A modified polystyrene and its production process

By introducing crosslinking agents and oxalyl chloride into modified polystyrene to form a microporous structure, and combining it with ligands and magnetic materials, the problem of low adsorption capacity of modified polystyrene was solved, achieving efficient adsorption and environmentally friendly preparation, which is suitable for the adsorption of azo dyes.

CN117209691BActive Publication Date: 2026-11-17ANHUI HAOYUAN CHEM IND GRP
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202311090440.6
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-08-28
Publication Date
2026-11-17
Estimated Expiration
2043-08-28

AI Technical Summary

Technical Problem

Existing modified polystyrene has a low adsorption capacity for azo dyes, and its preparation process uses highly toxic raw materials and pore-forming agents, making it difficult to produce industrially.

Method used

A hyperbranched hydrophilic modified polymer is formed using a crosslinking agent. A microporous/mesoporous structure is generated by crosslinking with oxaloyl chloride. Ligands and magnetic materials are introduced to form π-π conjugation and electrostatic adsorption, thereby improving the adsorption capacity. The polymer is also easily recovered through coordination bonds.

Benefits of technology

This improved the adsorption capacity of modified polystyrene for azo dyes, avoided the use of highly toxic raw materials, and enabled safe and environmentally friendly industrial production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN117209691B_ABST
    Figure CN117209691B_ABST
Patent Text Reader

Abstract

This invention discloses a modified polystyrene and its production process, belonging to the field of polystyrene synthesis technology. The production process includes the following steps: First, maleic anhydride and toluene are mixed, and styrene, a crosslinking agent, an initiator, and dodecyl mercaptan are added. Under nitrogen protection, the mixture reacts to obtain a hyperbranched hydrophilic modified polymer. Second, the hyperbranched hydrophilic modified polymer and potassium carbonate are added to DMF. Under nitrogen protection, the mixture is stirred and dispersed, and then oxalyl chloride is added. The mixture is heated to reflux and reacted to obtain a micropowder. Third, the micropowder and ligands are mixed in acetonitrile and reacted at room temperature to obtain ligand-grafted micropowder. Fourth, the ligand-grafted micropowder is mixed with methanol, a reducing agent is added, and the mixture is stirred continuously. Under nitrogen protection, the temperature is raised to 40°C, and then a ferrous fluoroborate methanol solution is added. The prepared modified polystyrene is applied in the field of azo dye adsorption, and the adsorption capacity of the modified polystyrene can be improved by process adjustment.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of polystyrene synthesis technology, specifically relating to a modified polystyrene and its production process. Background Technology

[0002] Polystyrene materials, due to their excellent mechanical properties, good chemical stability, and thermal stability, are widely used in wastewater treatment, pharmaceuticals, separation and purification, ion exchange, and imprinted polymers. Modification and alteration of polystyrene have always been a hot topic in polystyrene research. In the field of wastewater treatment, dye wastewater is characterized by its diverse components, stable chemical properties, resistance to degradation, toxicity, harmfulness, and potential carcinogenic and mutagenic risks. Dyes are widely used in industries such as plastics, papermaking, textiles, and clothing. If left untreated, it will not only pose a significant threat to the ecological environment but also hinder sustainable development.

[0003] Azo dyes are dyes containing azo groups (-N=N-) in their structure. They are difficult to degrade naturally after entering environmental water bodies. Methyl orange is a representative anionic azo dye, often used in laboratory acid-base indicators and the textile industry. Its structure contains azo and aromatic structures that are not easily degraded. Conventional biological and chemical treatment methods are time-consuming, require high equipment investment, and are prone to secondary pollution.

