Slot die adjustment with mixing control

Coordinating multiple actuators through a hybrid control process to adjust the cross-sectional height of the slot die solves the problem of insufficient spatial resolution of the slot die, achieves higher precision and consistency, and improves the quality and quality of the extruded film. Production efficiency.

CN117120237BActive Publication Date: 2024-10-293M INNOVATIVE PROPERTIES CO
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202180096936.7
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2021-04-16
Publication Date
2024-10-29
Estimated Expiration
2041-04-16

AI Technical Summary

Technical Problem

Existing slot dies have limited spatial resolution when controlling extruded web thickness, making it difficult to achieve high accuracy and consistency in tenter film operations, especially during transverse stretching of the film. Precise control of membrane width is limited.

Method used

Using a hybrid control process, by coordinating the movement of multiple primary actuators and secondary actuators, combined with precision sensors and controllers, the cross-sectional height of the slit mold is adjusted, thereby achieving local adjustment of the fluid flow channel and improving the amplitude. Material lateral spatial resolution.

Benefits of technology

Significantly improved die slit accuracy and consistency allows for finer film width control in the tenter film process, improving extrudate quality and production efficiency.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN117120237B_ABST
    Figure CN117120237B_ABST
Patent Text Reader

Abstract

The present invention provides methods and systems associated with adjusting a slot die. The slot die includes: a coating slot extending across the width of the slot die, the coating slot being in fluid communication with a fluid flow channel through the slot die; an adjustment mechanism including a slot die surface; and a plurality of primary actuators spaced apart along the width of the slot die. Each primary actuator is operably coupled to one or more secondary actuators, and each secondary actuator is operably coupled to the adjustment mechanism to adjust the cross-sectional height of the fluid flow channel at its respective position, thereby providing local adjustment of the fluid flow through the coating slot. The method includes: determining a target slot height profile, and then predicting a set of primary actuator settings and a set of secondary actuator settings based on the target slot height profile using a controller. Each primary actuator and secondary actuator are then individually positioned according to the predicted set of primary actuator settings and set of secondary actuator settings to adjust the slot die.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention provides a slot die and related components, systems and methods that can be used for continuous manufacturing of products. Background Art

[0002] Industrial manufacturers usually use slot dies for polymer processing. Slot dies can be used for coating, where liquid materials are extruded onto a moving flexible substrate (such as a backing or release liner). The liquid material can be a polymer melt or a reactive monomer mixture. When the material is applied to a substrate, the process is generally referred to as extrusion coating. In other cases, the extruded material can directly form a self-supporting film without a backing.

[0003] There are many variations in the way slot die extrusion is performed. As an example, the coating material may be at ambient temperature or at an elevated temperature. When the coating material temperature is elevated to ensure that the feed raw material is melted or liquefied for processing, the material is generally referred to as a "hot melt" coating. The extrudate may include a solvent diluent. The solvent may be water, an organic solvent, or any suitable fluid that dissolves or disperses the components of the coating. The solvent is typically removed in subsequent processing such as drying. The coating may include a single or multiple layers, and some slot dies may be used to apply multiple layers simultaneously. The coating may be a continuous coating across the width of the die or alternatively include shaped bands, each band extending across only a portion of the width of the die and separated from adjacent bands.

[0004] Generally speaking, a slot die includes a pair of opposed die lips forming a coating slot. The width of the coating slot may extend about the width of a moving web or the width of a roll receiving an extruded product such as a film. As used herein, "width" with respect to slot dies and components of slot dies refers to the cross-web dimension of the slot die and its components. The thickness of the extruded web is usually adjusted by changing the shape of one or both of the die lips, or by adjusting a choke bar located upstream of the die lips.

[0005] The technology of adjusting the cross-web profile on a film extrusion die or an extrusion coating die generally involves one of two methods. First, the die lip or choke bar can be manually adjusted using a differential bolt that uses a screw mechanism to make minor adjustments to the shape of the die lip or choke bar. Second, the die lip or choke bar can be adjusted using a thermal assist bolt that can change length with temperature and can engage the die lip or choke bar for even finer adjustments. Some of these processes are described in co-pending International Patent Application Nos. PCT / IB2020 / 061685 (Yapel et al.), PCT / IB2020 / 061687 (Yapel et al.), and PCT / IB2020 / 061688 (Secor et al.), and U.S. Provisional Patent Application No. 63 / 122,996 (Secor et al.), all of which were filed on December 9, 2020. Summary of the invention

[0006] Web transverse control spatial resolution is a problem of particular concern in the control of the die. The spatial resolution of the die slit limits the resolution of the control of the extruded web thickness and minimizes the transverse fluctuation of the web. This is of particular concern in stenter film operations, such as for optical grade films. In stenter film operations, the film is extruded and then stretched in the transverse direction, which affects the resolution of the die through the stretch factor. If the film is stretched transversely by 6 times, the actuator / bolt spacing of 1 cm on the die can only be controlled to 6 cm width of the final film. Transverse stretching can be a separate process step in a series of steps including extrusion (i.e., casting), length orientation, transverse orientation and / or combined biaxial stretching of the film.

[0007] Advantageously, the provided method uses a hybrid control process that coordinates the movement of two different actuators to achieve a significant enhancement in the transverse spatial resolution of the web. In some embodiments, these hybrid controls allow the use of existing metering and mapping back to the mold in the stenter film process. Conveniently, when using an existing metering system such as that already configured on a manufacturing line, the hybrid control can be used to operate the mold. In summary, these improved systems and methods increase the higher accuracy, consistency and understanding of the mold gap.

[0008] In a first aspect, a method of adjusting a slot die is provided. The slot die comprises: a coating slot extending across a width of the slot die, the coating slot being in fluid communication with a fluid flow channel through the slot die; an adjustment mechanism comprising a slot die surface; and a plurality of primary actuators spaced apart along the width of the slot die, wherein each primary actuator is operably coupled to one or more secondary actuators, and each secondary actuator is operably coupled to the adjustment mechanism to adjust a cross-sectional height of the fluid flow channel at a corresponding position thereof, thereby providing a local adjustment of a fluid flow through the coating slot. The method comprises: determining a target slot height profile; predicting a set of primary actuator settings and a set of secondary actuator settings using a controller based on the target slot height profile; and individually positioning each primary actuator and secondary actuator according to the predicted set of primary actuator settings and set of secondary actuator settings to adjust the slot die.

[0009] In a second aspect, a system is provided, the system comprising: a slot die, wherein the slot die includes: a coating slot, the coating slot extending across the width of the slot die, wherein the coating slot is fluidly connected to a fluid flow channel through the slot die; an adjustment mechanism, the adjustment mechanism including a slot die surface, the slot die surface for adjusting the cross-sectional height of the fluid flow channel through the coating slot; and a plurality of primary actuators, the plurality of primary actuators spaced along the width of the slot die surface, wherein each primary actuator is operably connected to one or more secondary actuators, and each secondary actuator is operably connected to the adjustment mechanism to adjust the cross-sectional height of the fluid flow channel at its corresponding position, thereby providing local adjustment of the fluid flow through the coating slot; and a controller, the controller being capable of independently setting the position of each primary actuator and each secondary actuator. BRIEF DESCRIPTION OF THE DRAWINGS

[0010] Figure 1 is a schematic diagram illustrating a production line including a slot die according to an exemplary embodiment.

