A resistive switching memory based on a maicoene-titanium oxide Schottky junction and its fabrication method
By utilizing the defects of macoene material as charge traps in the macoene-titanium oxide Schottky junction, the Schottky barrier is modulated, solving the performance fluctuation problem of resistive switching memory and realizing a resistive switching memory with high uniformity and stability, especially a memory with self-rectification characteristics.
Patent Information
- Application Number
- CN202210558350.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-05-20
- Publication Date
- 2026-11-17
- Estimated Expiration
- 2042-05-20
Smart Images

Figure CN117156866B_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the research and application of novel macoene-based memory devices, specifically a resistive switching memory based on a macoene-titanium oxide Schottky junction and its fabrication method. Background Technology
[0002] Metal-oxide junctions are one of the fundamental components of electronic devices. [1 -2]. Generally, due to the difference in work function between metals and electron affinity between oxides, a Schottky barrier forms at the metal-oxide interface. [3] In recent years, resistive random access memories (RRAMs) based on metal-oxide Schottky junctions have emerged as a popular choice due to their simple structure and high repeatability, meeting the rapidly growing demands in fields such as non-volatile data storage, logic operations, and neural computing. [4 -6]. However, the performance fluctuations caused by the random characteristics of the conductive filament resistive switching mechanism have become a major obstacle to the large-scale application of resistive random access memory (RRAM). [7] Therefore, finding a resistance switching mechanism that eliminates the involvement of localized conductive filaments is of great significance for developing highly uniform resistive switching memories. Another common resistance switching mechanism utilizes defect traps present throughout the top electrode and oxide interface to capture and release injected carriers, causing a change in the Schottky barrier, thereby achieving resistance switching behavior and effectively improving device performance uniformity.
[0003] MXenes are a class of transition metal carbides, transition metal nitrides, or transition metal carbonitrides with a two-dimensional layered structure. They are novel materials with a graphene-like structure obtained through MAX phase processing. Recently, with the realization of wafer-level high-resolution MXene thin film patterning technology... [8] Maicoene is known for its excellent electrical conductivity and good hydrophilicity. [9] This opens up new avenues for designing electrode materials for highly active, long-life resistive switching memories. Typically, in the preparation of maicoene materials, the etching process using hydrofluoric acid inevitably introduces a high concentration of defects into the maicoene.
[10] This makes macoene an ideal candidate electrode material for constructing uniform resistive switching memory.
[0004] References:
[0005] [1] SMSze, Physics of Semiconductor Devices, Phys. Today 15 (1981) 1438-1438.
[0006] [2]A.Zangwill,J.W.Gadzuk,Physics atSurfaces,Phys.Today 100(1988)1463-1464.
[0007] [3]Z.B.Yan,J.M.Liu,Coexistence of high performance resistance andcapacitance memory based on multilayered metal-oxide structures,Sci.Rep.3(2013)2482.
[0008] [4]Z.Yan,Y.Guo,G.Zhang,J.M.Liu,High-performance programmable memorydevices based on Co-doped BaTiO3,Adv.Mater.23(2011)1351-1355.
[0009] [5]C.Liu,H.Chen,X.Hou,H.Zhang,P.Zhou,Small footprint transistorarchitecture for photoswitching logic and in situ memory,Nat.Nanotechnol.14(2019)662.
[0010] [6]Z.Wang,S.Ambrogio,S.Balatti,I.Daniele,A 2-transistor / 1-resistorartificial synapse capable of communication and stochastic learning inneuromorphic systems,Front.Neurosci.8(2015)438.
[0011] [7]Z.Zhang,Z.Wang,T.Shi,C.Bi,P.Zhou,Memory materials and devices:fromconcept to application,InfoMat2(2020)261-290.
[0012] [8] B. Li, QB Zhu, C. Cui, ZH Wang, S. Feng, Y. Sun, et al. Patterning of wafer-scale MXene films for high-performance image sensor arrays. Adv. Mater. 34 (2022) 2201298.
[0013] [9] B.Lyu, M.Kim, H.Jing, J.Kang, JHcho, Large-area MXene electrode array for flexible electronics, ACS Nano 13 (2019) 11392-11400.
