Surface treated steel plate
By forming a Ni-W coating with a specific structure on the surface of the base steel plate, the problem of insufficient resistance of existing steel plates to LIB electrolyte in lithium-ion batteries is solved, achieving higher resistance to LIB electrolyte and improved performance of lithium-ion batteries.
Patent Information
- Application Number
- CN202280026347.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2021-04-08
- Filing Date
- 2022-03-30
- Publication Date
- 2026-11-17
- Estimated Expiration
- 2042-03-30
AI Technical Summary
Existing surface-treated steel plates lack sufficient resistance to LIB electrolyte in lithium-ion secondary batteries, failing to meet the requirements of large battery tanks. In particular, alternative materials such as aluminum and SUS plates are insufficient in terms of heat resistance and LIB electrolyte resistance.
A coating containing Ni and W is formed on the surface of the base steel plate. The W concentration of the coating is distributed as a high concentration layer near the surface and a low concentration layer inside. Specifically, the ratio of W concentration to Ni concentration in the high concentration layer is 2.0 to 20.0 atomic%, and the ratio of the low concentration layer is less than 0.7 times that of the high concentration layer. The amount of Ni attached in the coating is 2.6 to 35.6 g/m2.
It significantly improves the resistance of surface-treated steel plates to LIB electrolyte, making them suitable for large lithium-ion battery canisters. It enhances the heat resistance and strength of lithium-ion batteries, reduces weight, and improves the volumetric energy density and lifespan of the batteries.
Smart Images

Figure CN117098876B_ABST
Abstract
Description
Technical Field
[0001] This invention relates to a surface-treated steel sheet.
[0002] This application claims priority based on Japanese Patent Application No. 2021-065675 filed on April 8, 2021, the contents of which are incorporated herein by reference. Background Technology
[0003] Lithium-ion batteries (LIBs) are widely used as power sources for electric vehicles, etc. Lithium-ion battery cans are available in cylindrical and prismatic types. Cylindrical battery cans are used with the can connected directly to the negative electrode. Therefore, Ni-plated steel and SUS are used as materials for cylindrical lithium-ion battery cans. Aluminum, when connected to the negative electrode, will embed lithium (Li), so it cannot be used as a can material. On the other hand, prismatic cans are used in neutral environments, so aluminum and SUS are currently used as their materials.
[0004] However, from the perspective of further improving safety, such as heat resistance, there is a need to replace aluminum in the battery can with other materials. From the perspective of heat resistance, SUS is superior to aluminum, but from the perspective of resistance to leaching from LIB electrolyte (LIB electrolyte resistance), SUS is inferior to aluminum.
[0005] Surface-treated steel sheets can be considered as alternatives to aluminum and SUS for battery cans. Advantages of steel battery cans include: high heat resistance; weight reduction through thinner walls due to high strength; increased volumetric energy density; and low cost.
[0006] However, existing surface-treated steel sheets, such as Ni-plated steel sheets, have the problem of lower resistance to LIB electrolyte compared to aluminum and SUS. For steel sheets to be used as battery can materials for automobiles, it is preferable to improve the LIB electrolyte resistance of the steel sheets to a level equal to or close to that of aluminum.
[0007] As a technology related to steel plates for battery containers, Patent Document 1 discloses the following technology: a plated steel plate for battery containers is made by performing nickel plating on one side of the steel plate that becomes the inner surface of the battery container, or by performing heat treatment in a non-oxidizing atmosphere after nickel plating, followed by nickel-tungsten alloy plating, or by performing nickel plating followed by nickel-tungsten alloy plating, and then performing heat treatment in a non-oxidizing atmosphere. This plated steel plate is then formed into a battery container and applied to a battery.
[0008] Patent document 2 discloses a Ni-containing surface-treated steel sheet for containers, which is formed by stamping. The steel sheet comprises: a steel sheet having a first surface that becomes the outer side of the container after stamping; a Ni-containing layer disposed on the first surface of the steel sheet; and a Ni-W alloy plating layer disposed on the Ni-containing layer, wherein the Ni-containing layer has an Fe-Ni diffusion alloy layer, and the Ni content in the Ni-containing layer is 5 g / m³. 2 Above and 89g / m 2 Hereinafter, the thickness of the Ni-W alloy coating is 0.02 μm or more and 2 μm or less, and the W concentration in the Ni-W alloy coating is 10% or more and 65% or less by mass%.
[0009] Patent document 3 discloses a steel plate for a non-aqueous electrolyte secondary battery casing, characterized in that it comprises: a steel plate; and a Ni-W-Fe alloy coating formed on the surface of the steel plate, containing the Ni-W-Fe alloy, which becomes the inner surface of the non-aqueous electrolyte secondary battery casing.
[0010] Existing technical documents
[0011] Patent documents
[0012] Patent Document 1: Japanese Patent Application Publication No. 2007-51325
[0013] Patent Document 2: International Publication No. 2012 / 137823
[0014] Patent Document 3: International Publication No. 2017 / 006834 Summary of the Invention
[0015] The problem that the invention aims to solve
[0016] However, patent documents 1 and 2 do not specifically address resistance to LIB electrolytes, nor do they disclose the composition used in this process.