[0011] Figure 2 yes Figure 1 Perspective view of the slot die.

[0012] Figure 3 yes Figure 1 and Figure 2 A side cross-sectional view of a slot die in which a primary actuator and a secondary actuator are provided to adjust the height of a fluid flow channel at a given location.

[0013] Figure 4 It is shown Figures 1 to 3 A perspective view of the front end portion of the slot die secondary actuator.

[0014] Figures 5 to 7 is shown for operation Figures 1 to 4 Block diagram of the various control loops of the slot die.

[0015] Fig. 8A and Figure 8B It is shown Figures 1 to 4 Top view of the configuration of the primary actuator and the secondary actuator in the slot die before and after adjustment.

[0016] Fig. 9 is shown for operation Figures 1 to 4 Block diagram of another control loop of the slit die.

[0017] Fig.10 is a graph showing the temperature profile of an array of secondary actuators, followed by a parallel graph showing the power input profile of the same secondary actuators.

[0018] Fig.11 and Fig.12 is a graph showing the mean value and ±2s fluctuation limits of the cross-web thickness profile for extruded webs produced using two different methods of operating the slot die.

[0019] Reference symbols used repeatedly in the specification and drawings are intended to represent the same or similar features or elements of the present disclosure. It should be understood that those skilled in the art can design many other modifications and embodiments that fall within the scope and essence of the principles of the present disclosure. The drawings may not be drawn to scale. DETAILED DESCRIPTION

[0020] As used herein, the terms "preferred" and "preferably" refer to embodiments described herein that may provide certain benefits under certain circumstances. However, other embodiments may also be preferred under the same or other circumstances. In addition, the recitation of one or more preferred embodiments does not imply that other embodiments are not useful and is not intended to exclude other embodiments from the scope of the invention.

[0021] As used herein and in the appended claims, the singular forms "a / an" and "the" include plural referents unless the context clearly dictates otherwise. Thus, for example, reference to "a / an" or "the" component may include one or more components known to those skilled in the art or their equivalents. Additionally, the term "and / or" means one or all of the listed elements or a combination of any two or more of the listed elements.

[0022] It is worth noting that the term "including" and its variations do not have a restrictive meaning when appearing in the attached specification. In addition, "one", "an", "the", "at least one" and "one or more" are used interchangeably herein. Relative terms such as left, right, forward, backward, top, bottom, side, upper, lower, horizontal, vertical, etc. may be used herein, and if so, they are from the perspective observed in the specific drawings. However, these terms are only used to simplify the description and are not intended to limit the scope of the present invention in any way.

[0023] References throughout this specification to "one embodiment," "certain embodiments," "one or more embodiments," or "an embodiment" mean that the particular features, structures, materials, or characteristics described in relation to that embodiment are included in at least one embodiment of the present invention. Thus, phrases such as "in one or more embodiments," "in certain embodiments," "in one embodiment," or "in an embodiment" that appear in various places throughout this specification do not necessarily refer to the same embodiment of the present invention. Where applicable, trade names are listed in all capital letters.

[0024] Figure 1 A manufacturing process line, hereinafter indicated by the numeral 50, is shown according to an exemplary embodiment. The process line 50 includes various polymer processing stages that occur in sequence. These stages are sequentially performed through an extruder 52, a slot die 54, a casting roll assembly 56, a machine direction stretcher 58, a transverse stretcher 60, and a reel 62. These elements of the process line 50 are described in more detail below.

[0025] Extruder 52 is usually configured with a single screw or twin screw in a heated barrel, and can accept polymer raw materials in the form of pellets or powders. The raw materials are melted and mixed by extruder 52, and discharged through slot die 54 to provide extruded web 68. In order to assist the process, a melt pump or a metering pump can be used. Slot die 54 does not need to be particularly limited, and can be, for example, a film slot die, an extrusion die, a multilayer slot die, a hot melt extrusion coating die, a drop hammer forging die, a rotary rod die, an adhesive slot die, a solvent coating slot die, a water-based coating die, a slot feed knife die or a knife coater.

[0026] After leaving slot die 54, web 68 is directly arranged on the casting roll in casting roll assembly 56, then web is passed through machine direction stretcher 58, and this machine direction stretcher is along its web downward direction unidirectional stretching web 68.After being stretched along this dimension, web 68 is guided through transverse stretcher 60, and at this transverse stretcher place, the edge of web is clamped by clamp and web is stretched along its web cross direction.Once being fully stretched to required degree along two directions, web 68 just can be finally consolidated into roll via reel 62 as shown in the figure.Optionally, carry out edge trimming step to provide the film of uniform width before film is wound on core.

[0027] In this exemplary process, there are various locations at which the thickness of the web 68 can be measured, which are referred to as metering locations. Figure 1 , an extruded web 68 is conveyed from die 54 to a first metering location 64, and then to a second metering location 66, before being wound into a roll by mandrel 62. The first location 64 captures web thickness information immediately after the extruded web 68 is quenched on the initial casting roll. The second location 66 captures this information after the second stretching step by transverse stretcher 60 is completed and before the web 68 is taken up by mandrel 62. Optionally, location 66 may be after an edge trimming step is performed to give the web 68 a uniform width. If desired, thickness measurements may also be made at intermediate points, such as between the machine direction stretcher 58 and the transverse stretcher 60. Web thickness is directly related to coating weight, and for purposes of this disclosure, the two should be considered similar.

[0028] Metering of the extruded web 68 can be accomplished using any method known in the art. One useful thickness measurement technique uses a beta meter. A beta meter measures the normalized mass of a given web by transmitting web radiation emitted from a radioisotope source (e.g., based on promethium, krypton, or strontium) and detecting the resulting attenuation of the beta particles. The measurement footprint of the beta meter is small, so profile measurements are taken at different locations along a zigzag pattern across the width of the web. These measurements can then be tracked over time to account for time differences in measurements taken along the web. Even after the effects of process conditions have stabilized, a complete profile measurement may require averaging several scans (typically six or more) to average out machine direction variability.

[0029] Alternative metrology methods are also available, including those based on UV fluorescence, infrared absorption, interferometry, direct thickness measurement (such as laser triangulation), reflection methods (such as gamma backscattering), and capacitance-based sensing. Some of these methods are capable of capturing a web thickness profile across the entire width of the web simultaneously. It was determined that applying certain workflows described herein to simultaneously measure coating thickness across its entire width can provide a 4x to 12x improvement in cycle time compared to workflows using conventional scanning-based metrology methods.

[0030] Although not clearly shown here, other process lines are also possible.Some of these process lines do not include one or both of the machine direction stretcher 58 or the transverse stretcher 60. In other embodiments, machine direction stretching and transverse stretching are carried out in the same step. In a further alternative embodiment, the extruder 52 is arranged on the embossed surface by the still molten extruded web to provide a textured surface. When the extruded web passes between the pressure rollers in the casting roll assembly 56, the extruded web can also be arranged on a pre-existing film.

