A low temperature boron activation method

By depositing a hydrogenated boron-doped film layer on the surface of crystalline silicon and performing low-temperature thermal annealing, the problems of poor passivation effect of the p-type boron-doped polysilicon structure and high energy consumption of the high-temperature annealing process are solved, and efficient boron activation and electrode contact are achieved. Reduce production costs and equipment losses.

CN117153950BActive Publication Date: 2024-10-22WUXI SONGYU TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202311355611.3
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-10-19
Publication Date
2024-10-22
Estimated Expiration
2043-10-19

AI Technical Summary

Technical Problem

The existing p-type boron-doped polysilicon/tunneling silicon oxide/crystalline silicon structure has poor passivation effect, is difficult to form good contact with metal electrodes, and the high-temperature annealing process consumes high energy, affecting the life of the equipment hardware.

Method used

Using a low-temperature boron activation method, a hydrogenated intrinsic semiconductor film layer and a hydrogenated boron-doped semiconductor film layer are deposited on the surface of crystalline silicon where a selective tunneling layer is grown, and short-term thermal annealing is performed at 300~900°C to promote the hydrogen element. Redistribution and diffusion of boron elements to avoid defects and impurity problems caused by high-temperature annealing.

Benefits of technology

It improves the chemical and field effect passivation performance of the passivation structure, ensures good contact with metal electrodes, reduces power consumption and production costs, and extends the life of equipment hardware.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN117153950B_ABST
    Figure CN117153950B_ABST
Patent Text Reader

Abstract

The present invention belongs to the technical field of solar cells, and specifically relates to a low-temperature boron activation method. The present invention promotes the redistribution of hydrogen elements in the hydrogenated boron-doped semiconductor film layer by performing short-term rapid annealing at low temperature (300-900°C), thereby realizing the short-distance movement of the boron element (diffusion to the intrinsic layer). The adverse effect of increased defect state density in the hydrogenated boron-doped semiconductor film layer caused by the overflow of hydrogen elements caused by high-temperature (temperature>900°C) annealing is effectively avoided. The low-temperature boron activation method of the present invention effectively solves the adverse effect of poor chemical passivation effect of the selective tunneling layer caused by boron diffusion caused by high-temperature boron activation. The present invention fundamentally improves the chemical and field effect passivation performance of the passivated tunneling structure, and effectively ensures its good contact with the metal electrode. The low-temperature boron activation method of the present invention not only greatly reduces power consumption, but also reduces the production cost consumption caused by the hardware life of the equipment caused by high temperature.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of solar cells, and in particular relates to a low-temperature boron activation method. Background Art

[0002] Improving efficiency and reducing costs is an eternal topic in the development of photovoltaics. With the development of solar cell technology, the efficiency limit of PERC (Passivated Emitter and Rear Cell) solar cells based on p-type monocrystalline silicon substrates can no longer meet the development needs of photovoltaic technology due to their structure. N-type tunneling oxide passivated contact (TOPCon) solar cells have a theoretical limit efficiency of 28.7% due to their excellent structure (double-sided passivated contact structure), and have become the next generation of crystalline silicon solar cell structure to replace mass-produced PERC solar cells. N-type monocrystalline silicon has become the first choice for silicon substrates for TOPCon solar cells due to its superior characteristics of higher minority carrier lifetime and lower photoinduced attenuation than p-type monocrystalline silicon. At present, mass-produced TOPCon solar cells have a single-sided passivated contact structure, and their industry mass production efficiency is about 25.3%, which is still far from the theoretical efficiency. Therefore, efforts are still needed to improve the technology development of mass production efficiency.

[0003] A lot of efforts have been made by predecessors to develop TOPCon with double-sided passivation contact structure, but the actual results are not very ideal. The main reason is that the passivation effect of the p-type passivation contact structure, i.e., p-type high-concentration boron-doped semiconductor / tunneling silicon oxide / p-type low-concentration boron-doped crystalline silicon substrate, is not ideal. The main defects are: the p-type boron-doped polysilicon film needs to be annealed for a long time at high temperature (about 1000°C) to activate the boron element, and to promote the formation and growth of polysilicon grains to reduce the carrier grain boundary recombination with trace H elements or no H elements passivation. However, during the annealing process, because the solid solubility of silicon dioxide in boron is higher than that of silicon, a large amount of boron will enter the tunneling silicon oxide film, weakening its chemical passivation on the crystalline silicon surface. If the annealing temperature or annealing time is lowered, firstly, the activation amount of boron is difficult to obtain, which makes it difficult to form a good ohmic contact with the metal electrode; secondly, the crystallization rate and grain size of the polysilicon film cannot be guaranteed. Since the polysilicon film layer lacks H element passivation, the recombination of carriers during transmission in boron-doped amorphous silicon will be greatly increased; finally, high-temperature annealing has become a key factor restricting the cost reduction of solar cells, whether it is process energy consumption or the service life of equipment hardware. Summary of the invention

[0004] The present invention provides a low-temperature boron activation method to overcome the defects of the prior art p-type boron-doped polysilicon / tunneling silicon oxide / crystalline silicon structure, such as poor passivation effect, difficulty in forming good contact with metal electrodes, high energy consumption in the preparation process, and impact on the life of equipment hardware.