[0017] Patent Document 3 is investigating the suppression of battery performance degradation and casing corrosion associated with metal leaching. However, the surface-treated steel sheet disclosed in Patent Document 3 is primarily intended for use in small civilian mobile devices. For example, in battery canisters constituting large batteries such as automotive batteries, superior resistance to LIB electrolytes is required compared to the surface-treated steel sheet disclosed in Patent Document 3.
[0018] In view of the above, the objective of this invention is to provide a surface-treated steel sheet with better resistance to LIB electrolyte than existing SUS sheets and Ni-plated steel sheets.
[0019] Methods for solving problems
[0020] The key points of this invention are as follows.
[0021] (1) One aspect of the present invention relates to a surface-treated steel plate comprising: a base steel plate; and a coating disposed on the surface of the base steel plate and containing Ni and W, wherein the ratio of the average value of W concentration (in atomic percent) to the sum of the average value of Ni concentration, the average value of W concentration and the average value of Fe concentration in the region from the outermost surface of the coating to a depth of 150 nm is 2.0 to 20.0 atomic percent, and the ratio of the average value of W concentration (in atomic percent) to the sum of the average value of Ni concentration, the average value of W concentration and the average value of Fe concentration in the region from the outermost surface of the coating to a depth of 150 nm is less than 0.7 times the ratio in the region from the outermost surface of the coating to a depth of 150 nm.
[0022] (2) The surface-treated steel sheet according to (1) above, wherein the amount of Ni contained in the coating can also be 2.6 to 35.6 g / m 2 .
[0023] (3) The surface-treated steel plate according to (1) or (2) above, wherein the base steel plate may also be low-carbon aluminum killed steel or IF steel.
[0024] Invention Effects
[0025] According to the present invention, a surface-treated steel sheet with better resistance to LIB electrolyte than existing SUS sheets and Ni-plated steel sheets can be provided. Attached Figure Description
[0026] Figure 1 This is a schematic cross-sectional view of a surface-treated steel plate involved in one aspect of the present invention.
[0027] Figure 2 This is a conceptual diagram showing the average concentration of W in the high-concentration W layer and the low-concentration W layer.
[0028] Figure 3 This is a flowchart of a method for manufacturing a surface-treated steel plate according to another aspect of the present invention.
[0029] Figure 4 This is a diagram illustrating the deep drawing and pressing test of the embodiment.
[0030] Figure 5A The results are surface analysis of the surface-treated steel plate of level 1 after the deep drawing and edge pressing test.
[0031] Figure 5B The results are surface analysis of the surface-treated steel plate of level 3 after the deep drawing and pressing test. Detailed Implementation
[0032] The inventors of this invention have conducted extensive and repeated studies on methods to improve the resistance of surface-treated steel sheets to LIB electrolytes. As a result, it is believed that coating the surface-treated steel sheet with a Ni-W alloy is electrochemically effective in improving its resistance to LIB electrolytes.
[0033] However, the inventors of this invention have also discovered that adding W to the Ni plating bath only improves the electrochemical properties of the Ni plating layer, but does not sufficiently improve the resistance of the surface-treated steel sheet to LIB electrolyte. The reason for this is presumably because the Ni-W plating system is relatively hard and prone to cracking. In hard plating, micro-cracks are easily generated. The inventors of this invention believe that these cracks may impair the resistance of the surface-treated steel sheet to LIB electrolyte.
[0034] Based on the above insights, the inventors of this invention conducted further research. As a result, they discovered that forming a coating containing Ni and W on the surface of a base steel sheet, with a high-concentration W layer near the surface of this coating and a low-concentration W layer below it, is extremely effective in improving resistance to LIB electrolyte. It is speculated that this is because the low-concentration W layer inhibits the propagation of cracks from the surface of the surface-treated steel sheet inwards.
[0035] like Figure 1 As shown, a surface-treated steel sheet 1 according to one embodiment of the present invention obtained based on the above insights comprises: a base steel sheet 11; and a coating 12 disposed on the surface of the base steel sheet 11 and containing Ni and W, wherein the ratio of the average W concentration (in atomic percent) to the sum of the average Ni concentration, the average W concentration, and the average Fe concentration in a region from the outermost surface of the coating 12 to a depth of 150 nm (W high concentration layer 121) is 2.0 to 20.0 atomic percent, and the ratio of the average W concentration (in atomic percent) to the sum of the average Ni concentration, the average W concentration, and the average Fe concentration in a region from a depth of 150 nm to a depth of 300 nm (W low concentration layer 122) is 0.7 times or less of the aforementioned ratio in the region from the outermost surface of the coating to a depth of 150 nm. Hereinafter, the surface-treated steel sheet 1 according to this embodiment will be described in detail.
[0036] (Base material: steel plate 11)
[0037] The surface-treated steel sheet 1 has a base steel sheet 11. The base steel sheet 11 is a steel sheet that serves as the substrate for the surface-treated steel sheet 1. The composition, thickness, and microstructure of the base steel sheet 11 are not particularly limited. When the surface-treated steel sheet 1 is used as a raw material for a battery container, the base steel sheet 11 can be, for example, low-carbon aluminum-killed steel or IF steel (Interstitial Free Steel / Ultra-Low Carbon Steel). Specific examples of the chemical composition (unit: mass%) of the base steel sheet 11 are given below.