[0031] The process line may include any of a plurality of additional process stations. For example, an oven or other station for drying may be provided to cure the extruded web including the curable composition. Further process steps may include: a surface processing station to provide a corona treated or flame treated surface on the extruded web, or an inspection station to clarify any quality issues. It should be understood that all of these aforementioned variations are within the scope of the present disclosure provided.

[0032] Figure 2 and Figure 3 The slot die 54 is shown in perspective and cross-sectional views, respectively. Figure 3 As shown, the slot die 54 includes a pair of opposing die blocks 100, 102, which together define a path for fluid flow from the extruder to the coating slot 104. The distal end of the die block 100 is provided with a slot adjustment mechanism, here a die lip 106 that defines the surface of the coating slot 104. Although not shown in the figure, the slot adjustment mechanism can alternatively be provided by a choke bar located upstream of the die lip.

[0033] like Figure 2As shown, the slot die 54 includes six primary actuators 108. In some embodiments, the primary actuator 108 represents an assembly of components, including a motor that drives a linear actuator. It may be advantageous for each assembly to include a precision sensor, such as a linear variable differential transformer (LVDT) or a linear encoder, that detects position movement of an output shaft of the linear actuator. Further details related to available actuator assemblies are described in, for example, co-pending PCT patent applications Nos. PCT / IB2020 / 061685 (Yapel et al.), PCT / IB2020 / 061687 (Yapel et al.), and PCT / IB2020 / 061688 (Secor et al.), and U.S. Provisional Patent Application No. 63 / 122,996 (Secor et al.), all of which were filed on December 9, 2020.

[0034] Reference again Figure 2 , each of the six primary actuators 108 is mechanically coupled at its distal end to a plurality of secondary actuators 112. In this embodiment, each secondary actuator 112 is represented by one of a plurality of tines in the fork 110, wherein each tine is individually controllable. Alternatively, a secondary actuator having only a single tine may be used, which may be sufficient for applications where the spacing between the primary actuators 108 provides sufficient resolution in controlling the die lip 106. In preferred embodiments, each fork may include at least 2, 3, 4, 5, 6, 7, or 8 or more tines.

[0035] The distal end of the secondary actuator 112 engages a surface of the die lip 106, allowing local adjustment of the position of the die lip 106. In some cases, the engagement may be a mechanical coupling that allows the secondary actuator 112 to apply both push and pull forces to the die lip 106. Alternatively, the engagement between the secondary actuator 112 and the surface of the die lip 106 may simply be a contact that only allows the application of a push force. In other embodiments, the secondary actuator 112 may engage other surfaces of the slot die 54, such as a choke bar surface.

[0036] Figure 3 The internal features of the slot die 54 are shown in greater detail. As shown, the die blocks 100, 102 of the slot die 54 combine to form a fluid flow channel through the slot die 54 that is in fluid communication with the coating slot 104.

[0037] The primary actuator 108 is secured to mounting brackets 120, 121 along the width of the slot die 54, wherein the mounting brackets 120, 121 are fixed relative to the die block 100 and support the primary actuator 108 and the fork 110, respectively. Each primary actuator 108 is operable to adjust the height of the fluid flow channel at its corresponding location along the width of the slot die 54 by changing the position of the die lip 106 to provide localized adjustment of the fluid flow through the coating slot 104. The body 111 of each fork 110 extends through the mounting bracket 121 (optionally with the aid of a linear bushing) to help reduce buckling or flexing of the fork 110 when force is applied to the die lip 106. In some embodiments, the body 111 of the fork 110 can be coupled to a spindle 122, which is attached to the top of the fork 110 via a shoulder bolt attachment that provides minimal backlash.

[0038] During operation of the slot die 54, the extrudate entering the slot die 54 continues through the fluid flow channel of the slot die 54 before the extrudate exits through the coating slot 104 and is applied to a cooling roll to solidify the melt. Although not germane to the present disclosure, such processes include, but are not limited to, stretching, coating, texturing, printing, cutting, and laminating. In some processes, the production release liner may be removed and a release liner added, or one or more additional layers (such as a laminated transfer tape) may be added. In the case where the extrudate is a curable composition, a curing step may also occur, such as by exposure to an electron beam, an oven, or an ultraviolet (UV) chamber.

[0039] In a preferred embodiment, the primary actuator 108 operates with the assistance of a controller. The controller may receive position inputs from both the motor and the sensor. For example, the motor may be a stepper motor that provides an indication of the number of "steps" the stepper motor has taken from a known reference position of the stepper motor. The sensor may provide more accurate position information to the controller than is provided by the motor. The controller may further provide instructions to the motor to drive the spindle 122 of the primary actuator 108 to a preselected position. For example, the controller may monitor the position spindle 122 of the primary actuator 108 using the sensor 230 while operating the motor 210 so as to position the position spindle 122 of the primary actuator 108 according to the preselected position. In some examples, the controller may control a collection of primary actuators 108 simultaneously or sequentially. For example, the controller may simultaneously control each of the primary actuators 108 in the slot die 54, such as Figure 2 shown.

[0040] Compared to the slot die design using differential bolts as the actuation mechanism, as shown here, a zero-backlash coupling 124 can be used to connect the output shaft 126 to the spindle 122 of the primary actuator 108 with limited or no backlash. To achieve this, the primary actuator 108 can use a position sensor including a linear voltage displacement transducer, a digital scale, a capacitance meter, an optical displacement meter, a laser displacement meter, or a combination thereof to adjust the body 111 of the fork 110 to a precise position. However, since the differential bolt mechanism can have a backlash of more than one hundred microns, the zero-backlash coupling 124 can provide a nearly zero backlash, such as less than ten microns, or even less than five microns, such as about three microns.

[0041] In a slot die that utilizes a collection of differential bolts to control the coating slot width or choke bar position, the relatively large gap of each differential bolt means that adjusting the position of one differential bolt can change the height of the fluid flow channel at the other bolts. For this reason, the absolute position of the die lip 106 may never be known while operating the extrusion die. In contrast, in the slot die 54, the position of the spindle 122 of the primary actuator 108 corresponds directly to the local position of the die lip 106. The details of the actuator assembly are described in more detail, for example, in co-pending International Patent Application No. PCT / IB2020 / 061685 (Yapel et al.). The main advantages include repeatable and precise positioning, which is not available in slot dies utilizing conventional differential bolts.

[0042] Figure 4 An enlarged view of the fork 110 is shown disassembled from the rest of the slot die 54. As shown, the fork 110 is comprised of a series of six tines that serve as independently adjustable secondary actuators 112 extending outwardly from a body 111 toward the die lip 106. Advantageously, each secondary actuator 112 provides its own control zone, allowing for a six-fold increase in precision when controlling the shape of the die lip 106.