[0005] To achieve the above-mentioned purpose, the present invention is implemented by the following technical solutions:

[0006] A low temperature boron activation method comprises the following steps:

[0007] (S.1) depositing a hydrogenated intrinsic semiconductor film layer containing hydrogen on the surface of the crystalline silicon on which the selective tunneling layer is grown, to obtain silicon wafer I;

[0008] (S.2) depositing a hydrogenated boron-doped semiconductor film layer containing hydrogen and doped with boron on the surface of the silicon wafer I obtained in step (S.1) to obtain silicon wafer II;

[0009] (S.3) Take the silicon wafer II obtained in step (S.2) and perform thermal annealing at a temperature of 300-900°C for 3-10 minutes.

[0010] After further exploration, the inventors found that by utilizing the metastable characteristics of hydrogen, the boron element in the hydrogenated boron-doped semiconductor film layer can be caused to change in chemical activity due to the movement of hydrogen, that is, to produce high-concentration active boron that meets the performance requirements of the device. The present invention promotes the redistribution of hydrogen in the hydrogenated boron-doped semiconductor film layer by performing rapid and short-time (3-10min) thermal annealing at low temperature (300-900°C), thereby realizing the short-distance movement of boron (diffusion to the intrinsic layer). The adverse effects of increased defect state density in the hydrogenated boron-doped semiconductor film layer caused by the overflow of hydrogen caused by high-temperature (temperature>900°C) annealing are effectively avoided. At the same time, low-temperature short-time annealing helps to reduce impurity concentration and improve the purity and performance of the material. In addition, low-temperature annealing can improve the structure of the crystal by crystal rearrangement, lattice reorganization, etc., and further improve the crystal quality of the material. It can also promote the diffusion and activation of dopants in the crystal, improve the doping effect, and thus improve the conductive properties of the material. In addition, the low-temperature boron activation method of the present invention effectively solves the adverse effect of high-temperature boron activation, that is, the chemical passivation effect of the selective tunneling layer is deteriorated due to boron diffusion.

[0011] Preferably, the hydrogenated intrinsic semiconductor film layer in the step (S.1) is in any one of an amorphous state and a microcrystalline state.

[0012] Preferably, the hydrogenated boron-doped semiconductor film layer in the step (S.2) is in any one of an amorphous state and a microcrystalline state.

[0013] Preferably, the deposition method in step (S.1) and step (S.2) is any one of plasma enhanced chemical vapor deposition and hot wire assisted chemical vapor deposition.

[0014] The thin films prepared by plasma enhanced chemical vapor deposition (PECVD) and hot wire assisted chemical vapor deposition (hot wire CVD) have uniform thickness and excellent surface properties. Moreover, PECVD and hot wire CVD are usually carried out at lower temperatures, which makes the deposition process less thermally sensitive to the substrate material. It helps to reduce thermal damage to the substrate material and broadens the range of available substrate materials. At the same time, the composition, crystal structure and physical properties of the film can be adjusted by changing the deposition conditions, and the doping of the silicon film layer can be achieved, thereby regulating the conductive properties of the silicon film layer. Further precise control of the film properties is achieved, and flexibility is enhanced. In addition, PECVD and hot wire CVD have a high growth rate, which helps to improve the efficiency of large-area film preparation and further realize large-scale industrial production. In addition, compared with other thin film preparation technologies, PECVD and hot wire CVD do not require complex equipment and materials, which helps to reduce production costs and simplify the process flow.

[0015] Preferably, the gas source used in the deposition process in step (S.1) includes at least silane (SiH4) and hydrogen.

[0016] As a further preference, the gas source used in the deposition process in the step (S.1) includes silane (SiH4), hydrogen and argon.

[0017] Preferably, the gas source used in the deposition process in the step (S.2) includes at least silane and hydrogen, and also includes any one of diborane and trimethylboron.

[0018] As a further preference, the gas source used in the deposition process in the step (S.2) includes silane (SiH4), hydrogen, argon, and any one of diborane (B2H6) and trimethylboron.

