A bonding resin for nylon / polyethylene composite pipes, its preparation method and application
By preparing composites of polar monomer-grafted polyethylene and nylon elastomers with styrene-maleic anhydride copolymers, the problem of insufficient bonding strength in nylon/polyethylene composite pipes was solved, achieving high-strength chemical bonding and material compatibility, and meeting the peel strength requirements between composite layers.
Patent Information
- Application Number
- CN202311032501.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-08-16
- Publication Date
- 2026-11-17
- Estimated Expiration
- 2043-08-16
AI Technical Summary
The bonding strength of existing nylon/polyethylene composite pipes is insufficient, failing to meet the requirement of a peel strength greater than 10 N/mm between composite layers. Furthermore, existing adhesive resins have poor compatibility with nylon materials of different structures.
A bonding resin with excellent wettability and good adhesion was prepared by reacting and blending polyethylene, nylon elastomer, styrene-maleic anhydride copolymer and functional additives grafted with polar monomers at a specific temperature using a twin-screw extruder. High-strength bonding was achieved by utilizing the chemical reaction between the polar monomers and nylon.
It achieves high-strength bonding of nylon/polyethylene composite pipes, with a 180° peel strength greater than 12 N/mm and a cohesive failure peel state, improving the compatibility of nylon materials with different structures and providing stable bonding effect.
Smart Images

Figure BDA0004397798190000081 
Figure BDA0004397798190000102 
Figure BDA0004397798190000121
Abstract
Description
Technical Field
[0001] This invention belongs to the field of adhesive resins, specifically relating to an adhesive resin for nylon / polyethylene composite pipes, its preparation method, and its application. Background Technology
[0002] The information disclosed in this background section is intended only to enhance understanding of the overall background of the invention and is not necessarily to be construed as an admission or in any way implying that such information constitutes prior art known to those skilled in the art.
[0003] Polyamide, commonly known as nylon, is a polymer containing amide groups in its main chain. Nylon possesses excellent mechanical properties, high-temperature resistance, wear resistance, and good barrier properties against small molecules such as oxygen and hydrogen. However, it also has drawbacks such as temperature sensitivity, high water absorption, and high cost. Polyethylene has excellent toughness, water resistance, and low cost, but it suffers from poor heat resistance and poor barrier properties against small molecules such as oxygen and hydrogen. Polyethylene plastic pipes are currently commonly used in municipal and gas pipelines. However, they are prone to wear in high-friction industrial and mining applications involving the transportation of mineral slurries, and they have insufficient barrier properties when transporting hydrogen, a new energy source. By combining nylon and polyethylene to create a composite pipe with a nylon core and a polyethylene outer layer, the wear resistance and small molecule barrier properties of nylon can be combined with the excellent toughness and low cost of polyethylene, thus expanding the application areas of plastic pipes.
[0004] However, nylon is a polar material, while polyethylene is a non-polar material, and the difference in polarity between the two is significant. No reports have been found of high-strength adhesive resins suitable for nylon / polyethylene composite pipes. Patent CN104449469A discloses a polyethylene adhesive resin for barrier packaging. Its raw material formulation includes: 40%-80% high-density polyethylene, 10%-30% functionalized modified high-density polyethylene, 15%-30% vinyl elastomer, 1%-10% ethylene-vinyl acetate copolymer, and 0.01%-1% thermo-oxidative stabilizer. This adhesive resin is used as the adhesive layer in multilayer co-extruded barrier packaging films (sheets) of polyethylene (PE) / nylon (PA), and its peel strength against PE / nylon is 36-37 N / 15 mm. Patent CN112851861A discloses a compatible adhesive resin for PE and PA, comprising the following components in parts by weight: 40-60 parts polyethylene, 20-50 parts ethylene copolymer, 0.1-5 parts polar monomer, 0.1-2 parts initiator, and 0.1-2 parts coupling agent. This compatible adhesive resin exhibits a peel strength of 134-178 N / 25 mm for PE / PA. It is evident that the existing adhesive resins for bonding PA / PE exhibit relatively low peel strength, failing to meet the requirement of a peel strength greater than 10 N / mm between composite layers in composite pipes. Summary of the Invention
[0005] To address the shortcomings of existing technologies, the present invention aims to provide an adhesive resin for nylon / polyethylene composite pipes, its preparation method, and its application. The adhesive resin provided by the present invention, through the combination of its components, exhibits excellent wettability and good adhesion to nylon and polyethylene, two polymers with significantly different polarities. The 180° peel strength for bonded PA / PE is greater than 12 N / mm, and the peel state of bonded PA / PE is cohesive failure.
[0006] To achieve the above objectives, the technical solution of the present invention is as follows:
[0007] In a first aspect, the present invention provides an adhesive resin for nylon / polyethylene composite pipes, wherein the adhesive resin for nylon / polyethylene composite pipes, by weight, comprises the following raw materials: 20-30 parts of polyethylene grafted with polar monomers, 10-40 parts of nylon elastomer, 25-65 parts of polyethylene, 5-15 parts of styrene-maleic anhydride copolymer, and 0.5-1 parts of additives.
[0008] The polar monomer-grafted polyethylene is prepared by reactive extrusion of 90-97 parts high-density polyethylene, 3-10 parts ethylene propylene diene copolymer (i.e. ethylene propylene diene monomer rubber EPDM), 1.5-2.5 parts polar monomer and 0.02-0.10 parts peroxide initiator using a twin-screw extruder at 220-280°C.
[0009] A second aspect of the present invention provides a method for preparing the above-mentioned adhesive resin for nylon / polyethylene composite pipes, the method comprising the following steps:
[0010] The polar monomer-grafted polyethylene, nylon elastomer, polyethylene, styrene-maleic anhydride copolymer, and functional additives are mixed in proportion and then reacted, blended, and granulated using a twin-screw reactive extruder at 180-210℃ to obtain the final product.