[0043] Optionally and as shown, the body 111 and the tines are part of an integral construction. In this example, each tine has a length controlled by thermal expansion and contraction. In order to provide control, each of the tines contains a resistive heating element and has a connection to an electric power source and a thermal sensing device so that the control circuit can heat the tine to a predetermined temperature. These components are partially embedded in the tine to protect them from damage during operation of the slot die 54. The thermal sensing device can be incorporated into a cartridge heater in the tine or attached to the tine. Other means for heating the tine (such as infrared heating) are also possible. As a further option, it is also possible to provide the ability to cool each tine to obtain even better control of the tine temperature and achieve a faster response time. For example, such cooling can be achieved by forced air convection.

[0044] A suitable controller may be used to control the length of each secondary actuator 112, thereby defining the position at which mechanical engagement occurs between the secondary actuator 112 and the die lip 106. The controller may be separate from or integrated with the controller for the primary actuator 108. Available controllers include proportional integral derivative (PID) controllers that apply a control loop mechanism. The length of the secondary actuator 112 is most directly related to the temperature of the secondary actuator 112, but the length may also be controlled based on a predetermined correlation with the power input (i.e., power %) to each secondary actuator 112. The latter approach may be simpler, but tends to be more susceptible to thermal disturbances, which may affect the secondary actuators 112 unevenly.

[0045] The primary and secondary actuators 108, 112 jointly control the position of the die lip 106 based on the mechanical coupling between the distal end of the secondary actuator 112 and the die lip 106. It is noted that the primary and secondary actuators 108, 112 operate in tandem, and therefore, various combinations of actuator settings can provide the same end position of the die lip 106 for a given control zone. However, as will be shown, it may be advantageous to adjust the primary and secondary actuators 108, 112 in a coordinated manner when making slot height adjustments to the coating slot 104.

[0046] Figure 5 An exemplary workflow 150 is shown that uses a single control loop to implement a provided slot die (such as in Figure 1 Slit height adjustment in a slot die 54) operating in the environment of a manufacturing process line 50.

[0047] At the start, the manufacturing process line 50 is used to form an extruded web 68 using predetermined initial primary and secondary actuator setting profiles. These initial profiles may be saved based on historical data based on similar process conditions, or in the absence of such data, may be set to default values ​​based on user input. Thus, the primary and secondary actuators assume initial positions according to these predetermined settings at the start of the control loop. As a starting point, it may be convenient to make the predetermined settings of the primary and / or secondary actuators constant or flat across most or all of the width of the slot die.

[0048] Box 152 shows the first step of providing profile measurements for a web extruded from the coating slit of a slot die. As previously described, any known measurement technique may be used. Profile measurements may be made while cast or after some of the extrudate has been oriented or otherwise altered. In the former case, the measurement of the web thickness profile occurs close to where the extruded web exits the coating slit ("while cast"). Figure 1In, for example, the thickness measurement can be made at location 64 shortly after the molten web solidifies on the cooling rolls of the casting roll assembly 56. In the latter case, the profile measurement occurs after the web has undergone some processing ("at transition"). Figure 1 In , the measurement may be made at location 66 after the cast web has been stretched in both the cross-web direction and the down-web direction.

[0049] Note that many metrology devices scan back and forth across the width of a moving web to collect thickness data. In many cases, these measurements can involve a very large number of discrete measurements that are not only dispersed across the entire width of the web, but also taken at different points in time. To manage this, the controller can process the raw discrete measurements into a smaller number of data values ​​that use a form of cross-web and down-web averaging to capture a virtual snapshot of the cross-web thickness profile at a specific location along the continuous web.

[0050] The provided method can be used for both continuous full-web coated extrudates and strip coated extrudates. In full-web coating, the plurality of measured values ​​represent the entire coating width. In the case of strip coating, the measured thickness values ​​correspond to a plurality of coated areas spaced apart from each other in the cross-web direction, such that the measured values ​​cover only the coated strips and not the uncoated channels therebetween.

[0051] Box 154 represents the next step of performing a web-to-die mapping of these profile measurements. When mapping the gage measurements to the die, certain simplifying assumptions may be made. First, assuming that modern metrology systems have edge detection, it may be assumed that the data received from the profile measurements are taken from edge to edge. Second, it may be assumed that the gage data corresponds directly to the actual extrudate weight / thickness. If the web is disposed on a release liner, it may be further assumed that the basis weight of the release liner is subtracted and the data represents the coating amount only. Finally, it may be assumed that any necking from both edges of the extruded web occurs symmetrically.

[0052] The number and location of the coarse-grained measurements are typically different from the number and location of the die lip actuators, and therefore, a generalized method of mapping the measurement values ​​to the actuator positions is needed. Film necking calculations can take into account the effects of different flow rates, pull distances, and web speeds. In one embodiment, the coated web coordinates in physical units (inches or mm) are mapped to coordinates in actuator units (i.e., a mold coordinate system based on sequential actuator numbers). This process enables mapping from the coating measurement array values ​​to the physical coating web positions, and then to the physical mold positions through the web-to-mold mapping function. Here, the coating measurement array can represent, for example, the most recent thickness measurement array generated whenever a scanner traverses a moving web.

[0053] With an appropriate die-to-web or web-to-die mapping function, it may be advantageous to utilize the function elsewhere in the profile control scheme. For example, the mapping may incorporate cross-web variations in control parameters, such as controller gains or actuator interactions through the coating flow field. This may be done in an ad hoc manner based on production experience, or in a more scientific manner using a fluid dynamics model of the coating flow field.

[0054] Modeling of the flow may utilize any appropriate model that characterizes the rheological properties of the fluid. For example, the flow modeling step may include finite element analysis or may rely more directly on one or more formulas. Exemplary mathematical models are described elsewhere in co-pending PCT Application No. PCT / IB2020 / 061688 (Secor et al.), filed December 9, 2020.

[0055] Computational predictions of slot die adjustments are possible because the position of the actuator and, by inference, the slot height in combination with the desired extrudate target thickness, the current measured extrudate thickness, is known. Previously, the absolute position of the slot height during the extrusion process has not been known, for example due to play in differential bolts. Using the known target thickness and the measured extrudate thickness profile, these calculations can predict appropriate slot die changes. Based on this knowledge, the relationship between the slot height profile and the extrudate thickness profile is known, and the slot height profile can therefore be predicted to achieve the target thickness profile.

[0056] In some embodiments, this mapping combines any scan position to die bolt position mapping already built into the measurement system.Various commercial systems are capable of performing web-to-die mapping, such as the Contour Control Solution from NDC Infrared Engineering Inc. of Irwindale, California.

[0057] Proceeding to block 156, the profile deviation of the web thickness is then determined. This may be provided by an array of residual values ​​(i.e., a vector) representing the extent to which the current web thickness profile deviates from the target web thickness profile (block 158) at each control zone. As mentioned herein, the control zone may correspond to a section of the slot die corresponding to each primary actuator or, alternatively, each secondary actuator.

[0058] The initial target profile in block 158 may be defined near the location of the extrudate exiting the slot die (e.g., at Figure 1 ), or alternatively at a downstream location from which the web has been partially or completely transformed (e.g., at Figure 1 Combining these two types of measurements to fully understand and correct for deviations between the desired web thickness profile and the actual web thickness profile attributable to different sources in the process line 50 can have significant technical benefits.