[0038] (Example 1) Low-carbon aluminum killed steel
[0039] C: 0.057, Si: 0.004, Mn: 0.29, P: 0.014, S: 0.007, Al: 0.050, Cu: 0.034, Ni: 0.021, Remaining portion: Contains iron and impurities.
[0040] (Example 2) IF steel
[0041] C: 0.004, Si: 0.01, Mn: 0.16, P: 0.013, S: 0.006, Al: 0.029, Cu: 0.027, Ni: 0.022, Ti: 0.013, Remaining portion: Contains iron and impurities.
[0042] (Example 3) IF steel
[0043] C: 0.0012, Si: less than 0.01, Mn: 0.16, P: 0.013, S: 0.006, Al: 0.029, Cu: 0.027, Ni: 0.022, Ti: 0.020, Remaining portion: contains iron and impurities.
[0044] The thickness of the base steel plate 11 is not particularly limited. When the surface-treated steel plate 1 is used as a raw material for, for example, a battery container, the thickness of the base steel plate 11 can be, for example, 0.15 to 2.0 mm.
[0045] (Coating 12)
[0046] The surface-treated steel plate 1 involved in this embodiment has a coating 12 provided on the surface of the base steel plate 11 and containing Ni and W.
[0047] The coating 12 can also be an alloyed coating formed by the diffusion of Fe from the base steel plate 11 into a coating composed of Ni and W. That is, the coating 12 can also contain Ni, Fe, and W. The alloyed coating can be either a fully diffused coating where Fe diffuses to its surface or a partially diffused coating where Fe does not diffuse to its surface. In the case where the coating 12 is a partially diffused coating, the Fe concentration is considered to be 0 atomic percent when determining the "ratio of average W concentration" described later.
[0048] The coating 12 may also contain elements other than Ni, Fe, and W (e.g., impurity elements). Furthermore, the coating 12 may be applied to only one surface of the base steel plate 11 or to both surfaces. When the coating 12 is applied to both surfaces of the base steel plate 11, the Ni adhesion amount described later refers to the Ni adhesion amount on each side of the surface-treated steel plate 1.
[0049] Furthermore, the areas of coating 12 other than the high-concentration W layer 121 and the low-concentration W layer 122 described later can be constructed using the same structure as conventional surface-treated steel sheets (e.g., Ni-plated steel sheets for battery cans and alloyed Ni-plated steel sheets). This is because the resistance of the surface-treated steel sheet 1 to LIB electrolyte in this embodiment is achieved through the high-concentration W layer 121 and the low-concentration W layer 122.
[0050] (High-concentration W layer 121 of coating 12)
[0051] The ratio of the average W concentration (in atomic percent) to the sum of the average Ni concentration, the average W concentration, and the average Fe concentration (including 0 atomic percent) in the region from the outermost surface of the coating 12 to a depth of 150 nm is 2.0 to 20.0 atomic percent. Hereinafter, the region from the outermost surface of the coating 12 to a depth of 150 nm will be referred to as the "high W concentration layer 121". Furthermore, the ratio of the average W concentration (in atomic percent) to the average Ni concentration, the average W concentration, and the average Fe concentration will be referred to as the "W ratio". As described above, when Fe has not diffused to the surface of the coating 12 and the high W concentration layer 121 and / or the low W concentration layer 122 (described later) do not contain Fe, the Fe concentration is considered to be 0 atomic percent when calculating the W ratio of the high W concentration layer 121 and / or the low W concentration layer 122.
[0052] The average values of Ni, W, and Fe concentrations in the high-concentration layer 121 were obtained by continuously measuring the atomic concentrations of Ni, W, and Fe from the surface to the interior of the coating 12 using XPS (X-ray photoelectron spectroscopy). Figure 2 A conceptual diagram representing the average concentration of W. The method for determining the W ratio will be described in detail later.
[0053] The high-concentration W layer 121 is composed of a Ni-W alloy or a Ni-Fe-W alloy, which exhibits excellent resistance to LIB electrolyte. Therefore, the high-concentration W layer 121 improves the resistance of the surface-treated steel sheet 1 to LIB electrolyte. However, when the W ratio in the high-concentration W layer 121 is less than 2.0 atomic%, the resistance of the surface-treated steel sheet 1 to LIB electrolyte is insufficient. Therefore, the W ratio in the high-concentration W layer 121 is made to be 2.0 atomic% or more. Alternatively, the W ratio in the high-concentration W layer 121 can be 5.0 atomic% or more, 6.0 atomic% or more, 7.0 atomic% or more, or 8.0 atomic% or more.
[0054] On the other hand, when the W ratio in the high-concentration W layer 121 exceeds 20.0 atomic%, the resistance to LIB electrolyte is also insufficient. This is presumably because the high-concentration W layer 121 becomes embrittled, and fine cracks easily form in it, which impair the resistance to LIB electrolyte. Therefore, the W ratio in the high-concentration W layer 121 is kept to be 20.0 atomic% or less. Alternatively, the W ratio in the high-concentration W layer 121 can be kept to be 18.0 atomic% or less, 16.0 atomic% or less, or 15.0 atomic% or less.
