists of RL1 a RH1 b Fe c Co d B e , RL1 includes at least one of Pr and Nd, RH1 includes at least one of La, Ce, Sm, Gd, Ho and Y, wherein a, b, c, d, e represent weight percentages, 10.2≤a≤16.2, 12.4≤b≤18.9, 59.99≤c≤76.18, 0≤d≤2.6, 0.72≤e≤1.41; The shell layer comprises RL2 f RH2 g RH3 h Fe i Co j B k M1 l , RL2 includes at least one of Pr and Nd, RH2 includes at least one of La, Ce, Sm, Gd, Ho and Y, RH3 includes at least one of Dy and Tb, and M1 includes at least one of Zr, Ga, Cu, Sn, Al, Zn, Bi, Ta, In, Pb, Cd, Tl, Sb and Ge, wherein f, g, h, i, j, k, l represent weight percentages, 23.71≤f+g+h≤59.2, 3.7≤g≤7.72, 9≤h≤17.07, f>0, 18.33≤i≤68.17, 0≤j≤2, 0.22≤k≤0.57, 7.4≤l≤19; The composition of the grain boundary phase includes RL3 m RH4 n Fe o Co p M2 q , RL3 includes at least one of La, Ce, Sm, Pr and Nd, RH4 includes at least one of Dy and Tb, and M2 includes at least one of Zr, Ga, Cu, Sn, Al, Zn, Bi, Ta, In, Pb, Cd, Tl, Sb and Ge, wherein m, n, o, p, q represent weight percentages, and 34≤m+n≤57.8, 15.2≤n≤24.55, 12.56≤o≤53.19, 0≤p≤1.43, and 12.31≤q≤27.
31.
2. The permanent magnet according to claim 1, characterized in that The mass percentage of the tin-plated and / or galvanized graphene in the shell layer is 0.04%-1.58%, and the mass percentage of the tin-plated and / or galvanized graphene in the grain boundary phase is 0.07%-2.25%.
3. The permanent magnet according to claim 1, characterized in that In the composition of the inner core, 10.3≤a≤16, 12.5≤b≤18.7, 60.64≤c≤75.65, 0.2≤d≤2.5, and 0.75≤e≤1.
36.
4. The permanent magnet according to claim 1, characterized in that In the composition of the shell layer, 24≤f+g+h≤58, 4≤g≤7, 10≤h≤16, 21.2≤i≤66.6, 0.5≤j≤1.5, 0.3≤k≤0.5, and 8≤l≤18.
5. The permanent magnet according to claim 1, characterized in that In the composition of the grain boundary phase, 36≤m+n≤55, 16≤n≤23, 15.46≤o≤51.09, 0≤p≤1.43, and 12.31≤q≤27.
31.
6. The permanent magnet according to claim 1, characterized in that The mass percentage of the main phase in the permanent magnet is in the range of 60%-80%; the mass percentage of the grain boundary phase in the permanent magnet is in the range of 20%-40%.
7. The permanent magnet according to claim 1, characterized in that The thickness of the shell layer is in the range of 0.1 μm to 8.5 μm.
8. The permanent magnet according to claim 1, characterized in that The ratio of the sum of the masses of the RL2, the RH2 and the RH3 to the sum of the masses of the RL1 and the RH1 is 1:(1.01-2.62).
9. The permanent magnet according to claim 1, characterized in that: The average particle size of the tin-plated and / or zinc-plated graphene is 10nm-25nm.
10. The permanent magnet according to claim 1, characterized in that The permanent magnet is a sheet material, and the thickness of the permanent magnet is 1 mm-10 mm.
11. The permanent magnet according to any one of claims 1 to 10, characterized in that: The surface of the permanent magnet also has a diffusion alloy enriched layer, the thickness of the diffusion alloy enriched layer is 5μm-15μm; the composition of the diffusion alloy layer includes R4 x R5 y Fe z N t , R4 includes at least one of Pr and Nd, R5 includes at least one of Dy and Tb, N includes at least one of Ga, Cu, Sn, Al, Zn, Bi, Ta, In, Pb, Cd, Tl, Sb and Ge, x, y, z, t represent weight percentages, and 37.2≤x≤45.7, 23.8≤y≤32, 1.4≤z≤23, and 15.5≤t≤20.