[0059] In subsequent iterations of the workflow 150, the profile deviation determined in block 156 may be based on the initial target web thickness profile set in block 158, or, if necessary, based on a revised target web thickness profile. The revisions to the target web thickness profile are not particularly limited and may be made in a predetermined manner according to a computer algorithm or manually through input from an operator.

[0060] When workflow 150 is initially executed, the target web thickness profile may be based on a saved web thickness profile, such as a web thickness array used in a previous iteration of workflow 150 or other workflows performed under similar conditions. For example, a previously used target web thickness profile may be available when the same or similar die slot configuration and similar flow conditions through the slot die are being used. In many applications, a flat extrudate profile is desired, but there are situations where other profiles are preferred. For example, a "dog bone" shaped target profile may be needed to control edge instabilities in an extrusion process, such as those associated with pull resonance or edge fanning.

[0061] In block 156, a profile deviation is then determined based on the difference between the initial target web thickness profile from block 158 and the measured web thickness profile (if available). An initial iteration of the control loop in the workflow 150 may be performed before a complete set of web thickness measurements are available. If a measured web thickness profile is not yet available, adjustments in the slot die may be delayed until such time that a sufficient number of web thickness measurements exist. To the extent that partial profile measurements are available (block 152), the workflow 150 may be used to adjust the slot die along one portion of the coating slot but not another portion.

[0062] Using the profile deviation thus determined, the appropriate slot height adjustment can then be calculated (block 160). When predicting adjustments to the primary or secondary actuators engaged to the flexible die lip or choke bar suitable for achieving the initial target profile from block 158, it can be advantageous to apply a pressure die deflection model that enables the effects of fluid flow through the die to be decoupled from the mechanical effects associated with the slot die in the absence of fluid flow. A suitable model can predict the pressure profile across the coating slot and the corresponding amount of pressure deflection in the flexible die lip or choke bar. In some cases, this pressure-based deflection can be measured empirically.

[0063] The pressure deflection can be accounted for by adding it to the calculated slot height to obtain a target slot height profile. The target slot height profile can then be compared to the current slot height profile (block 162) to determine the appropriate adjustment. It is noteworthy that the current slot height includes a certain degree of pressure deflection (D) due to the flow of the extrudate composition through the coating slot. Therefore, assuming that any change in the amount of deflection D is small, the deflection D attributable only to the fluid can be subtracted from the pressure compensated slot height profile H+D to obtain a zero pressure slot height profile (H), which can then be used to calculate the target actuator position.

[0064] Mathematical models describing the fluid dynamics and pressure effects in the slot die are described in detail elsewhere, for example, in co-pending International Patent Application No. PCT / IB2020 / 061688 (Secor et al.) and U.S. Provisional Patent Application No. 63 / 122,996 (Secor et al.), both filed on December 9, 2020.

[0065] Using the zero-pressure slot height profile obtained above, the controller can then predict a set of discrete actuator settings suitable for achieving the desired slot height profile. In a preferred embodiment, the set of discrete actuator settings is based on a plurality of actuator settings corresponding to preselected cross-web profiles. As will be described below, the plurality of discrete actuator settings can be determined for a range of preselected cross-web profiles, thereby providing a predictive model to determine appropriate actuator adjustments (block 164).

[0066] In a preferred embodiment, predictions of discrete settings from the plurality of discrete settings and / or the current slot height at zero pressure (block 162) as derived from the current slot height can be obtained by a mathematical construct known as a stiffness matrix. The stiffness matrix converts actuator settings into corresponding slot height profiles in the absence of flow field physics effects. Although not examined in detail here, International Patent Publication No. WO 2012 / 170713 (Secor et al.) describes in more detail an example of how empirical test data can be used to populate a stiffness matrix for a given slot die.

[0067] At a high level, the stiffness matrix and the inverse stiffness matrix are used to convert actuator position changes to slit height changes and vice versa. The stiffness matrix can be represented by Equation 1 and Equation 2 below.

[0068]

[0069]

[0070] In Formula 1 and Formula 2, h0 and h are vectors representing the current slit height and the new slit height, respectively, A and A0 are vectors representing the current actuator position and the new actuator position (in the actuator unit), respectively, K is the stiffness matrix, I is the identity matrix, and k is the proportional constant that converts the actuator position change into the slit height change and is the same for each actuator.

[0071] The stiffness matrix K usually has N×N components (N is the total number of active actuators) and physically represents the stiffness due to the jth actuator setting A j The stiffness matrix can reflect the significant mechanical interactions between the actuators. Typically, changes in actuator position can produce changes in slit height at locations other than several actuators. In some embodiments, this is represented by a band stiffness matrix. In many cases, it can be assumed that the band stiffness matrix is ​​symmetrical. For example, the matrix may have significant non-zero components only along the 5 diagonals of the matrix (the main diagonal plus 2 diagonals on both sides).

[0072] Once the stiffness matrix is ​​determined, the slit height measurements can be used in two ways. First, for any set of actuator settings, the resulting slit height profile can be calculated by multiplying the stiffness matrix by the actuator displacement according to Equation 1 and Equation 2 above. Second, the actuator settings that will result in a specified slit height profile are calculated by multiplying the inverse of the stiffness matrix by the desired change in slit height. To determine the appropriate set of actuator adjustments, use Equation 3:

[0073] (A-A0) = K -1 (h-h0) (Formula 3)

[0074] In block 164, the active actuators may then be adjusted to the appropriate positions based on the actuator adjustments calculated above to achieve the desired slot height profile. In a preferred method for solving this linear algebra problem, Gaussian elimination is performed to obtain a matrix-based solution to the stiffness matrix transformation.

[0075] like Figure 5 As shown, the actuator adjustment in block 164 may be applied to the primary actuator, the secondary actuator, or both. In the case where the primary actuator is being adjusted, the secondary actuator may remain passive so that the tines of each fork move together rather than individually. In the case where the secondary actuator is being adjusted, the primary actuator may be fixed (or passive) while the secondary actuator is being adjusted. As a third possibility, and as will be discussed later in Figure 7 As described in , it is possible and may in fact be advantageous for both the primary actuator and the secondary actuator to be adjusted simultaneously.

[0076] With the actuator adjustments complete, the workflow 150 returns to block 152 where new profile measurements are taken and the process described above begins again. The steps in the workflow 150 can gradually improve the primary / secondary actuator settings / positions based on real-time web thickness measurements. Over time, through these gradual adjustments, the extrudate web thickness can converge to the desired target web thickness profile.

[0077] As the polymer melt is conveyed along the fluid flow path and discharged from the coating slot 104, the Figure 2 and Figure 3 164. Here, the controller predicts settings for one or both sets of primary actuators 108 and secondary actuators 112 to incrementally push or pull the die lip 106 at each of a plurality of control zones along the coating slot 104 according to the actuator adjustments determined in block 164. Because each primary actuator 108 corresponds to six secondary actuators 112, it is efficient for the controller to predict primary actuator settings to obtain a coarse-scale target slot height profile and then predict secondary actuator settings to obtain a finer-scale target slot height profile.