[0055] (W low-concentration layer 122 of coating 12)
[0056] In the coating 12 of the surface-treated steel sheet 1 according to this embodiment, the ratio of the average W concentration (in atomic percent) in the region from a depth of 150 nm to a depth of 300 nm of the coating 12 to the sum of the average Ni concentration, the average W concentration, and the average Fe concentration (including 0 atomic percent) is 0.7 times or less than the aforementioned ratio in the region from the outermost surface of the coating to a depth of 150 nm. Hereinafter, the region from a depth of 150 nm to a depth of 300 nm of the coating 12 is referred to as the "low W concentration layer 122". That is, in the coating 12 of the surface-treated steel sheet 1 according to this embodiment, the W ratio in the low W concentration layer 122 is 0.7 times or less than the W ratio in the high W concentration layer 121.
[0057] According to the experimental results of the inventors of the present invention, the low-concentration W layer 122 further improves the resistance of the surface-treated steel sheet 1 to LIB electrolyte. The reason for this is not yet clear, but the inventors of the present invention speculate that the low-concentration W layer 122 has the effect of preventing the propagation of micro-cracks generated in the hard high-concentration W layer 121 into the interior of the coating 12. It is speculated that by preventing the propagation of cracks, the resistance of the surface-treated steel sheet 1 to LIB electrolyte is further improved. Therefore, the W ratio in the low-concentration W layer 122 is 0.7 times or less of the W ratio in the high-concentration W layer 121. The W ratio in the low-concentration W layer 122 may also be 0.6 times or less, 0.5 times or less, or 0.4 times or less of the W ratio in the high-concentration W layer 121.
[0058] (Method for determining the W ratio in high-concentration W layer 121 and low-concentration W layer 122)
[0059] As described above, XPS was used to determine the W ratio in the high-concentration W layer 121 and the W ratio in the low-concentration W layer 122.
[0060] First, the surface of the surface-treated steel sheet 1 is sputtered using rare gas ions such as argon and xenon. Next, the composition of the coating 12 is measured from the surface to the interior of the surface-treated steel sheet 1. After the measurement, sputtering is performed again, and the measurement is repeated, in a continuous cycle.
[0061] Next, in Figure 2 The graph shown, with depth on the horizontal axis and W concentration on the vertical axis, plots the analysis results of W concentration along the depth direction. Then, the value obtained by integrating the W concentration curve within the 0nm–150nm interval corresponding to the high-concentration W layer 121, divided by the width of the 0nm–150nm interval (i.e., 150nm), is considered the average W concentration C1 from the outermost surface of the coating to a depth of 150nm. Similarly, the value obtained by integrating the W concentration curve within the 150nm–300nm interval corresponding to the low-concentration W layer 122, divided by the width of the 150nm–300nm interval (i.e., 150nm), is considered the average W concentration C2 from a depth of 150nm to a depth of 300nm in the coating.
[0062] By applying the above calculations for W concentration to the analysis results for Ni and Fe, the average Ni concentration (in atomic percent) and the average Fe concentration (in atomic percent) can be obtained in the region from the outermost surface of the coating to a depth of 150 nm and in the region from a depth of 150 nm to a depth of 300 nm. Based on these values, the average W concentration in the high-concentration W layer 121 and the average W concentration in the low-concentration W layer 122 can be calculated.
[0063] Furthermore, the composition of coating 12, which was analyzed using XPS, was performed using a Mg-ray source. In the analysis using the Mg-ray source, Auger peaks overlapping with the photoelectron peaks of Ni, W, and Fe were observed. Peaks were observed for Fe (2p orbital), Ni (2p orbital), and W (4f orbital).
[0064] In the surface-treated steel sheet 1 according to this embodiment, other configurations can be appropriately selected as long as the above-mentioned conditions related to the high-concentration layer 121 and the low-concentration layer 122 are met. Hereinafter, a more preferred configuration of the surface-treated steel sheet 1 according to this embodiment will be illustrated.
[0065] (Ni adhesion amount)
[0066] The amount of Ni contained in coating 12 is not particularly limited; for example, it can be 2.6–35.6 g / m. 2 By achieving a Ni adhesion amount of 2.6 g / m 2 The above measures can further improve the resistance of the surface-treated steel sheet 1 to LIB electrolyte. On the other hand, by achieving a Ni adhesion amount of 35.6 g / m... 2 The following can reduce the manufacturing cost of coating 12. The Ni adhesion amount can also be 4.5 g / m². 2 Above, 6.2g / m 2 Above or 8.9g / m 2 The above. The Ni adhesion amount can also be 26.7 g / m. 2 Below, 17.8g / m 2 Below or 13.4g / m 2 The following applies. Furthermore, there is no particular limitation on the thickness of the coating 12. Since both the high-concentration W layer 121 and the low-concentration W layer 122 are included in the coating 12, the thickness of the coating 12 must necessarily be 300 nm or more, which is their combined thickness. However, within this range, a preferred thickness of the coating 12 can be appropriately selected. For example, the thickness of the coating 12 can be in the range of 0.3 μm to 3.0 μm. Additionally, the thickness of the coating 12 is approximately determined by the amount of Ni attached.