[0014]
[10] Y.Tang, C.Yang, Summary of the Invention
[0015] The purpose of this invention is to provide a resistive switching memory (RSM) based on a maccene-titanium oxide Schottky junction and its fabrication method. By using new materials and designing the device structure, the uniformity of the RSM is improved. Utilizing the spontaneous introduction of defect traps during the preparation of maccene materials, an interface barrier modulation RSM based on the maccene-titanium oxide Schottky junction is constructed. Since the resistance switching behavior occurs throughout the entire maccene-titanium oxide interface, the constructed device exhibits high uniformity, strong durability, and stable cycle performance. Furthermore, by using a semiconductor material as the bottom electrode, a highly uniform self-rectifying RSM can be constructed, providing an effective solution for the application of maccene in the field of large-area memory.
[0016] The technical solution of this invention:
[0017] A resistive switching memory based on a malicene-titanium oxide Schottky junction is disclosed. The resistive switching memory structure consists of a bottom electrode, a resistive switching layer, and a top electrode arranged from bottom to top. The top electrode is malicene, the resistive switching layer is titanium oxide, and the bottom electrode is a metal or semiconductor material. By selecting different bottom electrode materials, resistive switching memories with different characteristics can be realized.
[0018] The aforementioned resistive switching memory based on a macoene-titanium oxide Schottky junction uses Ti3C2T as the macoene material. x High-precision patterning is achieved by combining photolithography and reactive ion etching processes; when semiconductor materials are selected for the bottom electrode, self-rectification characteristics are realized; and silicon wafers are used as both the substrate and the bottom electrode.
[0019] The resistive switching memory based on macoene-titanium oxide Schottky junction is obtained by spin-coating a macoene suspension with a concentration of 10-20 mg / mL onto the substrate surface to obtain a macoene film with a thickness of approximately 20-30 nm.
[0020] The resistive switching memory based on the maicoene-titanium oxide Schottky junction has a titanium oxide resistive switching layer with a thickness of 5-10 nm.
[0021] The aforementioned resistive switching memory based on the Maicoene-titanium oxide Schottky junction has an overall cross-shaped structure. The bottom electrode, resistive switching layer, and top electrode are all cuboid thin layers. The top of the vertical resistive switching layer is perpendicular to the bottom plane of the top electrode, the bottom of the vertical resistive switching layer is perpendicular to the top plane of the bottom electrode, and the top electrode is parallel to the bottom electrode and perpendicular to it in space.
[0022] The method for fabricating the resistive switching memory based on the maicoene-titanium oxide Schottky junction includes the following steps:
[0023] (1) The silicon oxide on the surface of a silicon wafer is thinned using reactive ion etching (RIE) process;
[0024] (2) Prepare metal or semiconductor bottom electrodes using photolithography, metallization and reactive ion etching processes;
[0025] (3) A titanium oxide resistive switching layer is constructed on the bottom electrode using atomic layer deposition;
[0026] (4) Hydrophilic treatment using oxygen plasma;
[0027] (5) Maicoene thin films were prepared using spin coating process;
[0028] (6) Pattern the maicoene thin film to prepare the top electrode.
[0029] In the fabrication method of the resistive switching memory based on the Maicoene-titanium oxide Schottky junction, in step (1), the silicon wafer used is a single-sided polished double-sided thermally oxidized wafer, and after etching, the remaining silicon oxide thickness is 25-35 nm.
[0030] In the fabrication method of the resistive switching memory based on the Maicoene-titanium oxide Schottky junction, the reactive ion etching process parameters in step (1) are as follows: power is 100W, time is 3-4min, and gas pressure is 3.9-4.2Pa.
[0031] In the method for fabricating the resistive switching memory based on the Maicoene-titanium oxide Schottky junction, in step (4), the power of the oxygen plasma is 180-220W, the gas flow rate is 160-200sccm, and the processing time is 4-6min.
[0032] In the fabrication method of the resistive switching memory based on the macoene-titanium oxide Schottky junction, in step (6), the macoene thin film is patterned using a reactive ion etching process with a power of 20-25W, a time of 2-4min, and a pressure of 3.9-4.2Pa.