[0078] In some embodiments, the position of the primary actuator is determined based on the corresponding target primary actuator position, and then the position of each secondary actuator corresponding to the primary actuator is determined based at least in part on the target primary actuator position. Advantageously, the target primary actuator position can be determined or adjusted to reduce the change in the length control signal in the secondary actuator. Although the length control signal for the secondary actuator is temperature here, other length control signals are possible, including power, piezoelectric voltage, or hydraulic pressure.

[0079] Figure 6 An alternative workflow 250 using nested control loops is shown. Workflow 250 combines some of the elements already described in workflow 150, including: casting profile measurement (box 252), web-to-die mapping (box 254), determination of profile deviation (box 256) based on an initial target casting profile (box 258), determination of slot height adjustment (box 260) based on a current slot height (box 262), and actuator adjustment (box 264). These steps that make up the inner control loop are similar to those examined above in workflow 150 and should not be revisited.

[0080] Workflow 250 also includes an outer control loop. The loop begins with box 266, where a transformed profile measurement is provided. This transformed profile measurement, taken downstream from the casting profile measurement (box 252), can occur at any time during the execution of the inner control loop. Therefore, the steps in the inner and outer loops do not need to coincide with each other.

[0081] Box 268 represents a web-to-die mapping step performed for the transformed profile measurements in box 266. The web-to-die mapping for the transformed web thickness profile may be more complex than the web-to-die mapping performed in box 254. In process line 50, for example, the action of machine direction stretcher 58 and transverse direction stretcher 60 essentially stretches the extruded film. Assuming these processes provide predictable and repeatable results, a mathematical model may be used to map the cross-web coordinate system after transformation to the cross-web coordinate system of the extruded web before its transformation.

[0082] Where there are multiple conversion processes, a series of mapping calculations are typically used to map the converted web thickness profile back to the slot die in a step-wise manner. In a preferred embodiment, the converted profile is mapped back to the casting profile, and then the casting profile is mapped back to the die, the latter step following the same process as described above for the web-to-die mapping step of block 254. For example, in Figure 1 The measured profile at position 66 can be mapped to the profile at position 64 and then mapped back to the profile at the mold 54. Conveniently, this allows the calculation algorithm from box 254 to be reused.

[0083] Proceeding to block 258, the target casting profile for web thickness may then be updated accordingly based on instructions from the controller. This casting profile replaces the previously used target casting profile. Similar to those mentioned above, useful controllers may include a PID controller that applies iterative, incremental changes to gradually improve the target casting profile represented by block 256 before reaching the desired transformed profile. When the inner and outer loops are operated simultaneously, the outer loop provides feedback on a much longer cycle time because the impact of changes set by the actuators cannot be known until the extruded web has traveled through the entire transformation process.

[0084] The outer loop and the inner loop preferably complement each other in a coherent optimization scheme. The inner loop is based on a first web thickness profile measured at a first location of the extruded web, wherein a target slot height profile remains constant for at least some iterations of the inner loop. The outer loop is based on a second web thickness profile measured at a second location of the extruded web downstream of the first location, and the target slot height profile is updated at each iteration of the outer loop. Thus, the inner loop operates on a short time frame and continuously adjusts the primary / secondary actuator settings seeking to converge to the target profile, while the outer loop operates on a longer time frame to periodically adjust the target profile "tracked" by the inner loop.

[0085] Figure 7 Yet another exemplary workflow 350 is shown, which illustrates a process such as Figures 2 to 4The interactions between the actuators of the primary and secondary actuators 108, 112 are shown. At the outset, it is noted that a number of interesting complications are introduced by having two actuators coupled end-to-end to each other. First, a single target web thickness profile may correspond to an indefinite number of solutions, since a lengthening of one actuator may be accompanied by a shortening of another actuator. Second, where a primary actuator is coupled to multiple secondary actuators, the range of possible positions of the secondary actuators is typically constrained by the position of the primary actuator. Third, in many cases, the primary and secondary actuators may have very different response times. Finally, in some cases, adjacent actuators may be subject to interference based on their proximity to each other, such as interference caused by heat transfer.

[0086] Some of these considerations are considered in workflow 350, which is similar to the previous workflows, including: web thickness profile measurement of the converted web (box 366), followed by web-to-die mapping of the profile (box 352), determination of profile deviation (box 356) relative to a target profile (box 358), and determination of slot height adjustment (box 360) relative to the current slot height (box 362). At box 361, an analysis is performed by the controller based on whether the following conditions are met:

[0087] |Dx|>d x

[0088] , where x is the length control signal of the primary actuator, Dx is the proposed actuator adjustment, and d x is a predetermined threshold value for the change in x that is related to the resolution of the primary actuator.

[0089] exist Figures 2 to 4 The actuator adjustment Dx presented in the exemplary configuration of can be determined by calculating the difference between the average tine temperature for a given fork 110 and the average target tine temperature for the same fork 110. Because the partial thermal expansion or contraction of the tines (secondary actuator 112) is linearly related to changes in temperature, this measurement is directly related to the change in actuator length.

[0090] The desired length control signal x may be calculated according to any of the aforementioned methods, such as by using the inverse stiffness matrix determined from bump test data, and optionally taking into account pressure effects caused by fluid flow in the slot die. x Reflects the primary actuator deadband, or the range of the length control signal is too small to be resolved by the primary actuator, but can be resolved by its coupled secondary actuator.

[0091] If the magnitude of the proposed actuator adjustment Dx is equal to or less than the threshold d x, the secondary actuator 112 is adjusted accordingly (block 364), and the process begins again with the transformed profile measurement (block 366). Here, the adjustment is made solely by the secondary actuator 112, with the primary actuator 108 position remaining stationary. Conversely, if the proposed actuator adjustment Dx is greater than the threshold value d x , then both the primary actuator and the secondary actuator are adjusted (block 365 ), as will be described in more detail below.

[0092] Illustrative examples are provided by Figure 3 108, 112 in which the primary actuator is moved using a helical differential coupling and the secondary actuator is moved by thermal expansion and contraction. More generally, the primary actuator may be driven by mechanical, thermally adjustable bolts, piezoelectric, hydraulic or pneumatic devices. Preferably, the primary actuator and the secondary actuator are adjusted in a coordinated manner. Optionally, both the primary actuator and the secondary actuator are adjusted simultaneously to provide a smoother adjustment of the overall actuator position.

[0093] In an exemplary primary actuation mechanism, the coating slot can be adjusted by applying a compressive load or a tensile load to the flexible die lip using a lever supported by a rotating shaft as a fulcrum and an operating rod displaced in the axial direction by the main body of the slot die. The rotational force of the lever is converted into a force in the axial direction of the operating rod, and the force in the axial direction becomes a compressive load or a tensile load acting on the flexible die lip. The lever can directly apply a force to the operating rod at the point of action of the lever.