[0067] The amount of Ni deposited in coating 12 was determined by ICP-OES. First, a specified area of coating 12 was dissolved in acid. Then, the total amount of Ni in the solution was quantitatively analyzed by ICP-OES. By dividing the total amount of Ni quantified by ICP-OES by the specified area, the amount of Ni deposited per unit area could be determined.
[0068] (use)
[0069] The application of the surface-treated steel sheet 1 according to this embodiment is not particularly limited. For example, the surface-treated steel sheet 1 according to this embodiment can be applied to the battery canister of a large lithium-ion battery. Since the base material of the surface-treated steel sheet 1 according to this embodiment is steel sheet, it has high strength and heat resistance. Therefore, the surface-treated steel sheet 1 according to this embodiment can improve the heat resistance and strength of lithium-ion batteries and reduce their weight. In addition, according to the surface-treated steel sheet 1 according to this embodiment, the volumetric energy density can be increased by thinning the battery canister. Furthermore, the surface-treated steel sheet 1 according to this embodiment has higher resistance to LIB electrolyte than conventional surface-treated steel sheets. Therefore, the surface-treated steel sheet 1 according to this embodiment contributes to the long lifespan of lithium-ion batteries.
[0070] (Manufacturing method of surface-treated steel plate 1)
[0071] The manufacturing method of the surface-treated steel plate 1 involved in this embodiment is not particularly limited. For example, the surface-treated steel plate 1 involved in this embodiment can be obtained according to the manufacturing method described below.
[0072] like Figure 3 As shown, another aspect of the present invention relates to a method for manufacturing a surface-treated steel sheet comprising:
[0073] Process S1: Ni plating is performed on the base steel plate;
[0074] Step S2 involves Ni-W alloy plating on a base steel plate with a Ni coating; and
[0075] Step S3 is the annealing of a base steel sheet having a Ni coating and a Ni-W alloy coating disposed thereon.
[0076] Here, the thickness of the Ni coating is kept in the range of 0.3–3.5 μm.
[0077] The thickness of the Ni-W alloy coating is kept within the range of 0.010–0.30 μm.
[0078] The average W concentration of the Ni-W alloy coating is 20–45% by mass.
[0079] Furthermore, the heating rate in annealing S3 is set to 5–10 °C / second within a temperature range of 600–700 °C.
[0080] (Ni plating process S1)
[0081] First, the base steel sheet is coated with Ni using an electroplating bath. There are no particular limitations on the type of base steel sheet; for example, low-carbon aluminum-killed steel and IF steel, as mentioned above, can be appropriately used. There are also no particular limitations on the Ni plating conditions. For example, the Ni plating conditions commonly used for battery-grade Ni-plated steel sheets can be appropriately used. If necessary, the base steel sheet may also undergo pretreatment such as degreasing and pickling before Ni plating.
[0082] The thickness of the Ni coating deposited in Ni plating process S1 is measured using XRF (X-ray Fluorescence). First, a calibration curve is prepared according to the following steps.
[0083] (1) Various Ni platings with different adhesion amounts are made on the surface of the base steel plate. When making various Ni platings, the bath composition and current density are kept under the same conditions.
[0084] (2) XRF was used to analyze the above-mentioned coated steel sheet to obtain quantitative analysis results of Ni.
[0085] (3) The Ni of the above-mentioned coated steel plate was quantitatively analyzed by ICP-MS (Inductively Coupled Plasma Mass Spectrometry) to determine its adhesion amount.
[0086] (4) A calibration curve for XRF is prepared by comparing the amount of Ni attached using ICP-MS with the quantitative analysis value of Ni obtained using XRF.
[0087] Next, by using the calibration curve obtained from the above steps, the Ni coating being measured is analyzed by XRF, thereby enabling the determination of the thickness of the Ni coating that was plated in the Ni plating process S1.
[0088] (Ni-W alloy plating process S2)
[0089] (Annealing process S3)
[0090] Next, the base steel sheet with a Ni coating is coated with a Ni-W alloy using an electroplating bath. Further, the base steel sheet with both the Ni coating and the Ni-W alloy coating disposed thereon is annealed. Annealing this double-layer coating allows the alloy components to diffuse, forming a high-concentration W layer and a low-concentration W layer.
[0091] Here, it is necessary to ensure that the thickness of the Ni-W alloy coating deposited in the Ni-W alloy plating step S2 is in the range of 0.010 to 0.30 μm, and further, that the average W concentration of the Ni-W alloy coating deposited in the Ni-W alloy plating step S2 is 20 to 45% by mass. More preferably, the thickness of the Ni-W alloy coating deposited in the Ni-W alloy plating step S2 is 0.20 μm or less. By annealing the base steel sheet having such a Ni-W alloy coating, a coating with a W ratio of 2.0 to 20.0 atomic% in the high-concentration W layer and a W ratio in the low-concentration W layer of less than 0.7 times that in the high-concentration W layer can be obtained. If the thickness of the Ni-W alloy coating deposited in the Ni-W alloy plating step S2 is insufficient, or if the concentration of the Ni-W alloy coating deposited in the Ni-W alloy plating step S2 is insufficient, the W ratio in the high-concentration W layer will be insufficient. On the other hand, when the thickness of the Ni-W alloy coating is excessive, or when the concentration of the Ni-W alloy coating is excessive, the W ratio in the high-concentration W layer and / or the W ratio in the low-concentration W layer is excessive.