[0004] Chinese invention patent CN110128571B discloses a method for preparing and applying modified polystyrene resin. The method involves dispersing sulfonyl chloride polystyrene resin in tetrahydrofuran, reacting it with aminoanthraquinone and a water-soluble compound containing terminal hydroxyl groups under acid-binding agent and micro-reflux conditions, respectively, and obtaining the modified polystyrene resin after washing with water and ethanol. However, aminoanthraquinone is expensive, has a certain degree of toxicity, and is difficult to biodegrade, and its large-scale use is detrimental to the environment. Summary of the Invention

[0005] The purpose of this invention is to provide a modified polystyrene and its production process, which produces a modified polystyrene as an adsorbent to solve the problem of low adsorption capacity of azo dyes.

[0006] The objective of this invention can be achieved through the following technical solutions:

[0007] A process for producing modified polystyrene includes the following steps:

[0008] Step 1: Heat maleic anhydride until completely dissolved, add toluene and mix, then add styrene, crosslinking agent, initiator and dodecyl mercaptan and mix. Under nitrogen protection, heat to 75°C and stir for 24 hours. After the reaction is complete, precipitate with methanol to obtain hyperbranched hydrophilic modified polymer.

[0009] The second step involves adding the hyperbranched hydrophilic modified polymer and potassium carbonate to DMF, stirring and dispersing for 6 hours under nitrogen protection, then adding oxalyl chloride, and refluxing for 16-18 hours. After removing DMF by vacuum concentration, the mixture is dried at 60°C under vacuum to constant weight to obtain micro powder.

[0010] The third step is to mix the micro powder and ligand in acetonitrile and react at room temperature for 5 hours. After the reaction is completed, the mixture is filtered and dried under vacuum at 40°C to obtain the ligand-grafted micro powder.

[0011] Step 4: At room temperature, mix the ligand-grafted micro powder with methanol, ultrasonically disperse for 10 min, add a reducing agent, continue stirring for 10 min, heat to 40°C under nitrogen protection, add ferrous fluoroborate methanol solution, continue stirring and react for 3 h, filter, wash with methanol, and vacuum dry at 40°C to obtain modified polystyrene.

[0012] Furthermore, in the first step, the ratio of maleic anhydride, toluene, styrene, crosslinking agent, initiator and dodecyl mercaptan is 2.1-2.2g: 20-30mL: 4-5g: 0.9-1g: 0.11-0.12g: 2.2-2.4g.

[0013] Furthermore, in the second step, the ratio of the amount of hyperbranched hydrophilic modified polymer, potassium carbonate, DMF and oxalyl chloride is 1-1.2g: 2-2.2g: 50-60mL: 0.1-0.12mL.

[0014] Furthermore, in the third step, the ratio of the amount of micronized powder, ligand, and acetonitrile used is 4.1-4.2g: 0.5-0.6g: 50-60mL.

[0015] Furthermore, in the fourth step, the ratio of ligand-grafted micropowder, methanol, reducing agent, and ferrous fluoroborate methanol solution is 1.8-2g: 30-40mL: 0.5-0.6g: 10-12mL.

[0016] Furthermore, the crosslinking agent is octavinyl-POSS, the initiator is azobisisobutyronitrile, and the reducing agent is ascorbic acid.

[0017] Furthermore, the ligand is one of 4-amino-1,2,4-triazole and 2-aminoethylimidazole.

[0018] A modified polystyrene is prepared by the above-described production process.

[0019] The beneficial effects of this invention are:

[0020] This invention provides a production process for modified polystyrene, which prepares a modified polystyrene for use in the adsorption of azo dyes. The adsorption capacity of the modified polystyrene is improved by adjusting the process. As an adsorption material, its porous structure is key. The preparation process in this invention is safe and environmentally friendly, does not require the addition of porogens, avoids a large amount of highly toxic raw materials, makes up for the shortcomings in the preparation process of polystyrene resin, and is also convenient for industrial production.