[0033] The design concept of this invention is:
[0034] This invention utilizes the defects introduced during the preparation of macoene as charge traps to form a space charge layer at the entire macoene-titanium oxide interface, thereby capturing and releasing charge carriers injected by the macoene top electrode, effectively controlling the height of the macoene-titanium oxide Schottky barrier, thus achieving resistive switching behavior and improving device uniformity.
[0035] This invention realizes a resistive switching memory (RSM) based on a maccolin-titanium oxide Schottky junction. Maccolin and titanium oxide serve as the top electrode and resistive switching layer, respectively. Different types of bottom electrode materials can be selected to achieve RSMs with different characteristics. The resistance switching behavior originates from the change in the potential barrier of the maccolin-titanium oxide Schottky junction caused by electric field modulation. Specifically, charge carriers injected by the maccolin top electrode can be captured by charge traps across the entire interface of the maccolin-titanium oxide junction, forming a space charge layer to regulate the barrier height. Therefore, the device exhibits high uniformity, long-term stability, and reliable durability. By using silicon as the bottom electrode, a self-rectified RSM with a high self-rectification ratio can be achieved in the high-resistivity state due to the difference in the height of the upper and lower Schottky barriers.
[0036] The advantages and beneficial effects of this invention are:
[0037] 1. This invention uses malicene as the top electrode and titanium oxide as the resistive switching layer. By selecting different bottom electrode materials, resistive switching memory with different characteristics can be realized. Utilizing the defects inherent in malicene as charge traps, a resistive switching memory based on an interface barrier modulation mechanism is constructed, and the device exhibits high uniformity, long-term stability, and reliable durability.
[0038] 2. By selecting different types of materials as bottom electrodes, this invention can realize a variety of functional resistive switching memory, including self-rectification characteristics. In particular, the use of semiconductor bottom electrodes to construct a highly uniform self-rectifying resistive switching memory demonstrates the broad application prospects of Maikeene in the field of large-area memory devices. Attached Figure Description
[0039] Figure 1 Flowchart for fabrication of the Maicoene-titanium oxide Schottky junction resistive switching memory.
[0040] Figure 2 The current-voltage characteristic curves of the Maicoene-titanium oxide-silicon resistive switching memory with silicon as the bottom electrode are shown.
[0041] Figure 3 The current-voltage characteristic curves of the Maicoene-titanium oxide-titanium resistive switching memory with titanium as the bottom electrode are shown.
[0042] Figure 4 A schematic diagram (a) and a SEM characterization image (b) of the Maicoene-titanium oxide-silicon resistive switching memory structure.
[0043] Figure 5 The figure shows the storage characteristics of the Maicoene-titanium oxide-silicon resistive switching memory, where (a) durability and (b) cycle performance.
[0044] Figure 6 The diagram shows the uniformity characteristics of the Maicoene-titanium oxide-silicon resistive switching memory, where (a) is the uniformity of the high and low resistance states, and (b) is the uniformity of the rectification ratio. Detailed Implementation
[0045] In specific implementation, the construction method of the present invention based on the Maicoene-titanium oxide Schottky junction resistive switching memory is as follows:
[0046] (1) Construct resistive switching memory based on different bottom electrodes of maicoene-titanium oxide Schottky junction, including silicon and titanium as bottom electrodes, and characterize the basic electrical properties.
[0047] (2) The uniformity of the device needs to be evaluated, including the uniformity of the high and low impedance states and the uniformity of the rectification ratio.
[0048] In the experiment, the following processes were optimized to achieve the optimal preparation parameters, mainly through the following attempts:
[0049] A resistive switching memory based on a maicoene-titanium oxide Schottky junction was fabricated using silicon and titanium as bottom electrodes. The device performance was characterized, and the different functions of devices with different bottom electrodes were verified. For example, silicon as the bottom electrode showed obvious rectification characteristics.
[0050] The feasibility of the present invention will be further demonstrated below through examples.