[0011] A third aspect of the present invention provides the application of the above-described adhesive resin for nylon / polyethylene composite pipes in bonding the nylon layer and the polyethylene layer in a composite pipe.
[0012] The beneficial effects of this invention are as follows:
[0013] (1) The adhesive resin for nylon / polyethylene composite pipes of the present invention incorporates nylon elastomers. Through the interaction between the anhydride and carboxyl groups on the polyethylene grafted with polar monomers and the amide groups on the nylon elastomers, a blending composite of polar nylon elastomers and non-polar polyethylene is achieved. Furthermore, by introducing nylon elastomers containing amide hard segments, the compatibility of the adhesive resin with nylon materials of different structures, such as nylon 6, nylon 6,6, nylon 11, and nylon 12, used in the pipes can be improved, providing a material basis for achieving high adhesion of the adhesive resin to composites of nylon / polyethylene with different structures.
[0014] (2) The adhesive resin for nylon / polyethylene composite pipes of the present invention contains a styrene-maleic anhydride copolymer. By adding the styrene-maleic anhydride copolymer, the adhesive resin is provided with maleic anhydride groups that can react with nylon. At the same time, the styrene-maleic anhydride copolymer can promote the microphase separation of each component of the adhesive resin, so that polar groups such as maleic anhydride and carboxyl groups are distributed on the surface of the adhesive resin, which is more conducive to the adhesive resin to wet the surface of nylon and polyethylene, and then form a high-strength chemical bond to nylon through chemical reaction.
[0015] (3) The adhesive resin of the present invention utilizes the anhydride groups and carboxyl groups grafted with polar monomers and the maleic anhydride groups of the added styrene-maleic anhydride copolymer. Through the principle of the reaction between maleic anhydride, carboxyl groups and amino groups of nylon, the adhesive resin and nylon are co-extruded and compounded at a temperature of 210-240°C, ensuring that maleic anhydride, carboxyl groups and amino groups of nylon undergo chemical reaction, and realizing the chemical bonding of the adhesive resin to nylon.
[0016] (4) The adhesive resin of the present invention, through the combination of its components, has excellent wettability and good adhesion to nylon and polyethylene, two polymers with large polarity differences. After bonding and compositing nylon / polyethylene, the 180° peel strength is greater than 12 N / mm, and the peel state is cohesive failure, thus achieving stable high-strength bonding of nylon and polyethylene. Detailed Implementation
[0017] In view of the fact that existing technologies for bonding nylon / polyethylene composites mainly employ multi-layer co-extrusion blown film or multi-layer co-extrusion casting methods, where nylon is mostly nylon 6 and there is a problem of low bonding strength between the nylon layer and the polyethylene layer, and that there are no reports on bonding resins suitable for bonding nylons with different molecular structures such as nylon 6, nylon 66, nylon 11, and nylon 12 with polyethylene, this invention provides a bonding resin applicable to nylon / polyethylene composite pipes with different molecular structures, its preparation method, and its application.
[0018] In a typical embodiment of the present invention, an adhesive resin for nylon / polyethylene composite pipes is provided. The raw materials of the adhesive resin for nylon / polyethylene composite pipes are composed of the following parts by weight: 20-30 parts of polar monomer-grafted polyethylene, 10-40 parts of nylon elastomer, 25-65 parts of polyethylene, 5-15 parts of styrene-maleic anhydride copolymer, and 0.5-1 parts of additives.
[0019] The polar monomer-grafted polyethylene is prepared by reactive extrusion of 90-97 parts high-density polyethylene, 3-10 parts ethylene propylene diene copolymer (i.e. ethylene propylene diene monomer rubber EPDM), 1.5-2.5 parts polar monomer and 0.02-0.10 parts peroxide initiator using a twin-screw extruder at 220-280°C.
[0020] This invention uses high-density polyethylene and ethylene propylene diene copolymer as the matrix for graft modification with polar monomers, and maleic anhydride and acrylic acid as graft modification monomers. The reaction grafting is carried out at 220-280℃. Through the action of peroxide initiator and the unsaturated double bond of ethylene propylene diene copolymer, polar monomers with anhydride and carboxyl groups can be more easily grafted onto the molecular chain of the matrix, and the grafting rate of the obtained polar monomers reaches more than 1.2%.
[0021] This invention uses high-density polyethylene and ethylene-propylene-diolefin copolymer as the matrix, and maleic anhydride and acrylic acid as polar grafting monomers. A high-graft-content, polar monomer-modified polyethylene is prepared through a grafting reaction. This polyethylene is then compounded with nylon elastomer, polyethylene, styrene-maleic anhydride copolymer, and functional additives, and blended using a twin-screw reactive extruder to prepare an adhesive resin with high adhesion to nylon / polyethylene composite pipes. The adhesive resin of this invention, through the combination of its components, exhibits excellent wettability and good adhesion to nylon and polyethylene, two polymers with significantly different polarities. The 180° peel strength for bonded nylon / polyethylene is greater than 12 N / mm, and the peel state of the bonded nylon / polyethylene is cohesive failure.
[0022] In one embodiment of this invention, the melt flow rate of the high-density polyethylene at 190°C and 2.16 kg is 5-20 g / 10 min.
[0023] In one embodiment of this invention, the diene content of the ethylene propylene diene copolymer is 0.5%-5% by mass.
[0024] In one embodiment of this invention, the polar monomer is a mixture of maleic anhydride and acrylic acid.
