A corrosion-resistant rare earth hafnium salt coating structure and its preparation method
By preparing rare earth hafnium salt coatings on the surface of hot-end components of aero-engines, the problem of existing coatings being susceptible to CMAS corrosion at high temperatures has been solved, achieving efficient and low-cost corrosion protection, which is suitable for mass production.
Patent Information
- Application Number
- CN202311096018.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-08-29
- Publication Date
- 2026-11-10
- Estimated Expiration
- 2043-08-29
Smart Images

Figure CN117107188B_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of inorganic material preparation technology, and more specifically, to a rare earth hafnium salt coating structure and preparation method that can be applied to the surface of ceramic composite matrix materials and high-temperature alloy materials to resist high-temperature CMAS corrosion. Background Technology
[0002] Aero engines are considered the crown jewel of modern industry, and their technological development level is a crucial indicator of a nation's scientific, military, and industrial capabilities. Currently, the surface temperature of hot-section components in next-generation high thrust-to-weight ratio aero engines exceeds 1500℃. However, when the operating temperature of these hot-section components exceeds 1230℃, solid particles (primarily composed of CaO-MgO-Al2O3-SiO2, CMAS) drawn in from the air, such as volcanic ash, solid dust, and ashes, melt to form liquid CMAS that adheres to the surface of hot-section components like blades, causing a significant performance degradation. Therefore, designing and fabricating a protective coating with excellent resistance to high-temperature CMAS corrosion is of paramount importance for extending the service life of aero engines.
[0003] Currently common protective coating materials include YSZ, rare earth zirconates, and rare earth silicates. However, YSZ is susceptible to CMAS corrosion, leading to coating failure, and its service temperature is relatively low (1200℃). Rare earth zirconates have poor mechanical properties, while rare earth silicates have high thermal conductivity but insufficient resistance to CMAS corrosion at 1500℃. Therefore, a new protective coating is needed to resist the damage caused by harsh service environments.
[0004] Studies have found that rare earth hafnium salts have advantages such as high melting point, low thermal conductivity, good mechanical properties and excellent high-temperature phase stability, making them candidate materials for high-temperature corrosion protective coatings. Summary of the Invention
[0005] To address the problems in the prior art, the present invention aims to provide a rare earth hafnium salt coating structure resistant to high-temperature CMAS corrosion and its preparation method.
[0006] According to one aspect of the present invention, a corrosion-resistant rare earth hafnium salt coating structure is provided, comprising a substrate and a coating on its surface, wherein the coating comprises a rare earth hafnium salt having the chemical formula RE4Hf3O. 12 RE can be Ho, Er, Tm, Yb, or Lu.
[0007] Preferably, the coating is prepared on the surface of the substrate by plasma spraying.
[0008] Preferably, the matrix is selected from graphite, SiC, Si3N4, C / C composite material, C / SiC composite material, and SiC. f / SiC composite materials, stainless steel or high-temperature alloy materials.
[0009] According to another aspect of the present invention, a method for preparing the above-mentioned corrosion-resistant rare earth hafnium salt coating structure is provided, comprising the following steps:
[0010] Step 1: Prepare a spraying powder, wherein the spraying powder includes rare earth hafnium salts;
[0011] Step 2: Prepare the coating by spraying the powder onto the substrate surface using plasma spraying.
[0012] Preferably, step 1 includes:
[0013] Step 1.1: Weigh the raw materials according to the molar ratio of HfO2:RE2O3 = 3:2;
[0014] Step 1.2: After mixing the raw materials, react and sinter them to obtain ceramic powder;
[0015] Step 1.3 involves sequentially crushing, preparing slurry, spray granulating and sintering the obtained ceramic powder, and then sieving it to obtain the spray coating powder.
[0016] Preferably, the sintering temperature in step 1.2 is 1400-1700℃, and the holding time is 8-12h.
[0017] Preferably, the particle size distribution of the ceramic powder in step 1 is 10-100 μm.
[0018] Preferably, step 2 further includes roughening the substrate surface before spraying the substrate surface.
[0019] Preferably, the roughening pretreatment is sandblasting pretreatment or laser patterning treatment.
[0020] Preferred: The process parameters of the plasma spraying method in step 2 include: plasma gas Ar: 22-45 slpm; plasma gas H2: 5-9 slpm; spraying distance: 100-150 mm; spraying voltage: 65-75 V; spraying power: 30-50 kW; powder feeding rate: 10-35 r / min.
[0021] Compared with the prior art, the beneficial effects of the technical solution of the present invention are as follows:
[0022] 1. The rare earth hafnium salt coating designed in this invention regulates the reaction process of the material under high-temperature CMAS corrosion, reducing the degree of reaction between the material and CMAS at high temperature. Compared with traditional YSZ coatings or rare earth zirconate coatings, it has better high-temperature CMAS corrosion resistance.