[0051] Example
[0052] like Figure 1 As shown, the fabrication process of the resistive switching memory based on the maicoene-titanium oxide Schottky junction is as follows:
[0053] (1) The silicon wafer used is a single-sided polished double-sided thermally oxidized wafer with a silicon oxide thickness of 100nm. The silicon substrate is thinned by reactive ion etching. The specific etching parameters are: power 100W, time 3-4min and gas pressure 3.9-4.2Pa. The remaining thickness after etching is 25-35nm.
[0054] (2) A silicon bottom electrode was fabricated using photolithography and reactive ion etching processes. The specific parameters were: power 100W, time 1-2min and gas pressure 3.9-4.2Pa.
[0055] (3) After the bottom electrode is completed, a titanium oxide resistive switching layer is grown by atomic layer deposition, with titanium tetraisopropoxide (C) as the precursor. 12 H 28 The mixture consists of O4Ti and water, with a cavity temperature of 250℃, a precursor heating temperature of 80℃, and a titanium oxide resistive switching layer thickness of 5-10nm.
[0056] (4) Use oxygen plasma treatment to improve the hydrophilicity of the substrate. The specific parameters are: power range of 180 to 220 W, gas flow range of 160 to 200 sccm, and treatment time range of 4 to 6 min.
[0057] (5) By spin coating, a 10-20 mg / ml aqueous solution of macoene is selected to obtain a 20-30 nm thick macoene film; then photolithography and development steps are performed, with the following parameters: photolithography time is 4-5 s and development time is 40-50 s. The purpose of these steps is to prepare a mask pattern.
[0058] (6) Electron beam evaporation of 40-60 nm aluminum metal was used as a mask, and reactive ion etching was used to pattern the maicoene. The specific parameters were: power 20-25 W, time 2-4 min and gas pressure 3.9-4.2 Pa.
[0059] (7) Remove the aluminum metal used as a mask, clean it with a weakly alkaline developing solution, and soak for 1-2 minutes.
[0060] like Figure 2 As shown, the Maicoene-titanium oxide-silicon resistive switching memory with silicon as the bottom electrode exhibits excellent resistive switching and rectification characteristics.
[0061] like Figure 3 As shown, the Maicoene-titanium oxide-titanium resistive switching memory with titanium as the bottom electrode exhibits excellent resistive switching characteristics.
[0062] like Figure 4 As shown, the schematic diagram and morphological characterization of the device structure prepared by the present invention are illustrated. In Figure a, the device structure is silicon (p... + The structure is composed of silicon (-Si), titanium dioxide, and malicene from bottom to top, with grounded silicon (p)+ The device uses Si as the bottom electrode, titanium dioxide as the resistive switching layer, and malicene as the top electrode. The overall device has a cross-shaped structure. The bottom electrode, resistive switching layer, and top electrode are all rectangular thin layers. The top of the vertical resistive switching layer is perpendicular to the bottom plane of the top electrode, and the bottom of the vertical resistive switching layer is perpendicular to the top plane of the bottom electrode. The top electrode is parallel to the bottom electrode and spatially perpendicular to it, forming a cross-shaped structure. Figure b shows the SEM image of the device (scale bar: 3μm), and the device size is 100μm. 2 .
[0063] like Figure 5 As shown, the durability and cycle performance of the Maicoene-titanium oxide-silicon resistive switching memory are demonstrated, with the device exhibiting a cycle life exceeding 10. 4 It has data retention capabilities and a cycle life of over 100 times.
[0064] like Figure 6 As shown, the uniformity statistics of the Maikeene-titanium oxide-silicon resistive switching memory show that the device has uniform high and low resistance states and rectification ratio, achieving extremely high uniformity.
[0065] The results of the embodiments show that the resistive switching memory and its fabrication method based on the maccene-titanium oxide Schottky junction of the present invention have the characteristics of high uniformity, strong durability, and stable cycle performance. The use of a semiconductor bottom electrode enables a highly uniform self-rectified resistive switching memory, demonstrating great application potential in the field of large-area maccene-based memory.
