A method for enhancing the mechanical properties of fluoropolymers and fluoropolymers
By treating fluoropolymers with an F2/N2 mixed gas, oxygen and other oxygen-containing gases are used to enhance the reactivity of fluoropolymers and promote cross-linking reactions. This solves the problems of complexity and high cost in improving the mechanical properties of fluoropolymers in existing technologies, and achieves significant improvement in mechanical properties, making it suitable for chemical equipment.
Patent Information
- Application Number
- CN202311105097.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-08-30
- Publication Date
- 2026-11-10
- Estimated Expiration
- 2043-08-30
AI Technical Summary
Existing technologies for enhancing the mechanical properties of fluoropolymers suffer from problems such as complex methods, high costs, and poor enhancement effects, especially the uneven dispersion of fillers and the high cost of modified monomers.
Fluoropolymers are treated with an F2/N2 mixed gas. By controlling the temperature and time, the fluoropolymers are brought into contact with the reinforcing gas. The process includes infiltration, reaction, and fluorination steps. Oxygen-containing gases such as oxygen enhance the reactivity of the fluoropolymers, promote cross-linking reactions, and improve mechanical properties.
It achieves a simple, low-cost, and highly effective improvement in the mechanical properties of fluoropolymers, significantly enhancing yield strength, tensile strength at break, and Shore hardness, making it suitable for chemical equipment such as pumps and valves.
Smart Images

Figure BDA0004421846060000161 
Figure BDA0004421846060000171 
Figure BDA0004421846060000181
Abstract
Description
[Technical Field]
[0001] This invention belongs to the field of fluorochemical technology, specifically relating to the field of enhancing the mechanical properties of fluoropolymers. [Background Technology]
[0002] Fluoropolymers, especially perfluoropolymers, are a special class of polymeric materials. Because fluorine atoms are the most electronegative of all elements, their van der Waals radii are small, and the CF bond energy is as high as 485 kJ / mol, making it the most energetic covalent single bond. The presence of numerous CF groups gives fluoropolymers excellent chemical resistance, heat resistance, weather resistance, and abrasion resistance, as well as low surface energy and excellent electrical insulation. Therefore, they are widely used in many industries and fields, including petrochemicals, aerospace, electronics, construction, textiles, transportation, semiconductors, medical, and food.
[0003] In the chemical industry, material transportation is a critical production process. However, many media, such as acids, alkalis, strong oxidants, and organic solvents, can corrode pipelines, fittings, and related equipment used to transport materials. Based on the excellent chemical corrosion resistance, solvent resistance, and heat resistance of fluoropolymers, pipelines, valves, pumps, and other chemical equipment using fluoropolymers as the main material or lining are currently the optimal choice for transporting corrosive media.
[0004] Materials widely used in fluoropolymer-lined pipes, valves, and pumps include polytetrafluoroethylene (PTFE), perfluoroethylene propylene (PFEP), and tetrafluoroethylene-perfluoroalkyl vinyl ether copolymers. These materials are typically used in applications requiring high temperature and corrosion resistance. However, due to their relatively low hardness, and especially the "cold flow" phenomenon in PTFE, significant deformation occurs after prolonged use, and the material strength degrades rapidly. As technology advances, the performance requirements for materials are increasingly stringent. Ordinary materials cannot meet the demands of more demanding applications and may pose safety hazards. Therefore, there is an urgent need to further improve the mechanical properties of these fluoropolymers, giving them higher strength and hardness, enabling their application in situations with higher performance requirements.
[0005] Currently, enhancing the mechanical properties of fluoropolymer materials is mainly achieved through blending or copolymerization. For example, patent EP0857756 discloses a resin composition blended with a fluorinated vinyl polymer containing specific functional groups and fillers, which exhibits improved mechanical properties. The method for reinforcing fluoropolymers primarily utilizes inorganic fillers such as carbon fibers, silica, aluminum borate, molybdenum disulfide, bronze, and aramid fibers, or non-meltable organic fillers. However, a common problem with blending fillers with fluoropolymers is uneven filler dispersion, leading to poor reinforcement, weak points in the material, and coloring issues affecting appearance due to the introduction of some fillers. Using dispersants or introducing surface-active functional groups such as hydroxyl and carboxyl groups into fluoropolymers can decrease the material's thermal stability and accelerate aging. Patent CN115490797 provides a method for improving the creep resistance of suspended PTFE. By adding a second monomer, perfluoropropyl vinyl ether, and a third monomer (an addition product of 2-aminodiphenyl sulfide and divinyl sulfone), the creep resistance of the polytetrafluoroethylene suspension resin is enhanced, thereby improving the mechanical strength of the product. Using modified monomer copolymerization to improve the mechanical properties of materials has the problem of requiring stricter control over the polymerization reaction conditions. The content and uniformity of the modified monomer copolymerization have a significant impact on the mechanical properties and temperature resistance of the product. Furthermore, modified monomers are often expensive, significantly increasing the production cost of the material.