[0019] Preferably, the thermal annealing in the step (S.3) is performed in a nitrogen atmosphere at atmospheric pressure.

[0020] Preferably, the thickness of the hydrogenated intrinsic semiconductor film layer obtained in the step (S.1) is 5-10 nm.

[0021] Preferably, the thickness of the hydrogenated boron-doped semiconductor film layer obtained in the step (S.2) is 30-100 nm.

[0022] Preferably, in the step (S.1) and the step (S.2), when the deposition method adopted is plasma enhanced chemical vapor deposition, the reaction temperature is 430-450°C; when the deposition method adopted is hot wire assisted chemical vapor deposition, the reaction temperature is 250-280°C.

[0023] Therefore, the present invention has the following beneficial effects:

[0024] (1) The present invention utilizes the metastable characteristics of hydrogen to cause the boron element in the hydrogenated boron-doped semiconductor film layer to undergo a change in chemical activity due to the movement of hydrogen, thereby generating high-concentration active boron that meets the performance requirements of the device;

[0025] (2) The present invention promotes the redistribution of hydrogen in the hydrogenated boron-doped semiconductor film layer by performing short-term rapid annealing at low temperature (300-900°C), thereby achieving short-distance movement of boron (diffusion to the intrinsic layer). This effectively avoids the adverse effect of increased defect state density in the hydrogenated boron-doped semiconductor film layer caused by hydrogen overflow caused by high temperature (temperature>900°C) annealing;

[0026] (3) The low-temperature boron activation method of the present invention effectively solves the adverse effect of high-temperature boron activation, which is caused by boron diffusion and leads to a deterioration in the chemical passivation effect of the selective tunneling layer;

[0027] (4) The present invention fundamentally improves the chemical and field effect passivation performance of the passivated tunneling structure, while effectively ensuring good contact between it and the metal electrode;

[0028] (5) The low-temperature boron activation method of the present invention not only greatly reduces power consumption, but also reduces production cost consumption caused by the life of equipment hardware due to high temperature. BRIEF DESCRIPTION OF THE DRAWINGS

[0029] Figure 1 Schematic diagram of the double-sided TOPCon solar cell structure.

[0030] Figure 2 Schematic diagram of p-type passivation contact structure film deposition and rapid thermal annealing.

[0031] Figure 3 The figure is a graph showing the electrochemical CV test results of the sample prepared in Example 1 (concentration variation with corrosion depth).

[0032] Figure 4 The figure is a graph showing the electrochemical CV test results of the sample prepared in Example 2 (concentration variation with corrosion depth).

[0033] Figure 5 The figure is a graph showing the electrochemical CV test results (concentration variation with corrosion depth) of the sample prepared in Example 3.

[0034] Figure 6 The figure is a graph of the electrochemical CV test results (concentration variation with corrosion depth) of the sample prepared in Example 4.

[0035] Figure 7This is a graph showing the electrochemical CV test results of the sample prepared in Comparative Example 1 (concentration variation with corrosion depth).

[0036] In the figure: 1 is p-type boron-doped crystalline silicon; 2 is a silicon dioxide tunneling layer; 3 is a hydrogenated intrinsic semiconductor film layer; 4 is a hydrogenated boron-doped semiconductor film layer; 5 is a boron-doped amorphous silicon layer after rapid thermal annealing, after which boron is activated and diffused and uniformly distributed in 3 and 4. DETAILED DESCRIPTION

[0037] The present invention is further described below in conjunction with the accompanying drawings and specific embodiments of the specification. Those of ordinary skill in the art will be able to implement the present invention based on these descriptions. In addition, the embodiments of the present invention involved in the following description are generally only embodiments of a part of the present invention, rather than all embodiments. Therefore, based on the embodiments of the present invention, all other embodiments obtained by those of ordinary skill in the art without making creative work should fall within the scope of protection of the present invention.

[0038] Example 1

[0039] A low temperature boron activation method comprises the following steps:

[0040] (S.1) Place a p-type boron-doped crystalline silicon 1 substrate into a furnace tube of a plasma enhanced chemical vapor deposition (PECVD) machine. The active boron concentration on the surface of the p-type boron-doped crystalline silicon 1 substrate is 8×10 18 / cm 3 The process temperature of the furnace tube is set at 450-430°C from the furnace mouth to the furnace tail. After vacuuming, nitrous oxide is introduced first, with a gas flow rate of 8000sccm, a pressure of 150Pa, a power of 12000W, and a process time of 150s. A silicon dioxide tunneling layer 2 with a thickness of about 1-2nm is grown in situ on the surface of p-type boron-doped crystalline silicon 1 using nitrous oxide plasma;

[0041] (S.2) Subsequently, vacuum is applied, and silane (SiH4), hydrogen (H2), and argon (Ar) are introduced, with gas flow rates of 2800sccm, 8000sccm, and 4000sccm, respectively. The pressure is 280Pa, the power is 12000W, and the process time is 180s. A 10nm thick hydrogenated intrinsic amorphous silicon film layer (a-Si:H) 3 is deposited on the surface of the silicon dioxide tunneling layer 2 to obtain silicon wafer I.