[0094] In another exemplary primary actuation mechanism, a thermally adjustable bolt automatically adjusts the coating gap using a plurality of adjustment pins coupled to corresponding thermoelectric elements disposed on the flexible die lip. The thermoelectric element may be controllable by a controller to adjust the coating gap by the action of mechanical forces applied to the flexible die lip by the corresponding adjustment pins through expansion or contraction of the thermoelectric element. As a further option, the actuation mechanism may include providing at least two adjustment pins and / or thermoelectric elements that are adjusted simultaneously.

[0095] Further aspects of the above and other variations are described in U.S. Pat. No. 9,700,911 (Nakano) and International Patent Publication No. WO 2019 / 219724 (Colell et al.).

[0096] A preferred embodiment of the above-mentioned coordinate adjustment includes using a primary actuator with a longer actuation stroke to provide most of the overall movement. The overall movement is based on the distal end of the secondary actuator used for each control zone. If multiple secondary actuators are connected to each primary actuator, the primary actuator adjustment can be calculated based on adjusting each primary actuator to a target position, which is calculated based on the average target position of its corresponding secondary actuator. Averaging can help avoid expanding or contracting the secondary actuator more than necessary. Using certain secondary actuators (such as hot bolts) to make large adjustments is not only technically challenging, but also may take a long time to implement and stabilize. This in turn can adversely affect the overall responsiveness of the control loop in the workflow 350.

[0097] The benefits of the above method are Fig. 8A and Figure 8B , which shows the primary and secondary actuators 108, 112 in two different configurations. The depicted configurations show the same final position, but with very different relative contributions from the primary and secondary actuators 108, 112. Fig. 8A In FIG. 1 , the secondary actuator 112 (grey shading) shows a significant change in length, which results in the secondary actuator 112 being heated to a very different temperature. In contrast, in Figure 8B In the latter case, the primary actuator 108 accurately compensates for the difference in length of the secondary actuator 112 by translating toward or away from the die lip as indicated by the block arrows.

[0098] While preserving the die lip position, redistribution of the length between the secondary actuator (i.e., tines) and the primary actuator (i.e., forks) can be achieved by adjusting these actuators by applying Equations 4 and 5:

[0099]

[0100] , where T 新 is the new tine temperature, T 旧 is the temperature of the old tine, is the average measured tine temperature within the fork, and is the average target tine temperature within the fork.

[0101]

[0102] , where A 新 is the new primary actuator position (in actuator settings), A 旧 is the old primary actuator position, and Y is the fixed conversion factor between temperature and actuator setting.

[0103] The uniform distribution of temperature can help minimize thermal disturbances caused by heat transfer between the secondary actuators 112 and to the flexible die lip of the slot die. Thermal disturbances reduce the predictability of the extrusion process and are generally considered undesirable. In a preferred embodiment, the average of the target tine temperatures for all secondary actuators 112 corresponds to the operating temperature of the slot die to further reduce the degree of undesirable heat transfer between the tines and the flexible die lip.

[0104] With the primary actuator settings recalibrated as described above, the net result is a reduced temperature change in the secondary actuator 112 while providing the same profile of actuator position, as shown by comparing Fig. 8A and Figure 8B Because the primary actuator 108 can respond much faster than the thermally controlled secondary actuator 112, it may be beneficial for the primary actuator 108 to be adjusted gradually to allow time to position the secondary actuator 112 and avoid sudden actuator length changes when manufacturing the product.

[0105] Now return to reference Figure 7 , the adjustment of the primary and secondary actuators in block 365 may then be completed. After this, a new transformed profile measurement may then be obtained (block 366) and the process begins again.

[0106] Fig. 9 Yet another workflow 450 is shown that combines elements of the previous workflows 150, 250, 350. As previously described, the process includes: casting profile measurement (box 452), web-to-die mapping (box 454), determination of profile deviation (box 454), and determination of appropriate slot height adjustment (box 460) using knowledge of the current slot height (box 462). Then, as previously described in the workflow 350, the test of box 461 is applied to determine whether a specific threshold for primary actuator adjustment is met. Depending on whether this test condition is met, the workflow 450 either continues to adjust the secondary actuator alone (box 464) or adjusts the primary and secondary actuators together (box 465).

[0107] The added refinement in workflow 450 is a combination of an inner control loop and an outer control loop. Thus, when the controller makes actuator adjustments based on cast profile measurements (block 452), there are also actuator adjustments based on the transformed profile measurements (block 466), requiring web-to-die mapping (block 468) and calculation of an updated target cast profile (block 458). These steps are similar to those in Figure 6. Unlike workflow 350, workflow 450 includes adjustments based on cast profile measurements, which have a much shorter response time. Combining both the inner control loop and the outer control loop can provide faster convergence on a solution and an overall significantly more responsive and efficient slot die adjustment process.

[0108] Fig.10 A practical example of a dashboard for a hybrid actuator control system is provided showing the temperature profile across 88 actuator control zones represented along the horizontal axis. In the example shown, the set point for the mold temperature is 240°C. Fig.10 The top graph in shows the tine temperature for each control zone. The bottom graph shows the % of power directed to each tine, which illustrates the non-uniformity of the power distribution going into the different control zones, particularly when comparing the center actuator to those closer to the coating slot edge. The non-uniformity can be attributed to differences in airflow in the tine cooling plenum; in this case, the graph reveals higher cooling rates near the center of the die slot compared to the ends. These data further demonstrate that the hybrid actuator control scheme is able to keep the average temperature of the tine close to the target average temperature, fork by fork.

[0109] Fig.11 and Fig.12 Significant technical benefits provided by a hybrid actuator control scheme are shown. Fig.11 The (Prior Art) graph shows the extruded web thickness profile over 144 control zones (corresponding to a 1 inch (2.54 cm) width of finished film) using a conventional control scheme using an EDI brand die (available from Nordson Extrusion Dies Industries LLC, Chippewa Falls, Wisconsin) with a 38 inch (965.2 mm) wide slot using heat bolts spaced 1.125 inches (31.115 mm) apart. Fig.12 The extruded web thickness profile of a hybrid die with a 965 mm wide slot with 16 primary actuators spaced 60 mm apart, each equipped with a fork comprising secondary actuators spaced 6×10 mm apart as tines, within the provided hybrid control scheme is shown. These data were collected during the manufacture of a full roll of extruded web. The center line shows the average thickness, and the dashed lines show the boundaries of two standard deviations (i.e., ±2s) from the average web thickness.

[0110] Fig.12 The data in the Figure 5 The workflow 150 described in the method is collected, where the primary actuator is adjusted while keeping the secondary actuator passive, and then transitions to Figure 6 The dual control loop workflow 250 converges towards steady-state operation simultaneously. As can be seen in these figures, the envelope of web thickness values ​​is significantly narrower when using the provided hybrid actuator control method compared to conventional methods.

[0111] The techniques described in the present disclosure may be implemented, at least in part, in hardware, software, firmware, or any combination thereof. For example, various instances of the techniques may be implemented within one or more microprocessors, digital signal processors (DSPs), application specific integrated circuits (ASICs), field programmable gate arrays (FPGAs), or any other equivalent integrated or discrete logic circuits, and any combination of such components embodied in a controller, user interface, or other device. The term "controller" may generally refer to any of the above logic circuits, alone or in combination with other logic circuits, or any other equivalent circuits.