[0023] 2. The prepared rare earth hafnium salt coating has uniform composition, dense structure, and no defects such as through cracks.
[0024] 3. The powder preparation process adopted in the technical solution of this invention has the advantages of low cost, high powder purity, high preparation efficiency, and suitability for batch preparation.
[0025] 4. The coating preparation method adopted in the technical solution of the present invention is plasma spraying, which has the advantages of fast deposition speed, low cost, good repeatability, large adjustable range of coating thickness, high production efficiency, and suitability for large-scale production. Attached Figure Description
[0026] Other features, objects, and advantages of the present invention will become more apparent from the following detailed description of non-limiting embodiments with reference to the accompanying drawings.
[0027] Figure 1 The Yb4Hf3O prepared in Example 1 of this invention is shown. 12 XRD pattern of powder;
[0028] Figure 2 The Yb4Hf3O prepared in Example 1 of this invention is shown. 12 Surface and cross-sectional morphology of the coating;
[0029] Figure 3 The Yb4Hf3O prepared in Example 1 of this invention is shown. 12 Cross-sectional morphology of the coating after CMAS etching;
[0030] Figure 4 The Lu4Hf3O prepared in Example 2 of this invention is shown. 12 Cross-sectional morphology of the coating after CMAS etching;
[0031] Figure 5 The cross-sectional morphology of the Gd2Zr2O7 coating prepared in Comparative Example 1 of the present invention after CMAS etching is shown.
[0032] Figure 6 The cross-sectional morphology of the YSZ coating prepared in Comparative Example 2 of the present invention after CMAS corrosion is shown. Detailed Implementation
[0033] Exemplary embodiments will now be described more fully with reference to the accompanying drawings. However, these exemplary embodiments can be implemented in many forms and should not be construed as limited to the embodiments set forth herein. Rather, these embodiments are provided so that the invention will be thorough and complete, and will fully convey the concept of the exemplary embodiments to those skilled in the art. The same reference numerals in the drawings denote the same or similar structures, and therefore repeated descriptions of them will be omitted.
[0034] In an embodiment of the present invention, a corrosion-resistant rare earth hafnium salt coating structure includes a substrate and a coating prepared on the surface of the substrate. The coating includes rare earth hafnium salts with the chemical formula RE4Hf3O. 12 RE can be any rare earth element among Ho, Er, Tm, Yb, or Lu.
[0035] The present invention also provides a method for preparing a coating, including the synthesis of powder and the preparation of coating.
[0036] The powder preparation method includes the following steps:
[0037] (1) Using RE2O3 powder and HfO2 powder as raw materials, RE is any rare earth element among Ho, Er, Tm, Yb or Lu, and the raw materials are weighed in a molar ratio of HfO2:RE2O3 = 3:2;
[0038] (2) Using anhydrous ethanol or deionized water as a medium, the raw materials in step (1) are mixed evenly and dried by planetary ball milling to obtain mixed raw materials;
[0039] (3) The mixed raw materials are placed in a high-temperature muffle furnace for reaction sintering to obtain rare earth hafnium salt ceramic powder material;
[0040] (4) The rare earth hafnium salt material obtained in step (3) is crushed, slurry prepared, spray granulated and sintered and screened in sequence to obtain spherical spray powder for plasma spraying.
[0041] Preferably, in step (2), the planetary ball milling method uses anhydrous ethanol as the medium, the planetary ball milling speed is 150-200 r / min, and the time is 5-10 h.
[0042] Preferably, the high-temperature reaction sintering in step (3) is carried out in an air atmosphere at a temperature of 1400-1700℃ for a holding time of 8-12h.
[0043] Preferably, the slurry in step (4) is a slurry with a powder solid content of 50%-65wt.% prepared by using powder, deionized water and PVA, and the mass of PVA is 5‰-12‰ of the powder mass.
[0044] Preferably, the sintering in step (4) is carried out in an air atmosphere at a temperature of 1300-1500℃ for a holding time of 3-6h.
[0045] Preferably, in step (4), the sieving is passed through a 270-mesh sieve, and the particle size of the spherical rare earth hafnium salt powder obtained for spraying is 10-100 μm.
[0046] The coating preparation method includes the following steps:
[0047] (1) Pretreatment of the substrate to roughen the surface;
[0048] (2) A corrosion-resistant rare earth hafnium salt coating was prepared by plasma spraying.
[0049] Preferably, in step (1), the matrix is selected from graphite, SiC matrix, Si3N4 matrix, C / C composite matrix, C / SiC composite matrix, and SiC. f One of the following: SiC composite matrix and stainless steel or high-temperature alloy matrix;
[0050] Preferably, the pretreatment in step (1) is sandblasting pretreatment or laser patterning treatment;
[0051] Preferably, the process parameters of the plasma spraying method in step (2) include: plasma gas Ar: 22-45 slpm; plasma gas H2: 5-9 slpm; spraying distance: 100-150 mm; spraying voltage: 65-75 V; spraying power: 30-50 kW; powder feeding rate: 10-35 r / min.