[0042] (S.3) After step (S.2), evacuate the gas, introduce silane (SiH4), diborane (B2H6, the main gas composition of which is a mixture of 5% pure B2H6 and 95% H2), hydrogen (H2), and argon (Ar), with gas flow rates of 2800sccm, 1000sccm, 7000sccm, and 4000sccm, respectively, at a pressure of 280Pa, a power of 15000W, and a process time of 800s, and deposit a layer of hydrogenated boron-doped amorphous silicon film layer (B:a-Si:H) 4 with a thickness of 65nm on the surface of the hydrogenated intrinsic amorphous silicon film layer (a-Si:H) 3 on the silicon wafer I obtained in step (S.1), to obtain silicon wafer II;

[0043] (S.4) The silicon wafer II with the surface deposited with hydrogenated boron-doped amorphous silicon film layer (B: a-Si: H) 4 obtained in step (S.3) is sent into a rapid thermal annealing furnace. The annealing environment is: nitrogen atmosphere, nitrogen flow rate is 12000sccm, atmospheric pressure, annealing process temperature is 900℃, process time is 3min, and the final boron-activated and uniformly distributed boron-doped amorphous silicon layer 5 is formed. The schematic diagram of the p-type passivation contact structure film deposition and rapid thermal annealing is shown in FIG. Figure 2 The further formed double-sided TOPCon solar cell structure is shown in Figure 1 The prepared samples were tested for active boron concentration and its distribution with corrosion depth using an electrochemical CV tester. The test results are shown in Figure 3 shown.

[0044] from Figure 3 The data analysis shows that the boron element in the boron-doped p-type passivation contact structure prepared by this method only exists in the boron-doped amorphous silicon layer, and the maximum surface concentration is 5.1×10 20 / cm 3 , and did not enter the crystalline silicon body due to high temperature annealing. In addition, the prepared samples were subjected to passivation testing using the Sinton WCT-120 minority carrier lifetime tester, a characterization method commonly used in the photovoltaic industry. The dark state saturation current density (J0) was 8fA / cm 2 This result shows that the present invention effectively solves the contradiction between the poor matching of the boron activation concentration and the failure of the chemical passivation effect of the silicon dioxide tunneling layer caused by high temperature annealing.

[0045] Example 2

[0046] A low temperature boron activation method comprises the following steps:

[0047] (S.1) Place a p-type boron-doped crystalline silicon 1 substrate into a furnace tube of a plasma enhanced chemical vapor deposition (PECVD) machine. The active boron concentration on the surface of the p-type boron-doped crystalline silicon 1 substrate is 8×10 18 / cm3 The process temperature of the furnace tube is set at 450-430°C from the furnace mouth to the furnace tail. After vacuuming, nitrous oxide is introduced first, with a gas flow rate of 8000sccm, a pressure of 150Pa, a power of 12000W, and a process time of 150s. A silicon dioxide tunneling layer 2 with a thickness of about 1-2nm is grown in situ on the surface of p-type boron-doped crystalline silicon 1 using nitrous oxide plasma;

[0048] (S.2) Subsequently, the vacuum was evacuated, and silane (SiH4), hydrogen (H2), and argon (Ar) were introduced, with gas flow rates of 2800sccm, 8000sccm, and 4000sccm, respectively. The pressure was 280Pa, the power was 12000W, and the process time was 135s. A layer of hydrogenated intrinsic amorphous silicon film (a-Si:H) 3 with a thickness of 7.5nm was deposited on the surface of the silicon dioxide tunneling layer 2 to obtain silicon wafer I;

[0049] (S.3) After step (S.2), evacuate the chamber and introduce silane (SiH4), diborane (B2H6, the main gas composition of which is a mixture of 5% pure B2H6 and 95% H2), hydrogen (H2), and argon (Ar). The gas flow rates are 2800sccm, 1000sccm, 7000sccm, and 4000sccm, respectively. The pressure is 280Pa, the power is 15000W, and the process time is 370s. A layer of hydrogenated boron-doped amorphous silicon film layer (B:a-Si:H) 4 with a thickness of 30nm is deposited on the surface of the hydrogenated intrinsic amorphous silicon film layer (a-Si:H) 3 on the silicon wafer I obtained in step (S.1), thereby obtaining silicon wafer II;