[0021] The present invention discloses a production process for modified polystyrene. Firstly, a crosslinking agent is added during the preparation process. Using the crosslinking agent as a branching monomer, a hyperbranched hydrophilic modified polymer is formed. The dendritic macromolecule, due to its unique physical properties, dendritic structure, and numerous active functional groups, provides a large number of adsorption sites for dye molecules. Then, oxalyl chloride is added for secondary crosslinking. The resulting micropores / mesopores can adsorb and accommodate more dye molecules. Furthermore, the larger pores formed after secondary crosslinking prevent pore blockage. The -C=O groups in the oxalyl chloride structure interact with dye molecules through π-π conjugation and electrostatic adsorption. These interactions, along with the -N= bonds in the subsequently introduced ligands, synergistically adsorb dye molecules, further enhancing the adsorption capacity. Finally, by loading a magnetic material onto the surface, polymer recovery is facilitated. The magnetic material forms coordination bonds with the ligands, which, after coordination, can coordinate with azo dye molecules, improving the selective adsorption of azo dye molecules and further enhancing the adsorption capacity. Attached Figure Description

[0022] The invention will now be further described with reference to the accompanying drawings.

[0023] Figure 1 This is a graph showing the absorption rate of methyl orange obtained by adjusting the sample amounts of Example 1 and Comparative Examples 1-3 in this invention. Detailed Implementation

[0024] The technical solutions of the present invention will be clearly and completely described below with reference to the embodiments of the present invention. Obviously, the described embodiments are only some embodiments of the present invention, and not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those of ordinary skill in the art without creative effort are within the scope of protection of the present invention.

[0025] Example 1

[0026] A process for producing modified polystyrene includes the following steps:

[0027] Step 1: Heat 2.1g of maleic anhydride to 60℃ until completely dissolved, add 20mL of toluene and mix, then add 4g of styrene, 0.9g of octavinyl-POSS, 0.11g of azobisisobutyronitrile and 2.2g of dodecyl mercaptan and mix. Under nitrogen protection, heat to 75℃ and stir for 24h. After the reaction is complete, precipitate with methanol to obtain hyperbranched hydrophilic modified polymer.

[0028] Step 2: Take 1g of hyperbranched hydrophilic modified polymer and 2g of potassium carbonate and add them to 50mL of DMF (N,N-dimethylformamide). Under nitrogen protection, stir and disperse for 6h. Then add 0.1mL of oxaloyl chloride and reflux for 16h. After concentration under reduced pressure to remove DMF, dry under vacuum at 60℃ to constant weight to obtain micro powder.

[0029] Step 3: Take 4.1g of micro powder and 0.5g of 4-amino-1,2,4-triazole and add them to 50mL of acetonitrile and mix. React at room temperature (around 25℃) for 5h. After the reaction is completed, filter and vacuum dry at 40℃ to obtain ligand-grafted micro powder.

[0030] Step 4: At room temperature (around 25°C), mix 1.8g of ligand-grafted micropowder with 30mL of methanol, sonicate for 10min, add 0.5g of ascorbic acid, continue stirring for 10min, heat to 40°C under nitrogen protection, add 10mL of ferrous fluoroborate methanol solution, which is a mixture of ferrous fluoroborate hexahydrate and methanol at a ratio of 0.5g:10mL, continue stirring and reacting for 3h, filter, wash with methanol, and vacuum dry at 40°C to obtain modified polystyrene.

[0031] Example 2

[0032] A process for producing modified polystyrene includes the following steps:

[0033] Step 1: Heat 2.2g of maleic anhydride to 60℃ until completely dissolved, add 30mL of toluene and mix, then add 5g of styrene, 1g of octavinyl-POSS, 0.12g of azobisisobutyronitrile and 2.4g of dodecyl mercaptan and mix. Under nitrogen protection, heat to 75℃ and stir for 24h. After the reaction is complete, precipitate with methanol to obtain hyperbranched hydrophilic modified polymer.

[0034] The second step involves adding 1.2g of hyperbranched hydrophilic modified polymer and 2.2g of potassium carbonate to 60mL of DMF (N,N-dimethylformamide). Under nitrogen protection, the mixture is stirred and dispersed for 6 hours. Then, 0.12mL of oxaloyl chloride is added, and the mixture is refluxed for 18 hours. After concentration under reduced pressure to remove DMF, the mixture is dried under vacuum at 60℃ to constant weight to obtain micro powder.