[0025] In one embodiment of this invention, the peroxide initiator is at least one selected from the following: di-tert-butyl peroxide diisopropylbenzene, di-tert-butyl peroxide, 2,5-dimethyl-2,5-di(2-ethylhexanoyl peroxide)hexane, tert-butyl peroxide isopropylbenzene, tert-butyl peroxide, tert-amyl peroxide, 1,1-di-tert-amyl peroxide-3,3,5-trimethylcyclohexane, and 1,1-di-tert-butyl peroxide-3,3,5-trimethylcyclohexane.
[0026] In one embodiment of this invention, the screw speed of the twin-screw extruder is 400-520 rpm during reactive extrusion.
[0027] In one embodiment of this invention, the nylon elastomer is a block copolymer with at least one of nylon 6, nylon 11 or nylon 12 as hard segments and polytetramethylene ether (PTMEG) or polyethylene glycol (PEG) as soft segments; preferably, the Shore hardness of the nylon elastomer is 35-75.
[0028] In one embodiment of this invention, the polyethylene is at least one of high-density polyethylene, linear low-density polyethylene, or metallocene linear low-density polyethylene; preferably, the polyethylene is at least one of high-density polyethylene or metallocene linear polyethylene.
[0029] In one embodiment of this invention, the mass percentage of maleic anhydride in the styrene-maleic anhydride copolymer is 5-25%; preferably, the weight-average molecular weight of the styrene-maleic anhydride copolymer is 5000-50000.
[0030] In one embodiment of this invention, the additive is at least one of an antioxidant, a UV stabilizer, and a pigment.
[0031] Preferably, the antioxidant is selected from pentaerythritol tetrakis[β-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate] (antioxidant 1010), octadecyl β-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate (antioxidant 1076), triethylene glycol ether di(3-tert-butyl-4-hydroxy-5-methylphenyl)propionate (antioxidant 245), 4,4'-thiobis(6-tert-butyl-3-methylphenol) (antioxidant 300), 1, One or more of the following: 3,5-tris(3,5-di-tert-butyl-4-hydroxybenzyl)isocyanuric acid (antioxidant 3114), 1,2-bis[β-(3,5-di-tert-butyl-4-hydroxyphenyl)propionyl]hydrazine (antioxidant 1024), N,N'-(hexane-1,6-diyl)bis[3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionamide] (antioxidant 1098), and tris(2,4-di-tert-butylphenyl) phosphite (antioxidant B215).
[0032] Preferably, the ultraviolet stabilizer is selected from 2-(2'-hydroxy-5'-methylphenyl)benzotriazole (UV-P), 2,4-dihydroxybenzophenone (UV-O), 2-hydroxy-4-methoxybenzophenone (UV-9), 2-hydroxy-4-n-octyloxybenzophenone (UV-531), 2-(2'-hydroxy-3',5'-di-tert-butylphenyl)-benzotriazole (UV-320), 2' ... The nano-oxide is selected from one or more of '-tert-butyl-5'-methylphenyl)-5-chlorobenzotriazole (UV-326), 2-(5-chloro-2H-benzotriazole-2-yl)-4,6-bis(1,1-dimethylethyl)phenol (UV-327), and hexamethylphosphoric triamine (HPT); the nano-oxide is selected from one or more of ATO (antimony tin oxide), AZO (aluminum-doped zinc oxide), and Ce-ATO (Ce-doped ATO).
[0033] Preferably, the pigment is selected from one or more of titanium dioxide, carbon black, graphite, titanium nickel yellow, titanium cobalt green, cobalt blue, copper chromium black, iron oxide, and mica coated with titanium dioxide.
[0034] In one embodiment of this invention, the 180° peel strength of the adhesive resin for the nylon / polyethylene composite pipe against nylon / polyethylene is greater than 12 N / mm.
[0035] In one embodiment of this invention, the peeling state of the nylon / polyethylene adhesive resin bonded to the nylon / polyethylene is cohesive failure.
[0036] Another typical embodiment of the present invention provides a method for preparing the above-mentioned adhesive resin for nylon / polyethylene composite pipes, the preparation method comprising the following steps:
[0037] The polar monomer-grafted polyethylene, nylon elastomer, polyethylene, styrene-maleic anhydride copolymer, and functional additives are mixed in proportion and then reacted, blended, and granulated using a twin-screw reactive extruder at 180-210℃ to obtain the final product.
[0038] A third aspect of the present invention provides the application of the above-described adhesive resin for nylon / polyethylene composite pipes in bonding the nylon layer and the polyethylene layer in a composite pipe.
[0039] In one embodiment of this implementation, the composite pipe includes a nylon / polyethylene composite pipe, a steel wire mesh reinforced nylon / polyethylene composite pipe, a fiberglass tape reinforced nylon / polyethylene composite pipe, a polyester fiber reinforced nylon / polyethylene composite pipe, and an aramid fiber reinforced nylon / polyethylene composite pipe.
[0040] In one embodiment of this invention, the bonding is performed by co-extrusion; the bonding temperature of the nylon layer and the adhesive resin is 210-240°C, and the bonding temperature of the polyethylene layer and the adhesive resin is 180-240°C.
[0041] To enable those skilled in the art to better understand the technical solution of the present invention, the technical solution of the present invention will be described in detail below with reference to specific embodiments.
[0042] Example 1
[0043] 1. Information on the raw materials used in Example 1 is as follows:
[0044] Preparation of polar monomer-grafted polyethylene (PE-g-M1): 90 parts of high-density polyethylene (2911, Fushun Petrochemical), 10 parts of ethylene-propylene-diolefin copolymer (3092PM, Shanghai Sinopec Mitsui Elastomer Co., Ltd.), 1 part of maleic anhydride, 1 part of acrylic acid, and 0.03 parts of di-tert-butyl peroxide diisopropylbenzene were mixed evenly by high-speed stirring. The mixture was then subjected to reactive extrusion at 240℃ using a twin-screw extruder with a screw length-to-diameter ratio of 40:1 and a diameter of 75 mm. Polar monomer-grafted PE-g-1 was obtained through reactive extrusion grafting. The monomer grafting rate was 1.42% after acid-base titration testing.