[0092] The thickness and composition of the Ni-W alloy coating deposited in the Ni-W alloy plating process S2 can be arbitrarily controlled by the composition of the plating bath and the electrical conditions. In other words, as long as the thickness and composition of the Ni-W alloy coating deposited in the Ni-W alloy plating process S2 are within the above-mentioned range, there are no particular limitations on the composition of the plating bath and the electrical conditions in the Ni-W alloy plating process S2.
[0093] The thickness and composition of the Ni-W alloy coating deposited in Ni-W alloy coating process S2 can be determined using XRF (X-ray Fluorescence). First, a calibration curve is prepared according to the following steps.
[0094] (1) Various Ni-W alloy coatings with different adhesion amounts are prepared on the surface of Ni-coated steel sheets with known Ni unit area weight. When preparing various Ni-W alloy coatings, the bath composition and current density are kept under the same conditions.
[0095] (2) XRF was used to analyze the above-mentioned coated steel sheet to obtain quantitative analysis results of Ni and W.
[0096] (3) The Ni and W of the above-mentioned coated steel plate were quantitatively analyzed by ICP-MS (Inductively Coupled Plasma Mass Spectrometry) to determine the amount of adhesion (the total amount of Ni coating on the lower layer and Ni-W alloy coating on the upper layer).
[0097] (4) By comparing the amount of Ni and W attached using ICP-MS with the quantitative analysis values of Ni and W obtained using XRF, a calibration curve for XRF is prepared.
[0098] Next, by using the calibration curve obtained from the above steps, the Ni-W alloy coating to be measured is analyzed by XRF, thereby enabling the determination of the thickness and composition of the Ni-W alloy coating deposited in the Ni-W alloy coating process S2.
[0099] In the annealing process S3 following the Ni-W alloy plating process S2, a heating rate of 5 to 10 °C / second is required within a temperature range of 600 to 700 °C. This allows for the formation of Ni and W concentrations, preferably varying in density, in the outermost layer of the plating. When the heating rate is less than 5 °C / second, excessive diffusion of Ni and W occurs, resulting in a lower W concentration in the high-concentration W layer and a higher W concentration in the low-concentration W layer, thus increasing the W ratio (W ratio of the low-concentration W layer ÷ W concentration of the high-concentration W layer). When the heating rate exceeds 10 °C / second, insufficient diffusion of Ni and W occurs, leading to a higher W concentration in the high-concentration W layer. Furthermore, "heating rate within a temperature range of 600 to 700 °C" refers to the "average heating rate" within this temperature range. The average heating rate is calculated by dividing 100 °C (=700 °C - 600 °C) by the time required for the temperature to rise from 600 °C to 700 °C.
[0100] As long as the heating rate is within the above-mentioned range, other annealing conditions are not particularly limited, and the annealing conditions of conventional Ni-plated steel sheets can be appropriately adopted while taking into account the amount of Ni adhesion. For example, as described above, the coating 12 of the surface-treated steel sheet 1 involved in this embodiment can be either a partially diffused alloying coating or a fully diffused alloying coating. Therefore, known annealing conditions for obtaining these alloying coatings can be appropriately adopted.
[0101] There is no particular limit to the amount of Ni adhered; for example, the total amount of Ni adhered in the Ni coating and the Ni-W alloy coating can be 2.6–35.6 g / m³. 2 The total amount of Ni attached was made 2.6 g / m. 2 The above measures can further improve the resistance of the surface-treated steel sheet 1 to LIB electrolyte. On the other hand, by achieving a total Ni adhesion amount of 35.6 g / m... 2 The following can reduce the manufacturing cost of coating 12. The total Ni adhesion amount can also be 4.5 g / m 2 Above, 6.2g / m 2 Above or 8.9g / m 2 The total Ni adhesion amount can also be 26.7 g / m². 2 Below, 17.8g / m 2 Below or 13.4g / m 2 the following.
[0102] Example
[0103] Under the conditions shown below, various surface-treated steel plates of levels 1 to 11, 14 and 15 are manufactured.
[0104] • Base steel plate: 0.40mm thick unannealed Al-K steel
[0105] • Plating bath composition: as shown in Tables 1-1 and 1-2
[0106] Plating bath temperature: 60℃
[0107] • Ni plating conditions and Ni-W alloy plating conditions: The base steel sheet was plated in the order of Ni plating and Ni-W alloy plating, in a manner that achieved the adhesion amounts described in Table 2-1. During this process, adjustments were made appropriately for each level to ensure that the current density was between 1.0 and 50.0 A / dm². 2 The energizing time is between 0.1 and 50.0 seconds, which is the target weight per unit area. (Ni plating was not performed in Level 1. In addition, Ni-W alloy plating was not performed in Level 12.) The thickness of the Ni plating is shown in Table 2-1.
[0108] Annealing: Heating to 800°C and holding at that temperature for 20 seconds is performed. The heating rate in the temperature range of 600–700°C is shown in Table 2-1.