[0035] Step 3: Take 4.2g of micro powder and 0.6g of 4-amino-1,2,4-triazole and add them to 60mL of acetonitrile and mix. React at room temperature (around 25℃) for 5h. After the reaction is completed, filter and vacuum dry at 40℃ to obtain ligand-grafted micro powder.

[0036] Step 4: At room temperature (around 25°C), mix 2g of ligand-grafted micropowder with 40mL of methanol, sonicate for 10min, add 0.6g of ascorbic acid, continue stirring for 10min, heat to 40°C under nitrogen protection, add 12mL of ferrous fluoroborate methanol solution, which is a mixture of ferrous fluoroborate hexahydrate and methanol at a ratio of 0.5g:10mL, continue stirring and reacting for 3h, filter, wash with methanol, and vacuum dry at 40°C to obtain modified polystyrene.

[0037] Example 3

[0038] A process for producing modified polystyrene includes the following steps:

[0039] Step 1: Heat 2.2g of maleic anhydride to 60℃ until completely dissolved, add 30mL of toluene and mix, then add 5g of styrene, 1g of octavinyl-POSS, 0.12g of azobisisobutyronitrile and 2.4g of dodecyl mercaptan and mix. Under nitrogen protection, heat to 75℃ and stir for 24h. After the reaction is complete, precipitate with methanol to obtain hyperbranched hydrophilic modified polymer.

[0040] The second step involves adding 1.2g of hyperbranched hydrophilic modified polymer and 2.2g of potassium carbonate to 60mL of DMF (N,N-dimethylformamide). Under nitrogen protection, the mixture is stirred and dispersed for 6 hours. Then, 0.12mL of oxaloyl chloride is added, and the mixture is refluxed for 18 hours. After concentration under reduced pressure to remove DMF, the mixture is dried under vacuum at 60℃ to constant weight to obtain micro powder.

[0041] Step 3: Take 4.2g of micro powder and 0.6g of 2-aminoethylimidazolium and add them to 60mL of acetonitrile. Mix them and react at room temperature (around 25℃) for 5h. After the reaction is completed, filter and vacuum dry at 40℃ to obtain ligand-grafted micro powder.

[0042] Step 4: At room temperature (around 25°C), mix 2g of ligand-grafted micropowder with 40mL of methanol, sonicate for 10min, add 0.6g of ascorbic acid, continue stirring for 10min, heat to 40°C under nitrogen protection, add 12mL of ferrous fluoroborate methanol solution, which is a mixture of ferrous fluoroborate hexahydrate and methanol at a ratio of 0.5g:10mL, continue stirring and reacting for 3h, filter, wash with methanol, and vacuum dry at 40°C to obtain modified polystyrene.

[0043] Comparative Example 1

[0044] Compared with Example 1, this comparative example does not undergo hyperbranching treatment (no crosslinking agent is added). The specific steps are as follows:

[0045] Step 1: Heat 2.1g of maleic anhydride to 60℃ until completely dissolved, add 20mL of toluene and mix, then add 4g of styrene, 0.11g of azobisisobutyronitrile and 2.2g of dodecyl mercaptan and mix. Under nitrogen protection, heat to 75℃ and stir for 24h. After the reaction is complete, precipitate with methanol to obtain the hydrophilic modified polymer.

[0046] Step 2: Take 1g of hydrophilic modified polymer and 2g of potassium carbonate and add them to 50mL of DMF (N,N-dimethylformamide). Under nitrogen protection, stir and disperse for 6h. Then add 0.1mL of oxaloyl chloride and reflux for 16h. After concentration under reduced pressure to remove DMF, dry under vacuum at 60℃ to constant weight to obtain micro powder.