[0112] When implemented in software, the functionality attributed to the systems and controllers described in this disclosure may be embodied as instructions on a computer-readable storage medium such as random access memory (RAM), read-only memory (ROM), non-volatile random access memory (NVRAM), electrically erasable programmable read-only memory (EEPROM), flash memory, magnetic media, optical media, etc. The instructions may be executed to cause one or more processors to support one or more instances of the functionality described in this disclosure.

[0113] Various examples have been described in the preceding paragraphs. These and other examples are within the scope of the claims provided herein.

[0114] All references, patents and patent applications cited in the above patent applications are incorporated herein by reference in their entirety in a consistent manner. In the event of inconsistency or conflict between the incorporated references and the present application, the information in the foregoing description shall prevail. The foregoing description, which is given to enable a person of ordinary skill in the art to practice the present disclosure protected by the claims, should not be construed as limiting the scope of the present disclosure, which is defined by the claims and all equivalents thereof.

Claims

1. A method for adjusting a slot die, the slot die comprising: a coating slot extending across a width of the slot die, the coating slot being in fluid communication with a fluid flow channel through the slot die; an adjustment mechanism, the adjustment mechanism comprising a slot die surface; and a plurality of primary actuators spaced apart along a width of the slot die, wherein each primary actuator is operably coupled to one or more secondary actuators, and each secondary actuator is operably coupled to the adjustment mechanism to adjust a cross-sectional height of a fluid flow channel at a respective location thereof, thereby providing localized adjustment of fluid flow through the coating slot, The method comprises: determining a target slit height profile; predicting, with a controller, a set of primary actuator settings and a set of secondary actuator settings based on the target slot height profile; and Each primary actuator and secondary actuator is individually positioned according to the predicted set of primary actuator settings and the set of secondary actuator settings to adjust the slot die.

2. The method of claim 1, wherein the primary actuator and the secondary actuator together comprise a fork having a plurality of tines, and further wherein each tine is individually controllable.

3. The method of claim 2, wherein each primary actuator comprises: The fork-shaped member has a main body portion, and a mechanical, piezoelectric, hydraulic or pneumatic device capable of driving the main body portion.

4. The method of claim 3, wherein the main body portion is positioned by a position sensor, the position sensor comprising a linear voltage displacement transducer, a digital scale, a capacitance meter, an optical displacement meter, a laser displacement meter, or a combination thereof.

5. A method according to any one of claims 1 to 4, wherein each secondary actuator comprises a tine which is controllable by heating the tine.

6. The method of claim 5, wherein the tines are heated to a predetermined temperature.

7. The method of claim 5, wherein heat is applied to the tines by resistive and / or infrared heaters.

8. The method of claim 5, wherein positioning each tine further comprises cooling at least one tine.

9. The method of claim 8, wherein the at least one tine is cooled by forced air convection.

10. The method of any one of claims 1 to 4, wherein positioning each primary actuator and secondary actuator comprises: determining a position of the primary actuator based on a corresponding target primary actuator position; as well as A position of each secondary actuator corresponding to the primary actuator is determined based at least in part on the target primary actuator position.

11. The method of claim 10, wherein the target primary actuator position is determined to reduce a variation in a length control signal in the secondary actuator.

12. The method of claim 11, wherein the length control signal comprises temperature, power, piezoelectric voltage or hydraulic pressure.

13. The method of claim 10, wherein the method is performed iteratively according to a control loop to gradually improve the positioning of each primary and secondary actuator.

14. The method of claim 13, wherein the control loop comprises: an inner loop based on a first web thickness profile measured at a first location on an extruded web, wherein for at least some iterations of the inner loop, the target slot height profile remains constant; and An outer loop is based on a second web thickness profile measured at a second location of the extruded web, the second location being downstream from the first location, wherein the target slot height profile is updated at each iteration of the outer loop.

15. The method of claim 14, further comprising conveying the extruded web between the first location and the second location.

16. The method of claim 13, wherein positioning of the primary actuator and the secondary actuator occurs simultaneously in each iteration of the control loop.

17. The method of claim 13, wherein the primary actuator is positioned according to a predetermined setting at the start of the control loop.

18. The method of claim 13, wherein the secondary actuator is positioned according to a predetermined setting at the start of the control loop.

19. The method of claim 17, wherein the predetermined setting of the primary actuator is constant across a width of the slot die.

20. The method of claim 18, wherein the predetermined setting of the secondary actuator is constant across a width of the slot die.

21. A system, comprising: A slot die, wherein the slot die comprises: a coating slot extending across a width of the slot die, wherein the coating slot is in fluid communication with a fluid flow channel through the slot die; an adjustment mechanism comprising a slot die surface for adjusting a cross-sectional height of a fluid flow channel through the coating slot; and a plurality of primary actuators spaced apart along a width of the slot die surface, wherein each primary actuator is operably coupled to one or more secondary actuators, and each secondary actuator is operably coupled to the adjustment mechanism to adjust a cross-sectional height of a fluid flow channel at a respective location thereof, thereby providing localized adjustment of fluid flow through the coating slot; and A controller is provided that is capable of independently setting the position of each primary actuator and each secondary actuator.

22. The system of claim 21, wherein the primary actuator and the secondary actuator together comprise a fork having a plurality of tines, and each primary actuator comprises a body portion of the fork and each secondary actuator comprises the tines.

23. The system of claim 22, wherein the position of the main body portion is aided by a position sensor comprising a linear voltage displacement transducer, a digital scale, a capacitance meter, an optical displacement meter, a laser displacement meter, or a combination thereof.

24. The system of any one of claims 22 or 23, wherein the fork has three or more tines.

25. The system of any one of claims 22 to 23, wherein the slot die further comprises a mounting bracket, wherein each body portion extends through the mounting bracket to reduce deflection of the body portion.

26. The system of any one of claims 21 to 23, wherein the slot die is selected from the group consisting of: an extrusion die, a drop hammer forging die, a rotating rod die.

27. The system of any one of claims 21 to 23, wherein the slot die is a film slot die.

28. The system of any one of claims 21 to 23, wherein the slot die is a multi-layer slot die.

29. The system of any one of claims 21 to 23, wherein the slot die is a hot melt extrusion coating die.

30. The system of any one of claims 21 to 23, wherein the slot die is an adhesive slot die.

31. The system of any one of claims 21 to 23, wherein the slot die is a solvent coating slot die.

32. The system of any one of claims 21 to 23, wherein the slot die is a water-based coating die.

33. The system of any one of claims 21 to 23, wherein the slot die is a slot-fed knife die.

34. The system of any one of claims 21 to 23, wherein the slot die is a knife coater.

Citation Information

Patent Citations

  • Die lip driving structure

    US9700911B2

  • Slot die position adjustment

    WO2012170713A1

  • Method for automatically regulating the size of a slot of a nozzle assembly and control and / or regulation system

    WO2019219724A1

  • Adjustment method for thickness of sheet film in t-die forming

    JP1998058518A

  • Wide slot die

    US5626888A