[0050] (S.4) The silicon wafer II with the hydrogenated boron-doped amorphous silicon film layer (B: a-Si: H) 4 deposited on the surface obtained in step (S.3) is sent into a rapid thermal annealing furnace. The annealing environment is: nitrogen atmosphere, nitrogen flow rate is 12000sccm, atmospheric pressure, annealing process temperature is 600℃, process time is 6.5min, and the final boron-activated and uniformly distributed boron-doped amorphous silicon layer 5 is formed. The prepared sample is tested for active boron concentration and its distribution with corrosion depth using an electrochemical CV tester. The test results are as follows: Figure 4 shown.

[0051] from Figure 4 The data analysis shows that the boron element in the boron-doped p-type passivation contact structure prepared by this method only exists in the boron-doped amorphous silicon layer, and the maximum surface concentration is 3.8×10 20 / cm 3 , and it did not enter the crystalline silicon body due to high temperature annealing. In addition, the prepared samples were subjected to passivation testing using the Sinton WCT-120 minority carrier lifetime tester, a characterization method commonly used in the photovoltaic industry. The dark state saturation current density (J0) was 7fA / cm2 This result shows that the present invention effectively solves the contradiction between the poor matching of the boron activation concentration and the failure of the chemical passivation effect of the silicon dioxide tunneling layer caused by high temperature annealing.

[0052] The thickness of the hydrogenated intrinsic amorphous silicon film deposited in this embodiment is 2.5 nm thinner than that in embodiment 1, and the thickness of the hydrogenated boron-doped amorphous silicon film is 35 nm thinner than that in embodiment 1. The rapid thermal annealing temperature is 300°C lower than that in embodiment 1, and the annealing time is 3.5 min longer. The activated boron concentration in the obtained boron-doped amorphous silicon layer is 1.4×10 20 / cm 3 In particular, the boron doping concentration of the boron-doped amorphous silicon layer close to the surface of the silicon dioxide tunneling layer is 1.8×10 20 / cm 3 The reason is that, under low temperature annealing, firstly, the original moving kinetic energy of H in the relatively metastable state is lower in low temperature rapid annealing than in high temperature rapid annealing, so the concentration of active boron element generated under low temperature is relatively low; secondly, it is relatively difficult for boron element to diffuse from hydrogenated boron-doped amorphous silicon film layer to hydrogenated intrinsic amorphous silicon film layer, so the diffusion concentration is significantly reduced. However, from the passivation data, J0 is lower than that of Example 1, and still meets the requirements of the passivation contact structure.

[0053] Example 3

[0054] A low temperature boron activation method comprises the following steps:

[0055] (S.1) Place a p-type boron-doped crystalline silicon substrate 1 into a furnace tube of a plasma enhanced chemical vapor deposition (PECVD) machine. The active boron concentration on the surface of the p-type boron-doped crystalline silicon substrate 1 is 8.2×10 18 / cm 3 The process temperature of the furnace tube is set at 450-430°C from the furnace mouth to the furnace tail. After vacuuming, nitrous oxide is introduced first, with a gas flow rate of 8000sccm, a pressure of 150Pa, a power of 12000W, and a process time of 150s. A silicon dioxide tunneling layer 2 with a thickness of about 1-2nm is grown in situ on the surface of p-type boron-doped crystalline silicon 1 using nitrous oxide plasma;

[0056] (S.2) Subsequently, vacuum is applied, and silane (SiH4), hydrogen (H2), and argon (Ar) are introduced, with gas flow rates of 2800sccm, 8000sccm, and 4000sccm, respectively. The pressure is 280Pa, the power is 12000W, and the process time is 90s. A layer of hydrogenated intrinsic amorphous silicon film (a-Si:H) 3 with a thickness of 5nm is deposited on the surface of the silicon dioxide tunneling layer 2 to obtain silicon wafer I;

[0057] (S.3) After step (S.2), evacuate the chamber, introduce silane (SiH4), diborane (B2H6, the main gas composition of which is a mixture of 5% pure B2H6 and 95% H2), hydrogen (H2), and argon (Ar), with gas flow rates of 2800sccm, 1000sccm, 7000sccm, and 4000sccm, respectively, at a pressure of 280Pa, a power of 15000W, and a process time of 1230s, and deposit a layer of hydrogenated boron-doped amorphous silicon film layer (B:a-Si:H) 4 with a thickness of 100nm on the surface of the hydrogenated intrinsic amorphous silicon film layer (a-Si:H) 3 on the silicon wafer I obtained in step (S.1), to obtain silicon wafer II;