[0052] The preparation method and coating prepared according to the embodiments of the present invention have good high-temperature CMAS corrosion resistance and are suitable for mass production.
[0053] The present invention will be described below with reference to specific embodiments.
[0054] Example 1
[0055] This embodiment uses plasma spraying to prepare Yb4Hf3O 12 The coating was applied, and its corrosion behavior in CMAS at 1500℃ was investigated.
[0056] The preparation method in this embodiment is as follows:
[0057] (1) Place HfO2 and Yb2O3 raw material powders in a ball mill jar at a molar ratio of 3:2, use anhydrous ethanol as a mixing agent, mix for 6 hours using planetary ball milling, and then dry at 100℃.
[0058] The dried mixed raw materials were placed in a muffle furnace and kept at 1500℃ for 10 hours to obtain Yb4Hf3O. 12 Material.
[0059] (2) Prepare Yb4Hf3O 12 The bulk material is crushed and a slurry is prepared. The slurry uses deionized water as a solvent and PVA as a binder, with a solid content of 50-65%. After spray granulation, the slurry is sintered at 1300℃ for 4 hours in air. Yb4Hf3O is obtained by passing it through a 270-mesh sieve, resulting in a median particle size of 30-50 μm and a particle size distribution of 10-100 μm, suitable for spraying.12 The powder.
[0060] (3) Yb4Hf3O was prepared on the surface of SiC substrate using atmospheric plasma spraying technology. 12 The parameters for the plasma spraying coating are shown in Table 1.
[0061] Table 1: Plasma Spraying of Yb4Hf3O 12 Coating process parameter table
[0062]
[0063] *slpm: Standard liters per minute.
[0064] XRD patterns of powder and coating in Example 1 are shown below. Figure 1 Cross-sectional morphology is shown in Figure 2 In Example 1, the coating melted well after spraying, exhibiting a relatively dense structure and a single phase without decomposition or the appearance of a second phase. It can be observed that the sprayed coating possesses the unique morphology characteristic of coatings prepared by plasma spraying, exhibiting special structures such as interfaces and transverse microcracks. The coating porosity is below 5%, effectively resisting CMAS penetration.
[0065] The coating was tested for resistance to CMAS corrosion under the following conditions: CMAS powder concentration was 35 mg / cm³. 2 The test temperature was 1500℃, and the test time was 25 hours. The cross-sectional microstructure of the coating after CMAS etching at 1500℃ for 25 hours is shown below. Figure 3 As shown, the coating structure did not suffer significant damage within this temperature range, and the penetration of CMAS was confined to the coating surface, indicating that this embodiment can effectively mitigate CMAS corrosion of the coating.
[0066] Example 2
[0067] In this embodiment, Lu4Hf3O was prepared using plasma spraying. 12 The coating was applied, and its corrosion behavior in CMAS at 1500℃ was investigated.
[0068] The preparation method in this embodiment is as follows:
[0069] (1) Lu2O3 and HfO2 raw material powders were placed in a ball mill jar at a molar ratio of 2:3, and anhydrous ethanol was used as the mixing agent. The mixture was mixed by planetary ball milling for 6 hours and then dried at 100℃. The dried mixture was placed in a muffle furnace and kept at 1500℃ for 10 hours to obtain Lu4Hf3O 12 Material.
[0070] (2) Prepare Lu4Hf3O 12The bulk material is crushed and a slurry is prepared. The slurry uses deionized water as a solvent and PVA as a binder, with a solid content of 50-65%. After spray granulation, the slurry is sintered at 1300℃ for 4 hours in air. The slurry is then passed through a 270-mesh sieve to obtain Lu4Hf3O with a median particle size of 30-50 μm and a particle size distribution of 10-100 μm, suitable for spraying. 12 The powder.
[0071] (3) Lu4Hf3O was prepared on the surface of a SiC substrate using atmospheric plasma spraying technology. 12 The coating parameters for the plasma spraying are the same as those in Example 1.
[0072] In this embodiment, the coating exhibited good surface melting after spraying, a relatively dense cross-sectional structure, and a single phase; no decomposition or second phase was observed during the spraying process. The coating's resistance to CMAS corrosion was tested under the following conditions: CMAS powder concentration of 35 mg / cm³. 2 The test temperature was 1500℃, and the test time was 25 hours. The cross-sectional microstructure of the coating after CMAS etching at 1500℃ for 25 hours is as follows. Figure 4 As shown, within this temperature range, the coating structure remains intact without any through cracks, and the penetration of CMAS is confined to the coating surface, indicating that this embodiment effectively mitigates the corrosion of CMAS.