[0045] Nylon elastomer: 4033SA01, Arkema, France.
[0046] Styrene-maleic anhydride copolymer (SMA): SMA-800, maleic anhydride content 8±2%, Jiaxing Huawen Chemical Co., Ltd.
[0047] Polyethylene: HPR3518CB (metallocene linear low-density polyethylene), Dushanzi Petrochemical.
[0048] Antioxidant: B215, Beijing Jiyi Chemical Co., Ltd.
[0049] 2. The specific steps for preparing the adhesive resin for nylon / polyethylene composite pipes are as follows:
[0050] Mix the components evenly using a mixer according to the proportions in Table 1, add the mixture to a twin-screw extruder, melt-blend at 200°C, and granulate to obtain adhesive resin granules.
[0051] Table 1 shows the adhesive resin for nylon / polyethylene composite pipes in Example 1.
[0052]
[0053] 3. Testing and application of adhesive resins for nylon / polyethylene composite pipes:
[0054] 3.1 Test of 180° peel strength of nylon / polyethylene sheet composite:
[0055] Nylon 6 (high viscosity nylon, YH3400, Baling Petrochemical) was pressed into 0.2mm sheets at 230℃, polyethylene (2480, Qilu Petrochemical) was pressed into 2mm sheets at 200℃, and adhesive resin was pressed into 0.15mm films at 200℃. The nylon and polyethylene sheets were first placed on a flat vulcanizing machine at 220℃. After the sheets melted, the adhesive resin was applied to the nylon sheet, and then the molten polyethylene sheet was applied to the adhesive resin film. The PA / adhesive resin / PE composite board was laminated under a pressure of 0.5MPa for 20s. After cooling, it was cut into 25mm wide peel test samples. The 180° peel strength was tested at a tensile speed of 100mm / min. The relevant data are shown in Table 6.
[0056] 3.2 Application of adhesive resin in 90° peel test of PA6 / PE composite pipes:
[0057] On a three-layer co-extrusion composite pipe processing equipment, high-viscosity nylon 6 (YH3400, Baling Petrochemical) was used as the core pipe, and the adhesive resin and polyethylene (2480, Qilu Petrochemical) were used as the outer layers. The temperature of the nylon and adhesive resin extruders was controlled at 230℃, and the processing temperature of the outer polyethylene extruder was controlled at 200℃. PA6 / PE composite pipes with dn110*10mm were obtained by co-extrusion. The thickness of the adhesive resin layer was controlled at 0.5-1.0mm, the thickness of the outer layer was controlled at 1.5-2.0mm, and the total thickness was 10.0-10.5mm. Peel test samples with a width of 25mm were cut along the pipe direction, and the 90° peel strength was tested at a tensile speed of 100mm / min. The relevant data are shown in Table 6.
[0058] Example 2
[0059] 1. Information on the raw materials used in Example 2 is as follows:
[0060] Preparation of polar monomer-grafted polyethylene (PE-g-M2): 95 parts of high-density polyethylene (T5070, Fushun Petrochemical), 5 parts of ethylene-propylene-diolefin copolymer (4770P, Dow Chemical), 1.5 parts of maleic anhydride, 0.5 parts of acrylic acid, and 0.05 parts of 2,5-dimethyl-2,5-di(2-ethylhexanoylperoxide)hexane were mixed evenly by high-speed stirring. The mixture was then subjected to reactive extrusion at 220℃ using a twin-screw extruder with a screw length-to-diameter ratio of 44:1 and a diameter of 75 mm. Polar monomer-grafted PE-g-M2 was obtained through reactive extrusion grafting. The monomer grafting rate was 1.51% after acid-base titration test.
[0061] Preparation of polar monomer-grafted polyethylene (PE-g-M3): 95 parts of high-density polyethylene (T5070, Fushun Petrochemical), 5 parts of ethylene-propylene-diolefin copolymer (4770P, Dow Chemical), 0.5 parts of maleic anhydride, 1.5 parts of acrylic acid, and 0.05 parts of 2,5-dimethyl-2,5-di(2-ethylhexanoylperoxide)hexane were mixed uniformly by high-speed stirring. The mixture was then subjected to reactive extrusion at 220℃ using a twin-screw extruder with a screw length-to-diameter ratio of 44:1 and a diameter of 75 mm. Polar monomer-grafted PE-g-M3 was obtained through reactive extrusion grafting. After acid-base titration testing, the monomer grafting rate was 1.33%.
[0062] Nylon elastomer: 7033SA01, Arkema, France.
[0063] Styrene-maleic anhydride copolymer (SMA): SMA-700, maleic anhydride content 18±2%, Jiaxing Huawen Chemical Co., Ltd.
[0064] Polyethylene: 7042 (linear low-density polyethylene), Daqing Petrochemical.
[0065] Antioxidant: 1010, Linyi Sanfeng Chemical Co., Ltd.
[0066] 2. The specific steps for preparing the adhesive resin for nylon / polyethylene composite pipes are as follows:
[0067] Mix the components evenly using a mixer according to the proportions in Table 2, add them to a twin-screw extruder, melt-blend at 200°C, and granulate to obtain adhesive resin granules.