[0109] Furthermore, as level 13, prepare a 0.40mm thick SUS304 (hereinafter SUS board).
[0110] The W ratio in the high-concentration W layer of various surface-treated steel sheets obtained through the above steps (i.e., the ratio of the average W concentration (in atomic percent) in the region from the outermost surface of the coating to a depth of 150 nm to the sum of the average Ni concentration, the average W concentration, and the average Fe concentration) is measured and shown in the "W Ratio of High-Concentration W Layer" column of Table 2-2. Furthermore, the W ratio in the low-concentration W layer (i.e., the ratio of the average W concentration (in atomic percent) in the region from a depth of 150 nm to a depth of 300 nm to the sum of the average Ni concentration, the average W concentration, and the average Fe concentration) is measured and shown in the "W Ratio of Low-Concentration W Layer" column of Table 2-2. Based on the measured W ratios in the high-concentration W layer and the low-concentration W layer, the W ratio in the low-concentration W layer relative to the high-concentration W layer is calculated and shown in the "W Ratio of Low-Concentration W Layer ÷ W Ratio of High-Concentration W Layer" column of Table 2-2. Furthermore, the resistance of various surface-treated steel sheets and SUS sheets obtained through the above steps to LIB electrolyte was evaluated.
[0111] The analytical methods for the thickness of the Ni coating before Ni-W alloy plating, the analytical methods for the W concentration and thickness of the Ni-W alloy coating on the coated steel sheet before annealing, and the methods for determining the W ratio in the high-concentration W layer and the W ratio in the low-concentration W layer of the surface-treated steel sheet after annealing are as described above. The results are shown in Table 2-2. The XPS apparatus was manufactured by ULVAC-PHI, model PHI 5600. XRF measurements were performed using Rigaku, model ZSX Primus II. Furthermore, the method for determining the amount of Ni adhering in the coating is as described above. The results are shown in the "Alloy Coating" column of Table 2-2. Further, the evaluation of the LIB electrolyte resistance of the surface-treated steel sheet and SUS sheet was conducted using processing simulation tests (deep drawing and edge pressing tests) and anolyte current tests. The results are shown in the "Evaluation Results" column of Table 2-2.
[0112] The deep drawing and blank holder test is conducted as follows: a surface-treated steel plate and a SUS plate are clamped together. Figure 4 Between the molds shown, pressing is then performed by pressing the mold in place. Further, while still pressed in the mold, the surface-treated steel sheet and SUS sheet are pulled out of the mold. The deep drawing and blank holder test simulates the pressing process of surface-treated steel sheets and SUS sheets for manufacturing battery cans. By evaluating the electrochemical characteristics of the surface-treated steel sheets and SUS sheets after the deep drawing and blank holder test, the electrochemical performance of battery cans manufactured using surface-treated steel sheets and SUS sheets can be anticipated.
[0113] The anodic current test was conducted by performing micro-electrochemical measurements on the surface of the surface-treated steel sheet and the SUS sheet after the deep drawing and edge pressing test. The anodic current test was performed using a Solratron Analytical Model 1287A potentiostat. The evaluation conditions are as follows.
[0114] • The shape of the evaluation area: a circle with a diameter of 500 μm
[0115] • Measurement sites: Five sites (the average value of the measurement results from the five sites will be used as the final evaluation result)
[0116] • Potential control: After setting up the measurement system, maintain the OCV (Open Circuit Voltage) for 5 minutes, then increase it to 4.5V. Set the scan rate during the rise to 20mV / s using vs. Li LSV (Linear Sweep Voltammetry).
[0117] • Measurement environment: air temperature below 23℃, dew point below -80℃, oxygen concentration below 0.7ppm
[0118] ·Electrolyte: 1mol / L LiPF6 EC (ethylene carbonate): EMC (ethyl methyl carbonate) (1:3 v / v%) + VC (vinylene carbonate) 2 wt%
[0119] ·Pass / fail criterion: A result is deemed acceptable when the anode current value at 3.8V is 0.025 μA or less
[0120] [Table 1-1]
[0121] Composition of Bath 1
[0122] Drug Name molar concentration (mol / L) g / L <![CDATA[NiSO4·6H2O]]> 1.29 340 <![CDATA[NiCl2·6H2O]]> 0.29 70 Boric acid 0,73 45 <![CDATA[H2SO4]]> 0.005 0.5
[0123] [Table 1-2]
[0124] Composition of Bath 2
[0125] Drug Name molar concentration (mol / L) g / L <![CDATA[Na2WO4·2H2O]]> 0.20 65.97 <![CDATA[NiSO4·6H2O]]> 0.20 52.57 Ammonium citrate 0.45 101.78 Sodium formate 0.20 13.60
[0126] [Table 2-1]
[0127]
[0128] [Table 2-2]
[0129]
[0130] Level 1 is a surface-treated steel sheet obtained by forming only a Ni-W alloy plating layer on the surface of a base steel sheet followed by annealing. Levels 2 to 11, 14 and 15 are surface-treated steel sheets obtained by forming a Ni plating layer on the surface of a base steel sheet, further forming a thin Ni-W alloy plating layer thereon, followed by annealing. Level 12 is a surface-treated steel sheet obtained by forming only a Ni plating layer on the surface of a base steel sheet followed by annealing. Level 13 is a SUS sheet having no plating layer.