[0073] The above description is merely a preferred embodiment of the present invention and is not intended to limit the scope of the invention. Various variations can be made to the above embodiments of the present invention. That is, all simple and equivalent changes and modifications made based on the claims and description of this invention fall within the protection scope of the claims of this patent. All aspects not described in detail in this invention are conventional technical content.
[0074] Comparative Example 1
[0075] The difference between this comparative example and the coating structure design described in Example 1 is that the coating composition is Gd2Zr2O7, while the rest is the same as in Example 1.
[0076] The resulting coating was subjected to CMAS etching at 1500°C, under the same conditions as in Examples 1 and 2. Figure 5 The cross-sectional morphology of the Gd2Zr2O7 coating after CMAS etching at 1500℃ for 25 hours is shown. It can be seen that the coating was completely penetrated after CMAS etching at 1500℃ for 25 hours. Therefore, it can be concluded that the CMAS corrosion resistance of the Gd2Zr2O7 coating is worse than that of the example.
[0077] Comparative Example 2:
[0078] The difference between this comparative example and the coating structure design described in Example 1 is that the coating composition is 8 wt% Y2O3 stabilized ZrO2 (YSZ), and the rest is the same as in Example 1.
[0079] The resulting coating was subjected to CMAS etching at 1500°C, under the same conditions as in Examples 1 and 2. Figure 6 The cross-sectional morphology of the YSZ coating after CMAS corrosion at 1500℃ for 25 hours is shown. It can be seen that after the reaction at 1500℃, the coating was completely penetrated, and transverse through-cracks appeared in the coating cross-section, indicating complete coating failure. Therefore, the CMAS corrosion resistance of the YSZ coating is far inferior to that of the coating in the example.
[0080] In summary, the coating of this invention exhibits superior resistance to high-temperature CMAS corrosion. The preparation process offers advantages such as rapid deposition, low cost, good repeatability, a wide adjustable range of coating thickness, high production efficiency, and suitability for large-scale production.
[0081] The above description, in conjunction with specific preferred embodiments, provides a further detailed explanation of the present invention. It should not be construed that the specific implementation of the present invention is limited to these descriptions. For those skilled in the art, various simple deductions or substitutions can be made without departing from the concept of the present invention, and all such modifications and substitutions should be considered within the scope of protection of the present invention.
Claims
1. A method for preparing a corrosion-resistant rare earth hafnium salt coating structure, characterized in that: Includes the following steps: Step 1: Prepare a spraying powder, wherein the spraying powder includes rare earth hafnium salts, and the chemical formula of the rare earth hafnium salts is RE4Hf3O. 12 RE is Ho, Er, Tm, Yb, or Lu; step 1 includes: Step 1.1: Weigh the raw materials according to the molar ratio of HfO2:RE2O3 = 3:2; Step 1.2: The raw materials are mixed with anhydrous ethanol or deionized water as a medium and then subjected to reaction sintering. The mixture is prepared by planetary ball milling at a speed of 150-200 r / min for 5-10 h to obtain ceramic powder. The sintering temperature in Step 1.2 is 1400-1700 ℃ and the holding time is 8-12 h. Step 1.3: The obtained ceramic powder is crushed, slurry prepared, spray granulated and sintered, and then sieved to obtain the spray coating powder; the sintering temperature is 1300-1500℃. The slurry is prepared using powder, deionized water, and PVA, with a powder solid content of 50%-65wt.% and the PVA mass being 5‰-12‰ of the powder mass. Step 2: Prepare a coating by spraying the powder onto the substrate surface using plasma spraying.
2. The method for preparing the corrosion-resistant rare earth hafnium salt coating structure according to claim 1, characterized in that: The particle size distribution of the ceramic powder in step 1 is 10-100 μm.
3. The method for preparing the corrosion-resistant rare earth hafnium salt coating structure according to claim 1, characterized in that: Step 2 further includes roughening the substrate surface before spraying the substrate surface.
4. The method for preparing the corrosion-resistant rare earth hafnium salt coating structure according to claim 3, characterized in that: The roughening pretreatment is either sandblasting or laser patterning.
5. The method for preparing the corrosion-resistant rare earth hafnium salt coating structure according to claim 1, characterized in that: The process parameters for the plasma spraying method in step 2 include: plasma gas Ar: 22-45 slpm; plasma gas H2: 5-9 slpm; spraying distance: 100-150 mm; spraying voltage 65-75 V; spraying power: 30-50 kw; powder feeding rate: 10-35 r / min.
Citation Information
Patent Citations
Nano-structure rare earth hafnate ceramic powder feed for thermal spraying as well as preparation method and application of nano-structure rare earth hafnate ceramic powder feed
CN116023136A