[0047] Step 3: Take 4.1g of micro powder and 0.5g of 4-amino-1,2,4-triazole and add them to 50mL of acetonitrile and mix. React at room temperature (around 25℃) for 5h. After the reaction is completed, filter and vacuum dry at 40℃ to obtain ligand-grafted micro powder.

[0048] Step 4: At room temperature (around 25°C), mix 1.8g of ligand-grafted micropowder with 30mL of methanol, sonicate for 10min, add 0.5g of ascorbic acid, continue stirring for 10min, heat to 40°C under nitrogen protection, add 10mL of ferrous fluoroborate methanol solution, which is a mixture of ferrous fluoroborate hexahydrate and methanol at a ratio of 0.5g:10mL, continue stirring and reacting for 3h, filter, wash with methanol, and vacuum dry at 40°C to obtain modified polystyrene.

[0049] Comparative Example 2

[0050] Compared with Example 2, this comparative example does not perform the second step of processing. The specific steps are as follows:

[0051] Step 1: Heat 2.1g of maleic anhydride to 60℃ until completely dissolved, add 20mL of toluene and mix, then add 4g of styrene, 0.11g of azobisisobutyronitrile and 2.2g of dodecyl mercaptan and mix. Under nitrogen protection, heat to 75℃ and stir for 24h. After the reaction is complete, precipitate with methanol to obtain the hydrophilic modified polymer.

[0052] The second step involves mixing 4.1g of the hydrophilic modified polymer and 0.5g of 4-amino-1,2,4-triazole in 50mL of acetonitrile and reacting at room temperature (around 25℃) for 5 hours. After the reaction is complete, the mixture is filtered and dried under vacuum at 40℃ to obtain ligand-grafted micro powder.

[0053] Step 3: At room temperature (around 25°C), 1.8g of ligand-grafted micropowder and 30mL of methanol were mixed and ultrasonically dispersed for 10min. 0.5g of ascorbic acid was added and stirring was continued for 10min. Under nitrogen protection, the temperature was raised to 40°C and 10mL of ferrous fluoroborate methanol solution was added. The ferrous fluoroborate methanol solution was prepared by mixing ferrous fluoroborate hexahydrate and methanol at a ratio of 0.5g:10mL. The reaction was continued by stirring for 3h. After filtration, washing with methanol, and vacuum drying at 40°C, modified polystyrene was obtained.

[0054] Comparative Example 3

[0055] Compared with Example 3, this comparative example does not perform the first step processing or the second step processing. The specific steps are as follows:

[0056] Step 1: Heat 2.1g of maleic anhydride to 60℃ until completely dissolved, add 20mL of toluene and mix, then add 4g of styrene, 0.11g of azobisisobutyronitrile and 2.2g of dodecyl mercaptan and mix. Under nitrogen protection, heat to 75℃ and stir for 24h. After the reaction is complete, precipitate with methanol to obtain the hydrophilic modified polymer.

[0057] The second step involves mixing 4.1g of the hydrophilic modified polymer and 0.5g of 4-amino-1,2,4-triazole in 50mL of acetonitrile and reacting at room temperature (around 25℃) for 5 hours. After the reaction is complete, the mixture is filtered and dried under vacuum at 40℃ to obtain the modified polystyrene.

[0058] The samples prepared in Example 1 and Comparative Examples 1-3 were tested. 0.5, 1.0, 1.5, 2.0, 2.5, 3.0, 3.5, 4.0, 4.5, and 5.0 mg of the samples prepared in Example 1 and Comparative Examples 1-3 were weighed and added to 5 mL of a 40 mg / L methyl orange solution. The pH was adjusted to approximately 2.5, and the solution was shaken in a shaker for 90 min. The samples were then separated and adsorbed. The absorbance values ​​of the solutions before and after adsorption were measured, and the absorbance values ​​were recorded. Example 1 was designated as Group A, Comparative Example 1 as Group B, Comparative Example 2 as Group C, and Comparative Example 3 as Group D. The results are referred to [reference needed]. Figure 1 As shown. From Figure 1As can be seen, the modified polystyrene prepared according to the production process disclosed in this invention has good adsorption performance, high yield, and higher absorption capacity compared to the sample in the comparative example. After adsorption, the modified polystyrene adsorbed with methyl orange was placed in water, sonicated, and then dried for continued use, maintaining good adsorption performance.