[0068] Table 2. Nylon / polyethylene adhesive resin formulation in Example 2
[0069]
[0070] 3. Testing and application of adhesive resins for nylon / polyethylene composite pipes:
[0071] 3.1 Test of peel strength of nylon / polyethylene composite:
[0072] Nylon 12 (high-viscosity nylon, L3000, Wanhua Chemical Group Co., Ltd.) was pressed into 0.2mm sheets at 210℃, polyethylene (2480, Qilu Petrochemical) was pressed into 2mm sheets at 200℃, and adhesive resin was pressed into 0.15mm films at 200℃. The nylon and polyethylene sheets were first placed on a flat vulcanizing machine at 220℃. After the sheets melted, the adhesive resin was applied to the nylon sheet, and then the molten polyethylene sheet was applied to the adhesive resin film. The PA / adhesive resin / PE composite board was laminated under a pressure of 0.5MPa for 20s. After cooling, it was cut into 25mm wide peel test samples. The 180° peel strength was tested at a tensile speed of 100mm / min. The relevant data are shown in Table 6.
[0073] 3.2 Adhesive resin for bonding PA12 / PE composite pipes:
[0074] On a three-layer co-extrusion composite pipe processing equipment, high-viscosity nylon 12 (L3000, Wanhua Chemical Group Co., Ltd.) was used as the core tube, the adhesive resin of Example 2 was used as the outer layer, and polyethylene (2480, Qilu Petrochemical) was used as the outer layer. The temperature of the nylon extruder was controlled at 210℃, the temperature of the adhesive resin extruder was controlled at 230℃, and the processing temperature of the outer polyethylene extruder was controlled at 180℃. PA12 / PE composite pipe with dn110*10mm was obtained by co-extrusion. The thickness of the adhesive resin layer was controlled at 0.5-1.0mm, the thickness of the outer layer was controlled at 1.5-2.0mm, and the total thickness was 10.0-10.5mm. Peel test samples with a width of 25mm were cut along the pipe direction, and the 90° peel strength was tested at a tensile speed of 100mm / min. The relevant data are shown in Table 6.
[0075] Example 3
[0076] 1. Information on the raw materials used in Example 3 is as follows:
[0077] Preparation of polar monomer grafted polyethylene (PE-g-M1): Same as in Example 1.
[0078] Nylon elastomer: 5533SP 01, Arkema, France.
[0079] Styrene-maleic anhydride copolymer (SMA): SMA-725, maleic anhydride content 25±2%, Jiaxing Huawen Chemical Co., Ltd.
[0080] Polyethylene: 8320 (linear low-density polyethylene), Daqing Petrochemical.
[0081] Antioxidant: 3114, BASF.
[0082] 2. The specific steps for preparing the adhesive resin for nylon / polyethylene composite pipes are as follows:
[0083] Mix the components evenly using a mixer according to the proportions in Table 3, add them to a twin-screw extruder, melt-blend at 190°C, and granulate to obtain adhesive resin granules.
[0084] Table 3. Nylon / polyethylene adhesive resin formulation in Example 3
[0085]
[0086] 3. Testing and application of adhesive resins for nylon / polyethylene composite pipes:
[0087] 3.1 Test of peel strength of nylon / polyethylene composite:
[0088] Three types of nylon matrix (Nylon 6, YH3400, Baling Petrochemical; Nylon 11FX0082, Arkema, France; Nylon 12, L3000, Wanhua Chemical Group Co., Ltd.) were pressed into 0.2mm sheets at 210℃, polyethylene (2480, Qilu Petrochemical) was pressed into 2mm sheets at 200℃, and adhesive resin was pressed into a 0.15mm film at 200℃. The nylon and polyethylene sheets were first placed on a flat vulcanizing machine at 220℃. After the sheets melted, the adhesive resin was applied to the nylon sheet, and then the molten polyethylene sheet was applied to the adhesive resin film. The PA / adhesive resin / PE composite board was laminated under a pressure of 0.5MPa for 20s. After cooling, it was cut into 25mm wide peel test samples. The 180° peel strength was tested at a tensile speed of 100mm / min. The relevant data are shown in Table 6.
[0089] 3.2 Adhesive resin is used for bonding PA / PE composite pipes reinforced with steel wire mesh:
[0090] (1) Preparation of PA6 / PE composite pipe reinforced with steel wire mesh:
[0091] On a multi-layer co-extrusion composite steel wire mesh reinforced composite pipe processing equipment, high-viscosity nylon 6 (YH3400, Baling Petrochemical) is used as the core tube, and the adhesive resin of Example 3 is co-extruded at 220℃. Then, 24 steel wires of 0.6mm each are wound on the core tube by left-hand and right-hand winding. A 1.2-1.5mm layer of adhesive resin of Example 3 is extruded on the surface of the steel wire reinforcement layer. Finally, polyethylene (2480, Qilu Petrochemical) is extruded on the surface of the adhesive resin at 210℃ as the outer layer. After cooling, a dn110*1.6MPa steel wire mesh reinforced PA6 / PE composite pipe is obtained.
[0092] (2) Preparation of PA11 / PE composite pipe reinforced with steel wire mesh skeleton:
[0093] On a multi-layer co-extrusion composite steel wire mesh reinforced composite pipe processing equipment, high-viscosity nylon 11 (FX0082, Arkema, France) is used as the core tube, and the adhesive resin of Example 3 is co-extruded at 220℃. Then, 24 steel wires of 0.6mm each are wound on the core tube by left-hand and right-hand winding. A 1.2-1.5mm layer of adhesive resin of Example 3 is extruded on the surface of the steel wire reinforcement layer. Finally, polyethylene (2480, Qilu Petrochemical) is extruded on the surface of the adhesive resin at 210℃ as the outer layer. After cooling, a dn110*1.6MPa steel wire mesh reinforced PA6 / PE composite pipe is obtained.