12. A method for preparing a permanent magnet, characterized in that: The preparation method comprises the following steps: (1) uniformly mixing a first main phase alloy powder raw material, a second main phase alloy powder raw material, and a grain boundary phase alloy powder raw material to obtain a first mixed material, and then performing magnetic field orientation pressing, sintering, and a first tempering treatment to obtain a permanent magnet blank; Wherein, the composition of the first main phase powder raw material includes R1 a’ Fe b’ Co c’ B d’ , R1 includes at least one of Pr and Nd, a', b', c', d' represent weight percentages, and 25.5≤a'≤29.5, 66.4≤b'≤73.1, 0≤c'≤2, 0.9≤d'≤1.2; the composition of the second main phase alloy powder raw material is: R2 e’ Fe f’ Co g’ B h’ , R2 includes at least one of La, Ce, Sm, Gd, Ho and Y, e', f', g', h' represent weight percentages, and 27.5≤e'≤31.5, 0≤g'≤2.5, 63.85≤f'≤71.2, 0.8≤h'≤1.25; the composition of the grain boundary phase alloy powder raw material is: R3 i’ Fe j’ Co k’ M l’ , R3 includes at least one of La, Ce, Sm, Pr and Nd, M includes at least one of Zr, Ga, Cu, Sn, Al, Zn, Bi, Ta, In, Pb, Cd, Tl, Sb and Ge, i', j', k', l' represent weight percentages, and 40≤i'≤65, 5.1≤j'≤49.5, 0≤k'≤4, 10≤l'≤25; (2) uniformly mixing the tin-plated and / or galvanized graphene and the diffusion alloy powder raw material to obtain a second mixture, and placing the second mixture on the surface of the permanent magnet blank; (3) sequentially performing hot pressing and diffusion treatment on the permanent magnet blank with the second mixed material on the surface, or sequentially performing the hot pressing, diffusion and surface polishing treatments to obtain the permanent magnet according to any one of claims 1 to 11; Wherein, the composition of the diffusion alloy powder raw material includes R4 x R5 y Fe z N t , R4 includes at least one of Pr and Nd, R5 includes at least one of Dy and Tb, N includes at least one of Ga, Cu, Sn, Al, Zn, Bi, Ta, In, Pb, Cd, Tl, Sb and Ge, x, y, z, t represent weight percentages, and 37.2≤x≤45.7, 23.8≤y≤32, 1.4≤z≤23, and 15.5≤t≤20.
13. The preparation method according to claim 12, characterized in that: In the diffusion alloy powder raw material, 38≤x≤45, 24≤y≤30, 5.1≤z≤21.5, and 16≤t≤19.
14. The preparation method according to claim 12, characterized in that: The mass percentage of the grain boundary phase alloy powder raw material in the permanent magnet raw material is 3%-15%; the mass ratio of the first main phase alloy powder raw material to the second main phase alloy powder raw material is 1:(0.6-1.33).
15. The preparation method according to claim 12, characterized in that: The mass percentage of the tin-plated and / or galvanized graphene in the second mixture is 0.1%-3%.
16. The preparation method according to claim 12, characterized in that: The conditions of the heat pressing treatment include: performing the treatment under vacuum, with an absolute vacuum degree of 10 -3 Pa-10 -2 Pa, the pressing pressure is 80MPa-150MPa, the temperature is 550℃-800℃, and the holding time is 30min-150min.
17. The method according to claim 12, characterized in that The conditions of the diffusion treatment process include: temperature of 600°C-1000°C, time of 2h-12h, absolute vacuum of 10 -5 Pa-10 -2 Pa.
18. A permanent magnet drive motor, characterized in that: The permanent magnet drive motor has a permanent magnet as described in any one of claims 1-11.
Citation Information
Patent Citations
Method for preparing crystal boundary nano-composite intensified neodymium iron boron magnet
CN103646777A
High-strength and high-toughness permanent magnet and preparation method thereof
CN107452456A
High-temperature-resistant and multi-principal-phase high-abundance rare-earth permanent magnet material and preparation method thereof
CN108766703A
High-coercivity rare earth permanent magnet and preparation method thereof
CN112071543A
Rare earth permanent magnet material and preparation method thereof
CN113838620A