[0059] It should be noted that, in this document, relational terms such as "first" and "second" are used only to distinguish one entity or operation from another, and do not necessarily require or imply any such actual relationship or order between these entities or operations. Furthermore, the terms "comprising," "including," or any other variations thereof are intended to cover non-exclusive inclusion, such that a process, method, article, or apparatus that comprises a list of elements includes not only those elements but also other elements not expressly listed, or elements inherent to such process, method, article, or apparatus.

[0060] Although embodiments of the invention have been shown and described, it will be understood by those skilled in the art that various changes, modifications, substitutions and alterations can be made to these embodiments without departing from the principles and spirit of the invention, the scope of which is defined by the appended claims and their equivalents.

Claims

1. A process for producing modified polystyrene, characterized by, Includes the following steps: Step 1: Heat maleic anhydride until it is completely dissolved, add toluene and mix, then add styrene, crosslinking agent, initiator and dodecyl mercaptan and mix. Under nitrogen protection, heat to 75°C and stir for 24 hours. After the reaction is complete, precipitate with methanol to obtain hyperbranched hydrophilic modified polymer. The second step involves adding the hyperbranched hydrophilic modified polymer and potassium carbonate to DMF, stirring and dispersing for 6 hours under nitrogen protection, then adding oxalyl chloride, and refluxing for 16-18 hours. After removing DMF by vacuum concentration, the mixture is dried at 60°C under vacuum to constant weight to obtain micro powder. The third step is to mix the micro powder and ligand in acetonitrile and react at room temperature for 5 hours. After the reaction is completed, the mixture is filtered and dried under vacuum at 40°C to obtain the ligand-grafted micro powder. Step 4: At room temperature, mix the ligand-grafted micro powder with methanol, disperse by ultrasonication, add a reducing agent, continue stirring, raise the temperature to 40°C under nitrogen protection, add ferrous fluoroborate methanol solution, continue stirring and react for 3 hours, filter, wash with methanol, and vacuum dry at 40°C to obtain modified polystyrene. Wherein, the crosslinking agent is octavinyl-POSS, the initiator is azobisisobutyronitrile, the reducing agent is ascorbic acid, and the ligand is 4-amino-1,2,4-triazole.

2. The process for producing modified polystyrene according to claim 1, characterized by, In the first step, the ratio of maleic anhydride, toluene, styrene, crosslinking agent, initiator and dodecyl mercaptan is 2.1-2.2g: 20-30mL: 4-5g: 0.9-1g: 0.11-0.12g: 2.2-2.4g.

3. The process for producing modified polystyrene according to claim 1, characterized by, In the second step, the ratio of the amount of hyperbranched hydrophilic modified polymer, potassium carbonate, DMF and oxaloyl chloride is 1-1.2g: 2-2.2g: 50-60mL: 0.1-0.12mL.

4. The process for producing modified polystyrene according to claim 1, characterized by, In the third step, the ratio of the amount of micronized powder, ligand, and acetonitrile used is 4.1-4.2g: 0.5-0.6g: 50-60mL.

5. The process for producing modified polystyrene according to claim 1, characterized by, In the fourth step, the ratio of ligand-grafted micropowder, methanol, reducing agent, and ferrous fluoroborate methanol solution is 1.8-2g: 30-40mL: 0.5-0.6g: 10-12mL.

6. A modified polystyrene characterized by, It is prepared by the production process described in any one of claims 1-5.

Citation Information

Patent Citations

  • A method for preparing modified polystyrene resin and its application

    CN110128571B

  • Preparation method of hyperbranched multifunctional dispersant

    CN104211849A

  • Method for preparing super-crosslinked polyaniline by using N-alkylation reaction

    CN114957737A