[0094] (3) Preparation of PA12 / PE composite pipe reinforced with steel wire mesh skeleton:
[0095] On a multi-layer co-extrusion composite steel wire mesh reinforced composite pipe processing equipment, high-viscosity nylon 12 (Nylon 12, L3000, Wanhua Chemical Group Co., Ltd.) is used as the core tube, and the adhesive resin of Example 3 is co-extruded at 220℃. Then, 24 steel wires of 0.6mm each are wound around the core tube in a left-hand and right-hand manner. A 1.2-1.5mm layer of adhesive resin of Example 3 is extruded on the surface of the steel wire reinforcement layer. Finally, polyethylene (2480, Qilu Petrochemical) is extruded at 210℃ as the outer layer on the surface of the adhesive resin. After cooling, a dn110*1.6MPa steel wire mesh reinforced PA6 / PE composite pipe is obtained.
[0096] (4) Cut the composite pipes prepared in (1)-(3) into 25mm wide peel test samples along the pipe direction and test the 90° peel strength at a tensile speed of 100mm / min. The relevant data are shown in Table 6.
[0097] Comparative Example 1
[0098] 1. The information on the raw materials used in Comparison 1 is as follows:
[0099] Polar monomer grafted polyethylene (PE-g-M1): Same as Example 1.
[0100] Nylon elastomer: 4033SA01, Arkema, France.
[0101] Styrene-maleic anhydride copolymer (SMA): SMA-800, maleic anhydride content 8±2%, Jiaxing Huawen Chemical Co., Ltd.
[0102] Polyethylene: HPR3518CB (metallocene linear low-density polyethylene), Dushanzi Petrochemical.
[0103] Antioxidant: B215, Beijing Jiyi Chemical Co., Ltd.
[0104] 2. The specific steps for preparing the adhesive resin for nylon / polyethylene composite pipes are as follows:
[0105] Mix the components evenly using a mixer according to the proportions in Table 4, add them to a twin-screw extruder, melt-blend at 200°C, and granulate to obtain adhesive resin granules.
[0106] Table 4 shows the nylon / polyethylene adhesive resin formulations in Comparative Example 1.
[0107]
[0108] 3. Testing and application of adhesive resins for nylon / polyethylene composite pipes:
[0109] 3.1 Test of 180° peel strength of nylon / polyethylene sheet composite:
[0110] Nylon 6 (high viscosity nylon, YH3400, Baling Petrochemical) was pressed into 0.2mm sheets at 230℃, polyethylene (2480, Qilu Petrochemical) was pressed into 2mm sheets at 200℃, and adhesive resin was pressed into 0.15mm films at 200℃. The nylon and polyethylene sheets were first placed on a flat vulcanizing machine at 220℃. After the sheets melted, the adhesive resin was applied to the nylon sheet, and then the molten polyethylene sheet was applied to the adhesive resin film. The PA / adhesive resin / PE composite board was laminated under a pressure of 0.5MPa for 20s. After cooling, it was cut into 25mm wide peel test samples. The 180° peel strength was tested at a tensile speed of 100mm / min. The relevant data are shown in Table 6.
[0111] 3.2 Application of adhesive resin in 90° peel test of PA6 / PE composite pipes:
[0112] On a three-layer co-extrusion composite pipe processing equipment, high-viscosity nylon 6 (YH3400, Baling Petrochemical) was used as the core pipe, comparative example 1 adhesive resin was used, and polyethylene (2480, Qilu Petrochemical) was used as the outer layer. The temperature of the nylon and adhesive resin extruder was controlled at 230℃, and the processing temperature of the outer polyethylene extruder was controlled at 200℃. PA6 / PE composite pipe with dn110*10mm was obtained by co-extrusion. The thickness of the adhesive resin layer was controlled at 0.5-1.0mm, the thickness of the outer layer was controlled at 1.5-2.0mm, and the total thickness was 10.0-10.5mm. Peel test samples with a width of 25mm were cut along the pipe direction, and the 90° peel strength was tested at a tensile speed of 100mm / min. The relevant data are shown in Table 6.
[0113] Comparative Example 2
[0114] 1. Information on the raw materials used in Comparative Example 2 is as follows:
[0115] Preparation of polar monomer-grafted polyethylene (PE-g-M4): 95 parts of high-density polyethylene (T5070, Fushun Petrochemical), 5 parts of ethylene-propylene-diolefin copolymer (4770P, Dow Chemical), 2 parts of maleic anhydride, and 0.05 parts of 2,5-dimethyl-2,5-di(2-ethylhexanoylperoxide)hexane were mixed evenly by high-speed stirring. The mixture was then subjected to reactive extrusion at 220℃ using a twin-screw extruder with a screw length-to-diameter ratio of 44:1 and a diameter of 75 mm. Polar monomer-grafted PE-g-M4 was obtained through reactive extrusion grafting. After acid-base titration testing, the monomer grafting rate was 1.05%.
[0116] Preparation of polar monomer-grafted polyethylene (PE-g-M5): 95 parts of high-density polyethylene (T5070, Fushun Petrochemical), 5 parts of ethylene-propylene-diolefin copolymer (4770P, Dow Chemical), 2 parts of acrylic acid, and 0.05 parts of 2,5-dimethyl-2,5-di(2-ethylhexanoylperoxide)hexane were mixed evenly by high-speed stirring. The mixture was then subjected to reactive extrusion at 220℃ using a twin-screw extruder with a screw length-to-diameter ratio of 44:1 and a diameter of 75 mm. Polar monomer-grafted PE-g-M5 was obtained through reactive extrusion grafting. The monomer grafting rate was 0.77% after acid-base titration testing.
[0117] Preparation of polar monomer-grafted polyethylene (PE-g-M6): 100 parts of high-density polyethylene (T5070, Fushun Petrochemical), 1.5 parts of maleic anhydride, 0.5 parts of acrylic acid, and 0.05 parts of 2,5-dimethyl-2,5-di(2-ethylhexanoylperoxide)hexane were mixed evenly by high-speed stirring. The mixture was then subjected to reactive extrusion at 220℃ using a twin-screw extruder with a screw length-to-diameter ratio of 44:1 and a diameter of 75 mm. Polar monomer-grafted PE-g-M6 was obtained through reactive extrusion grafting. The monomer grafting rate was 0.88% after acid-base titration testing.