[0058] (S.4) The silicon wafer II with the hydrogenated boron-doped amorphous silicon film layer (B: a-Si: H) 4 deposited on the surface obtained in step (S.3) is sent into a rapid thermal annealing furnace. The annealing environment is: nitrogen atmosphere, nitrogen flow rate is 12000sccm, atmospheric pressure, annealing process temperature is 300°C, process time is 10min, and the final boron-activated and uniformly distributed boron-doped amorphous silicon layer 5 is formed. The prepared sample is tested for active boron concentration and its distribution with corrosion depth using an electrochemical CV tester. The test results are as follows: Figure 5 shown.

[0059] from Figure 5 The data analysis shows that the boron element in the boron-doped p-type passivation contact structure prepared by this method only exists in the amorphous silicon layer, and the maximum surface concentration is 2×10 20 / cm 3 , and did not enter the crystalline silicon body due to high temperature annealing. In addition, the prepared samples were subjected to passivation testing using the Sinton WCT-120 minority carrier lifetime tester, a characterization method commonly used in the photovoltaic industry. The dark state saturation current density (J0) was 6.8fA / cm 2 This result shows that the present invention effectively solves the contradiction between the poor matching of the boron activation concentration and the failure of the chemical passivation effect of the silicon dioxide tunneling layer caused by high temperature annealing.

[0060] The thickness of the hydrogenated intrinsic amorphous silicon film deposited in this embodiment is 5 nm thinner than that in embodiment 1, and the thickness of the hydrogenated boron-doped amorphous silicon film is 35 nm thicker than that in embodiment 1. The rapid thermal annealing temperature is 600°C lower than that in embodiment 1, and the annealing time is 7 min longer. The activated boron concentration in the obtained boron-doped amorphous silicon layer is 3.1×10 20 / cm 3The reason is that, under low temperature annealing, the original kinetic energy of H in the metastable state is lower in low temperature rapid annealing than in high temperature rapid annealing, so the concentration of active boron element generated under low temperature is relatively low. However, from the passivation data, J0 is lower than that in Example 1, so the low temperature annealing still meets the requirements of the passivation contact structure.

[0061] Example 4

[0062] A low temperature boron activation method comprises the following steps:

[0063] (S.1) Place a p-type boron-doped crystalline silicon substrate 1 into a furnace tube of a plasma enhanced chemical vapor deposition (PECVD) machine. The active boron concentration on the surface of the p-type boron-doped crystalline silicon substrate 1 is 8×10 18 / cm 3 The process temperature of the furnace tube is set at 450-430°C from the furnace mouth to the furnace tail. After vacuuming, nitrous oxide is introduced first, with a gas flow rate of 8000sccm, a pressure of 150Pa, a power of 12000W, and a process time of 150s. A silicon dioxide tunneling layer 2 with a thickness of about 1-2nm is grown in situ on the surface of p-type boron-doped crystalline silicon 1 using nitrous oxide plasma;

[0064] (S.2) Place the sample of the p-type boron-doped crystalline silicon 1 substrate and the silicon dioxide tunneling layer 2 deposited with a thickness of 1-2 nm in step (S.1) into the chamber of a hot wire assisted chemical vapor deposition (hot wire CVD) machine. The process temperature in the process chamber is 250°C, the chamber is evacuated, silane (SiH4) and hydrogen (H2) are introduced, and the gas flow rates are 2800sccm and 8000sccm respectively, the pressure is 5Pa, the hot wire temperature is 1950°C, the process time is 120s, and a layer of hydrogenated intrinsic microcrystalline silicon film (a-Si:H) 3 with a thickness of 10nm is deposited on the surface of the silicon dioxide tunneling layer 2 to obtain silicon wafer I;

[0065] (S.3) After step (S.2), evacuate the chamber, introduce silane (SiH4), diborane (B2H6, the main gas composition of which is a mixture of 5% pure B2H6 and 95% H2), and hydrogen (H2), with gas flow rates of 2800sccm, 1000sccm, and 7000sccm, respectively, and the pressure is 5Pa. The hot wire temperature is 1950°C, and the process time is 795s. A layer of hydrogenated boron-doped microcrystalline silicon film layer (B:a-Si:H) 4 with a thickness of 65nm is deposited on the surface of the hydrogenated intrinsic microcrystalline silicon film layer (a-Si:H) 3 on the silicon wafer I obtained in step (S.1), thereby obtaining silicon wafer II;