[0131] Levels 3 to 6 and Levels 8 to 11 are invention examples having a W high-concentration layer with a W ratio of 2.0 to 20.0 at% and a W low-concentration layer with a W ratio of 0.7 times or less that of the W high-concentration layer. These are superior in LIB electrolyte resistance to Level 1, which is a conventional Ni-W alloy plated steel sheet, Level 12, which is a conventional Ni plated steel sheet, and Level 13, which is a conventional SUS sheet. That is, according to the present invention, it is possible to provide a surface-treated steel sheet having better LIB electrolyte resistance than conventional SUS sheets, Ni plated steel sheets and the like, and a method for producing the same.
[0132] Furthermore, levels 2 and 7, like levels 3-6 and 8-10, are obtained by annealing after forming the Ni coating and the Ni-W alloy coating. However, in level 2, the W ratio in the high-concentration W layer is excessive, and the low-concentration W layer also contains a large amount of W, thus failing the LIB electrolyte resistance test. This is believed to be because the Ni-W alloy coating in level 2 is too thick. In level 7, the W ratio in the high-concentration W layer is too low, thus failing the LIB electrolyte resistance test. This is believed to be because the Ni-W alloy coating in level 7 is too thin.
[0133] In Level 14, the heating rate in the temperature range of 600℃ to 700℃ was too low, resulting in substandard resistance to LIB electrolyte. This is believed to be due to excessive diffusion of Ni and W, leading to a decrease in W concentration in the high-concentration W layer and an increase in W concentration in the low-concentration W layer, thus the W ratio in the low-concentration W layer exceeds 0.7 times that in the high-concentration W layer.
[0134] In Level 15, the heating rate within the temperature range of 600℃ to 700℃ was too high, resulting in substandard resistance to LIB electrolyte. This is believed to be due to insufficient diffusion of Ni and W, leading to a higher W ratio in the high-concentration W layer.
[0135] Figure 5A This represents the surface analysis results of the surface-treated steel plate at level 1 after the deep drawing and edge clamping test. Figure 5B This represents the surface analysis results of the surface-treated steel plate at level 3 after the deep drawing and edge pressing test. Figure 5A as well as Figure 5B In the image, the top left image is a SEM photograph of the surface-treated steel plate, the top right image is the surface analysis result of the Fe concentration at the location where the SEM photograph was taken, the bottom left image is the surface analysis result of the Ni concentration at the location where the SEM photograph was taken, and the bottom right image is the surface analysis result of the W concentration at the location where the SEM photograph was taken.
[0136] The surface of the surface-treated steel sheet at Level 1 exhibits multiple Ni and W deficiency sites. These deficiency sites also show high Fe concentrations. In the Level 1 surface-treated steel sheet, it is believed that the hard Ni-W alloy coating develops numerous cracks, exposing the base steel sheet. On the other hand, no Ni and W deficiency sites were observed on the surface of the Level 4 surface-treated steel sheet. It is speculated that by suppressing the exposure of the base steel sheet, the resistance of the Level 4 surface-treated steel sheet to LIB electrolyte is significantly improved compared to Level 1.
[0137] Explanation of reference numerals in the attached figures
[0138] 1 Surface-treated steel plate
[0139] 11 Base steel plate
[0140] 12 coatings
[0141] 121W high-concentration layer
[0142] 122W low concentration layer
[0143] The average concentration of W in the high-concentration layer of C1 W
[0144] The average concentration of W in the low-concentration layer of C2 W
[0145] S1 Ni plating process
[0146] S2 Ni-W alloy plating process
[0147] S3 annealing process.
Claims
1. A surface-treated steel sheet comprising: a base steel sheet; and a coating disposed on the surface of the base steel sheet and containing Ni and W. in, The ratio of the average W concentration (in atomic percent) to the average Ni concentration, the average W concentration, and the average Fe concentration in the region from the outermost surface of the coating to a depth of 150 nm is 2.0 to 20.0 atomic percent. The ratio of the average W concentration (in atomic percent) to the sum of the average Ni concentration, the average W concentration, and the average Fe concentration in the region from a depth of 150 nm to a depth of 300 nm of the coating is less than 0.7 times the ratio in the region from the outermost surface of the coating to a depth of 150 nm.
2. The surface-treated steel plate according to claim 1, characterized in that, The amount of Ni in the coating is 2.6–35.6 g / m. 2 .
3. The surface-treated steel plate according to claim 1 or 2, characterized in that, The base steel plate is low-carbon aluminum killed steel or IF steel.
Citation Information
Patent Citations
Plated steel plate for battery case, battery case using the steel plate for battery case and battery using the battery case
JP2007051325A
Folding chair having rod hanger for outdoor fishing
JP2021065675A
Ni-containing surface-treated steel sheet for containers, and method for producing same
WO2012137823A1
Steel plate for case of non-aqueous-electrolyte secondary cell, and case of non-aqueous-electrolyte secondary cell
WO2017006834A1
Ni-containing-surface-treated steel sheet for can and manufacturing method thereof
US20140017515A1