[0118] Nylon elastomer: 7033SA01, Arkema, France.
[0119] Styrene-maleic anhydride copolymer (SMA): SMA-700, maleic anhydride content 18±2%, Jiaxing Huawen Chemical Co., Ltd.
[0120] Polyethylene: 7042 (linear low-density polyethylene), Daqing Petrochemical.
[0121] Antioxidant: 1010, Linyi Sanfeng Chemical Co., Ltd.
[0122] 2. The specific steps for preparing the nylon / polyethylene adhesive resin are as follows:
[0123] Mix the components evenly using a mixer according to the proportions in Table 5, add them to a twin-screw extruder, melt-blend at 200°C, and granulate to obtain adhesive resin granules.
[0124] Table 5 shows the nylon / polyethylene adhesive resin formulations in Comparative Example 2.
[0125]
[0126] 3. Testing and application of adhesive resins for nylon / polyethylene composite pipes:
[0127] 3.1 Test of peel strength of nylon / polyethylene composite:
[0128] Nylon 12 (high-viscosity nylon, L3000, Wanhua Chemical Group Co., Ltd.) was pressed into 0.2mm sheets at 210℃, polyethylene (2480, Qilu Petrochemical) was pressed into 2mm sheets at 200℃, and adhesive resin was pressed into 0.15mm films at 200℃. The nylon and polyethylene sheets were first placed on a flat vulcanizing machine at 220℃. After the sheets melted, the adhesive resin was applied to the nylon sheet, and then the molten polyethylene sheet was applied to the adhesive resin film. The PA / adhesive resin / PE composite board was laminated under a pressure of 0.5MPa for 20s. After cooling, it was cut into 25mm wide peel test samples. The 180° peel strength was tested at a tensile speed of 100mm / min. The relevant data are shown in Table 6.
[0129] 3.2 Adhesive resin for bonding PA12 / PE composite pipes:
[0130] On a three-layer co-extrusion composite pipe processing equipment, high-viscosity nylon 12 (L3000, Wanhua Chemical Group Co., Ltd.) was used as the core tube, adhesive resin (Comparative Example 2) was used as the adhesive resin, and polyethylene (2480, Qilu Petrochemical) was used as the outer layer. The temperature of the nylon extruder was controlled at 210℃, the temperature of the adhesive resin extruder was controlled at 230℃, and the processing temperature of the outer polyethylene extruder was controlled at 180℃. PA12 / PE composite pipe with dn110*10mm was obtained by co-extrusion. The thickness of the adhesive resin layer was controlled at 0.5-1.0mm, the thickness of the outer layer was controlled at 1.5-2.0mm, and the total thickness was 10.0-10.5mm. Peel test samples with a width of 25mm were cut along the pipe direction, and the 90° peel strength was tested at a tensile speed of 100mm / min. The relevant data are shown in Table 6.
[0131] Table 6 shows the 180° peel strength of the adhesive resin bonded PA / PE composite sheet and the 90° peel strength of the PA / PE composite pipe obtained through the above embodiments and comparative examples.
[0132] Table 6. Data on the 180° peel strength of PA / PE composite sheets bonded with adhesive resin and the 90° peel strength of PA / PE composite pipes.
[0133]
[0134]
[0135]
[0136] From the performance data of Examples 1-3 and Comparative Examples 1-2 shown in the table above, it can be seen that:
[0137] In Examples 1-3 of this invention, the 180° peel strength of the PA / PE sheet bonding was greater than 12 N / mm, and the peel state was cohesive failure. In Comparative Examples 1 and 2, the 180° peel strength of the PA / PE sheet bonding was less than 11 N / mm, and the peel state was uncertain. This indicates that the adhesive resin of this invention has higher peel strength, and the peel state is cohesive failure, demonstrating good stability of the peel force.
[0138] A comparison of Example 1 and Comparative Example 1 4A shows that the absence of styrene-maleic anhydride copolymer leads to a decrease in the peel strength of the adhesive resin, and the peel state changes from cohesive failure to either sticking to nylon or sticking to PE. A comparison of Example 1 and Comparative Examples 1 4B and 4C shows that when more than 15 parts of styrene-maleic anhydride copolymer are added, the adhesive resin exhibits a peel strength to PA / PE that drops below 12 N / mm, and the peel state is characterized by non-sticking to PE. The PA / PE composite pipe adhesive resin of this invention, by introducing 5-15 parts of styrene-maleic anhydride copolymer into the formulation, enables the adhesive resin to possess good adhesion and penetration properties to both PA and PE, and the peel state is characterized by cohesive failure.
[0139] The comparison of Examples 1 and 2 and Comparative Examples 4D and 4E shows that when the amount of nylon elastomer added to the adhesive resin is 10-40 parts, it can have good adhesion to PA / PE; when no nylon elastomer is added, the adhesive resin has poor adhesion to nylon; when more than 40 parts of nylon elastomer are added, the adhesive resin has poor adhesion to PE.
[0140] A comparison of Examples 2B and Comparative Examples 25A, 5B, and 5C shows that only by simultaneously adding both maleic anhydride and acrylic acid monomers to the polar monomer grafted polyethylene, and by adding 3-10 parts of ethylene propylene diene copolymer to the matrix, can the grafting rate of the polar monomer be guaranteed to be higher than 1.2%. Adding only maleic anhydride, only acrylic acid, or no ethylene propylene diene copolymer to the matrix all result in a low grafting rate of the polar monomer, thus leading to low peel strength of the adhesive resin for PA / PE bonding.