[0066] (S.4) The silicon wafer II with a hydrogenated boron-doped microcrystalline silicon film layer (B: a-Si: H) 4 deposited on the surface obtained in step (S.3) is sent into a rapid thermal annealing furnace. The annealing environment is: nitrogen atmosphere, nitrogen flow rate is 12000sccm, atmospheric pressure, annealing process temperature is 900°C, process time is 3min, and the final boron-activated and uniformly distributed boron-doped microcrystalline silicon layer 5 is formed. The prepared sample is tested for active boron concentration and its distribution with corrosion depth using an electrochemical CV tester. The test results are as follows: Figure 6 shown.

[0067] from Figure 6 The data analysis shows that the boron element in the boron-doped p-type passivation contact structure prepared by this method only exists in the microcrystalline silicon layer, and the maximum surface concentration is 5.7×10 20 / cm 3 , and it did not enter the crystalline silicon body due to high temperature annealing. In addition, the prepared samples were subjected to passivation testing using the Sinton WCT-120 minority carrier lifetime tester, a characterization method commonly used in the photovoltaic industry. The dark state saturation current density (J0) was 8.2fA / cm 2 This result shows that the present invention effectively solves the contradiction between the poor matching of the boron activation concentration and the failure of the chemical passivation effect of the silicon dioxide tunneling layer caused by high temperature annealing.

[0068] The equipment used in this embodiment to deposit hydrogenated intrinsic microcrystalline silicon and hydrogenated boron-doped microcrystalline silicon is hot-filament CVD. The deposition thickness and rapid annealing process are the same. The activated boron concentration in the obtained boron-doped microcrystalline silicon layer is 6×10 higher than that in Example 1. 19 / cm 3 The reason is that in the hot-filament CVD process, the degree of hydrogen ionization is higher than that in the PECVD process, and the hydrogen content in the hydrogenated intrinsic microcrystalline silicon film layer is higher than that in Example 1. Therefore, the relative metastable H content is higher, and accordingly, the density of boron activation brought about by the movement of metastable H is higher than that in Example 1. However, from the perspective of passivation, compared with Example 1, J0 is slightly higher, mainly because the high boron activation concentration has a slight effect on the chemical passivation of the silicon dioxide tunneling layer, but it still meets the requirements of the passivated contact structure.

[0069] For the hot wire CVD chamber deposition temperature between 250 and 280° C., the effect brought about is the change of the grain size of microcrystalline silicon, and has little effect on the doping concentration of boron, which will not be further elaborated in the present invention.

[0070] Comparative Example 1

[0071] This comparative example provides a boron activation method for a conventional p-type passivated contact structure, comprising the following steps:

[0072] (S.1) A p-type boron-doped crystalline silicon substrate 1 is placed in a furnace tube of a low-pressure chemical vapor deposition (LPCVD) machine, wherein the active boron concentration on the surface of the p-type boron-doped crystalline silicon substrate 1 is 8×10 18 / cm 3 The furnace process temperature from the furnace mouth to the furnace tail is set to 600~590℃, and the furnace is vacuumed. Then oxygen is introduced first. The gas flow rate is 15000sccm, the pressure is 1030mTorr, and the process time is 20min. A silicon dioxide tunneling layer 2 with a thickness of about 1~2nm is grown on the surface of the p-type boron-doped crystalline silicon 1 using oxygen;

[0073] (S.2) Subsequently, the temperature is raised to 600-610°C, vacuum is drawn, silane (SiH4) is introduced, the gas flow rate is 1200 sccm, the pressure is 210 mTorr, the process time is 30 min, and a layer of hydrogenated intrinsic polysilicon film (poly-Si) 3 with a thickness of 120 nm is deposited on the surface of the silicon dioxide tunneling layer 2 to obtain silicon wafer I;

[0074] (S.3) After step (S.2), the silicon wafer I is taken out of the cavity and sent into a boron diffusion furnace tube, evacuated, heated to 890°C, and introduced with boron trichloride (BCl3), oxygen (O2), and nitrogen (N2). The gas flow rates are 200sccm, 800sccm, and 3500sccm, respectively. The pressure is 150Pa, and the process time is 600s. A layer of boron-doped silicon oxide (BSG) 4 with a thickness of about 20nm is deposited on the surface of the hydrogenated intrinsic polysilicon film layer (poly-Si) 3 on the silicon wafer I obtained in step (S.2), thereby obtaining silicon wafer II;

[0075] (S.4) Then, nitrogen gas was introduced at a flow rate of 6000sccm and a pressure of 450mbar, and the temperature was raised to 1030°C under vacuum. When the temperature stabilized at 1030°C, nitrogen gas was stopped and oxygen gas was introduced at a gas flow rate of 15000sccm for high-temperature oxidation and boron diffusion. The process time was 20min to form the final boron-diffused boron-doped polysilicon layer 5. The prepared samples were tested for active boron concentration and its distribution with corrosion depth using an electrochemical CV tester. The test results are shown in Figure 2. Figure 7 shown.