Claims
1. A resistive switching memory based on a maicone-titanium oxide Schottky junction, characterized in that, The resistive switching memory structure is composed of a bottom electrode, a resistive switching layer, and a top electrode arranged from bottom to top. The top electrode is malicene, the resistive switching layer is titanium oxide, and the bottom electrode is a metal or semiconductor material. By selecting different bottom electrode materials, resistive switching memory with different characteristics can be realized. Malicene is a type of transition metal carbide, transition metal nitride, or transition metal carbonitride with a two-dimensional layered structure. The defects introduced during the preparation of macoene act as charge traps, forming a space charge layer at the entire macoene-titanium oxide interface. This traps and releases the charge carriers injected by the macoene top electrode, effectively controlling the height of the macoene-titanium oxide Schottky barrier, thereby achieving resistive switching behavior and improving device uniformity. The resistance switching behavior arises from the change in the barrier of the maccene-titanium oxide Schottky junction caused by electric field modulation. That is, the charge carriers injected by the maccene top electrode can be captured by the charge traps of the entire interface of maccene-titanium oxide, forming a space charge layer to regulate the barrier height.
2. The resistive switching memory based on a maicone-titanium oxide Schottky junction according to claim 1, characterized in that, Maikeene material is Ti3C2T x High-precision patterning is achieved by combining photolithography and reactive ion etching processes; when semiconductor materials are selected for the bottom electrode, self-rectification characteristics are realized; and silicon wafers are used as both the substrate and the bottom electrode.
3. The resistive switching memory based on a maicone-titanium oxide Schottky junction according to claim 1, characterized in that, A macoene film with a thickness of 20-30 nm was obtained by spin-coating a macoene suspension with a concentration of 10-20 mg / mL onto the substrate surface.
4. The resistive switching memory based on a maicone-titanium oxide Schottky junction according to claim 1, characterized in that, The thickness of the resistive switching layer titanium oxide is 5~10nm.
5. The resistive switching memory based on a maicone-titanium oxide Schottky junction according to claim 1, characterized in that, The resistive switching memory has a cross-shaped structure. The bottom electrode, resistive switching layer, and top electrode are all cuboid thin layers. The top of the vertical resistive switching layer is perpendicular to the bottom plane of the top electrode, the bottom of the vertical resistive switching layer is perpendicular to the top plane of the bottom electrode, and the top electrode and bottom electrode are parallel and perpendicular in space, forming a cross-shaped structure.
6. A method for fabricating a resistive switching memory based on a maicone-titanium oxide Schottky junction as described in any one of claims 1 to 5, characterized in that, Includes the following steps: (1) The silicon oxide on the surface of a silicon wafer is thinned using reactive ion etching (RIE) process; (2) Prepare metal or semiconductor bottom electrodes using photolithography, metallization and reactive ion etching processes; (3) A titanium oxide resistive switching layer is constructed on the bottom electrode using atomic layer deposition; (4) Hydrophilic treatment using oxygen plasma; (5) Maicoene thin films were prepared using spin coating. (6) Pattern the maicoene thin film to prepare the top electrode.
7. The method for fabricating a resistive switching memory based on a maicone-titanium oxide Schottky junction according to claim 6, characterized in that, In step (1), the silicon wafer used is a single-sided polished double-sided thermally oxidized wafer. After etching, the remaining silicon oxide thickness is 25~35nm.
8. The method for fabricating a resistive switching memory based on a maicone-titanium oxide Schottky junction according to claim 6, characterized in that, In step (1), the reactive ion etching process parameters are as follows: power is 100W, time is 3~4min, and gas pressure is 3.9~4.2Pa.
9. The method for fabricating a resistive switching memory based on a maicone-titanium oxide Schottky junction according to claim 6, characterized in that, In step (4), the power of the oxygen plasma is 180~220W, the gas flow rate is 160~200sccm, and the processing time is 4~6min.
10. The method for fabricating a resistive switching memory based on a maicone-titanium oxide Schottky junction according to claim 6, characterized in that, In step (6), the maicoene film is patterned using reactive ion etching process with a power of 20~25W, a time of 2~4min, and a pressure of 3.9~4.2Pa.
Citation Information
Patent Citations
Resistive-switching memory elements having improved switching characteristics
WO2010118380A2