[0141] As can be seen from Examples 1, 2, and 3 of the present invention, the adhesive resin of the present invention has good adhesion to different nylons such as nylon 6, nylon 11, and nylon 12 and polyethylene. It can be used not only for the composite of PA / PE plastic pipes, but also for the composite of PA / PE composite pipes with steel wire mesh reinforcement.
[0142] The above description is merely a preferred embodiment of the present invention and is not intended to limit the invention. Various modifications and variations can be made to the present invention by those skilled in the art. Any modifications, equivalent substitutions, improvements, etc., made within the spirit and principles of the present invention should be included within the scope of protection of the present invention.
Claims
1. An adhesive resin for nylon / polyethylene composite pipes, characterized in that, The adhesive resin for the nylon / polyethylene composite pipe has the following raw material composition by mass parts: 20-30 parts of polar monomer grafted polyethylene, 10-40 parts of nylon elastomer, 25-65 parts of polyethylene, 5-15 parts of styrene-maleic anhydride copolymer, and 0.5-1 parts of additives. The polar monomer-grafted polyethylene is prepared by reactive extrusion of 90-97 parts high-density polyethylene, 3-10 parts ethylene propylene diene copolymer, 1.5-2.5 parts polar monomer and 0.02-0.10 parts peroxide initiator using a twin-screw extruder at 220-280°C. The polar monomer is a mixture of maleic anhydride and acrylic acid; The grafting rate of the polar monomer-grafted polyethylene is greater than 1.2%; The nylon elastomer is a block copolymer with at least one of nylon 6, nylon 11 or nylon 12 as hard segments and polytetramethylene ether or polyethylene glycol as soft segments.
2. The adhesive resin for nylon / polyethylene composite pipes as described in claim 1, characterized in that, The melt flow rate of the high-density polyethylene at 190°C and 2.16 kg is 5-20 g / 10 min; Alternatively, the diene content of the ethylene-propylene diene copolymer is 0.5%-5% by mass; Alternatively, the peroxide initiator is at least one selected from the following: di-tert-butyl peroxide diisopropylbenzene, di-tert-butyl peroxide, 2,5-dimethyl-2,5-di(2-ethylhexanoyl peroxide)hexane, tert-butyl peroxide isopropylbenzene, tert-butyl peroxide, tert-amyl peroxide, 1,1-di-tert-amyl peroxide-3,3,5-trimethylcyclohexane, and 1,1-di-tert-butyl peroxide-3,3,5-trimethylcyclohexane; Alternatively, when the twin-screw extruder performs reactive extrusion, the screw speed is 400-520 rpm.
3. The adhesive resin for nylon / polyethylene composite pipes according to claim 1, characterized in that, The Shore hardness of the nylon elastomer is 35-75; Alternatively, the polyethylene may be at least one of high-density polyethylene, linear low-density polyethylene, or metallocene linear low-density polyethylene.
4. The adhesive resin for nylon / polyethylene composite pipes according to claim 3, characterized in that, The polyethylene is at least one of high-density polyethylene or metallocene linear low-density polyethylene.
5. The adhesive resin for nylon / polyethylene composite pipes according to claim 1, characterized in that, The styrene-maleic anhydride copolymer contains 5-25% maleic anhydride by mass.
6. The adhesive resin for nylon / polyethylene composite pipes according to claim 5, characterized in that, The weight-average molecular weight of the styrene-maleic anhydride copolymer is 5000-50000.
7. The adhesive resin for nylon / polyethylene composite pipes according to claim 1, characterized in that, The additive is at least one of antioxidants, UV stabilizers, and pigments.
8. The adhesive resin for nylon / polyethylene composite pipes according to claim 1, characterized in that, The adhesive resin used for the nylon / polyethylene composite pipe has a 180° peel strength greater than 12 N / mm against nylon / polyethylene.
9. The adhesive resin for nylon / polyethylene composite pipes according to claim 1, characterized in that, The peeling state of the nylon / polyethylene adhesive used to bond the nylon / polyethylene in the nylon / polyethylene composite pipe is cohesive failure.
10. A method for preparing an adhesive resin for nylon / polyethylene composite pipes according to any one of claims 1-9, characterized in that, The preparation method includes the following steps: The polar monomer-grafted polyethylene, nylon elastomer, polyethylene, styrene-maleic anhydride copolymer, and functional additives are mixed evenly in a certain proportion, and then reacted, blended, and granulated using a twin-screw reactive extruder at 180-210℃ to obtain the final product.
11. The application of the adhesive resin for nylon / polyethylene composite pipes according to any one of claims 1-9 in bonding the nylon layer and the polyethylene layer in the composite pipe.
12. The application of the adhesive resin for nylon / polyethylene composite pipes according to claim 11 in bonding the nylon layer and the polyethylene layer in the composite pipe, characterized in that, The composite pipes include nylon / polyethylene composite pipes, steel wire mesh reinforced nylon / polyethylene composite pipes, fiberglass tape reinforced nylon / polyethylene composite pipes, polyester fiber reinforced nylon / polyethylene composite pipes, and aramid fiber reinforced nylon / polyethylene composite pipes.
13. The application according to claim 11, characterized in that, The bonding is achieved through co-extrusion; the bonding temperature between the nylon layer and the adhesive resin is 210-240℃, and the bonding temperature between the polyethylene layer and the adhesive resin is 180-240℃.
Citation Information
Patent Citations
Compatible adhesive resin for PE and PA and preparation method of compatible adhesive resin
CN112851861A
Method for preparing polyethylene type adhesive resin for multilayer co-extrusion barrier package
CN104449469A
High-temperature-resistant halogen-free flame-retardant nylon composite material and preparation method thereof
CN104497570A