[0076] from Figure 7 The data analysis shows that the maximum polysilicon area is 5.5×10 20 / cm 3 This concentration is similar to that in Example 1. However, the slope of the concentration change of the curve between the polysilicon region and the p-type crystalline silicon region is significantly slowed down, and the region changes from 120nm to 160nm, and the concentration at 160nm reaches 1.5×10 19 / cm 3 , while the basic concentration on the surface of the source is only 8×1018 / cm 3 , indicating that during the high-temperature process diffusion, the boron source not only entered the polysilicon, but also a certain concentration of boron entered the silicon dioxide tunneling layer, and a part of it entered the p-type crystalline silicon from the silicon dioxide tunneling layer. Since the solid solubility of silicon dioxide in boron is higher than that of silicon, this indirectly indicates that the concentration of boron in the silicon dioxide tunneling layer is higher than that on the surface of p-type crystalline silicon. It can be inferred that the chemical passivation of the silicon dioxide tunneling layer may be destroyed by the boron element doped therein. Furthermore, the sample was then subjected to a passivation test using the Sinton WCT-120 minority carrier lifetime tester, a characterization method commonly used in the photovoltaic industry. The test showed that the dark state saturation current density (J0) of the prepared sample was 15fA / cm 2 This result shows that the above inference is correct. This comparison shows that the low-temperature boron activation scheme of Example 1 is more suitable for boron activation of p-type passivated tunneling structure.

[0077] The above description is only a detailed description of the preferred embodiments and principles of the present invention. For ordinary technicians in this field, according to the ideas provided by the present invention, there will be changes in the specific implementation methods, and these changes should also be regarded as the protection scope of the present invention.

Claims

1. A low temperature boron activation method, characterized in that: The following steps are involved: (S.1) depositing a hydrogenated intrinsic semiconductor film layer containing hydrogen element on the surface of the crystalline silicon having the selective tunneling layer, to obtain silicon wafer I; the gas source used in the deposition process includes at least silane and hydrogen; the gas flow rates of silane and hydrogen are 2800 sccm and 8000 sccm respectively; (S.2) depositing a hydrogenated boron-doped semiconductor film layer containing hydrogen and doped with boron on the surface of the silicon wafer I obtained in step (S.1) to obtain silicon wafer II; the gas source used in the deposition process includes at least silane and hydrogen, and also includes any one of diborane and trimethylboron; the gas flow rates of silane, hydrogen and diborane are 2800sccm, 7000sccm and 1000sccm respectively; (S.3) Take the silicon wafer II obtained in step (S.2) and perform thermal annealing at a temperature of 300-900°C for 3-10 minutes.

2. A low temperature boron activation method according to claim 1, characterized in that: The hydrogenated intrinsic semiconductor film layer in the step (S.1) is in any one of an amorphous state and a microcrystalline state.

3. A low temperature boron activation method according to claim 1, characterized in that: The hydrogenated boron-doped semiconductor film layer in the step (S.2) is in any one of an amorphous state and a microcrystalline state.

4. A low temperature boron activation method according to claim 1, characterized in that: The deposition method in the step (S.1) and the step (S.2) is any one of plasma enhanced chemical vapor deposition and hot wire assisted chemical vapor deposition.

5. A low temperature boron activation method according to claim 1, characterized in that: The annealing environment for thermal annealing in the step (S.3) is: carried out under atmospheric pressure in a nitrogen atmosphere.

6. A low temperature boron activation method according to claim 1 or 2, characterized in that: The thickness of the hydrogenated intrinsic semiconductor film layer obtained in the step (S.1) is 5-10 nm.

7. A low temperature boron activation method according to claim 1 or 3, characterized in that: The thickness of the hydrogenated boron-doped semiconductor film layer obtained in the step (S.2) is 30-100 nm.

8. A low temperature boron activation method according to claim 1, characterized in that: In the step (S.1) and the step (S.2), when the deposition method adopted is plasma enhanced chemical vapor deposition, the reaction temperature is 430-450°C; when the deposition method adopted is hot wire assisted chemical vapor deposition, the reaction temperature is 250-280°C.