[0006] Therefore, finding a simple, low-cost, and highly effective method for reinforcing fluoropolymers is currently a key challenge that the industry urgently needs to overcome. [Summary of the Invention]
[0007] To address the problems existing in the current technology for enhancing the mechanical properties of fluoropolymers, this invention provides a simple, low-cost method for enhancing the mechanical properties of fluoropolymers, as well as the fluoropolymer obtained therefrom.
[0008] To solve the above-mentioned technical problems, the present invention adopts the following technical solution:
[0009] First, the present invention provides a method for enhancing the mechanical properties of fluoropolymers, comprising the following steps:
[0010] Step 1: In the reactor, the fluoropolymer is brought into contact with the oxygen-containing reinforcing gas at 60-180℃ for a set time t1, where t1 ≥ 1 min;
[0011] Step 2: Add F2 / N2 mixture A to the reactor, and let the fluoropolymer and F2 / N2 / reinforcing gas mixture B contact at 150-250℃ for a set time t2, where t2≥1min;
[0012] Step 3: After removing the F2 / N2 / enhancing gas mixture B from the reactor, or replacing it with a new reactor, add the F2 / N2 mixture C back into the reactor, and allow the fluoropolymer to contact the F2 / N2 mixture C at 150-200℃ for a set time t3, where t3 ≥ 1 min.
[0013] Preferably, the F2 / N2 mixture A contains the following components in molar proportions: 5-20 parts of fluorine gas and 80-95 parts of nitrogen gas.
[0014] Preferably, the F2 / N2 mixture C contains the following components in molar proportions: 15-30 parts of fluorine gas and 70-85 parts of nitrogen gas.
[0015] Preferably, the enhancing gas is any one or any combination of two or more of oxygen, carbon monoxide, nitric oxide, nitrogen dioxide, and sulfur dioxide.
[0016] Preferably, the amount of the reinforcing gas added in step one accounts for 0.05%-1% of the total molar fraction of fluorine in the F2 / N2 mixture A in step two.
[0017] Preferably, in step one, 1h≤t1≤6h; and / or, the fluoropolymer is contacted with the reinforcing gas carrying oxygen atoms at 90-150°C.
[0018] Preferably, in step two, 1h≤t2≤6h; and / or, the fluoropolymer is contacted with the mixture B of F2 / N2 / reinforcing gas at 180-220°C.
[0019] Preferably, in step three, 1h≤t3≤6h; and / or, the fluoropolymer is contacted with the F2 / N2 mixed gas C at 150-200°C.
[0020] Preferably, the fluoropolymer is any one of perfluoroethylene propylene, tetrafluoroethylene-perfluoroalkyl vinyl ether copolymer, and polytetrafluoroethylene suspension resin.
[0021] In another aspect, the present invention also provides a fluoropolymer, which is obtained by treating the fluoropolymer using the above-described method, thereby enhancing the mechanical properties of the fluoropolymer.
[0022] Treating fluoropolymers with an F2 / N2 mixture is a well-known and widely used method for treating unstable end groups in fluoropolymers. This method utilizes the strong reactivity of F2; at a certain temperature, fluorine radicals attack the C-C bonds connecting the unstable end groups to the main chain of the fluoropolymer, thereby removing the unstable end groups. This process involves multiple free radical reactions. If the F2 content is too high, the reactivity is too strong, leading to the breakage of the fluoropolymer main chain and causing material degradation; if the F2 content is too low, the unstable end groups will not be fully reacted.
[0023] In their experimental study using an F2 / N2 mixture to treat fluoropolymers, the applicant surprisingly discovered that under low F2 concentrations, unstable end groups could not be fully reacted. However, the addition of a certain amount of oxygen, carbon monoxide, nitric oxide, nitrogen dioxide, or sulfur dioxide—similar to oxygen-containing gases—as reinforcing gases, enhanced the reactivity of the original F2, making the unstable end groups more readily reacted and resulting in cross-linked polymers. The applicant hypothesizes that these substances, in the reaction system, form peroxy radicals with fluorine radicals, promoting the cross-linking of -CF2 radicals.
[0024] Therefore, based on the above findings, the technical solution adopted in this invention is as follows:
[0025] Step one is the process of enhancing gas permeation, which involves contacting the fluoropolymer with the oxygen-containing reinforcing gas at 60-180℃ for a set time. Because fluoropolymers have strong resistance to permeation, in order to achieve the goal of enhancing the mechanical properties of fluoropolymers through chemical reaction, the reaction gas needs to be permeated first; otherwise, the reaction uniformity will be poor, affecting the enhancement effect.
[0026] Step two involves the reaction process of the F2 / N2 / reinforcing gas mixture. The fluoropolymer is brought into contact with the F2 / N2 / reinforcing gas mixture B at 150-250°C for a set time. Through chemical reaction, the molecular structure of the fluoropolymer changes, thereby enhancing its mechanical properties.
[0027] Step 3 involves contacting the fluoropolymer with the F2 / N2 mixed gas C at 150-200℃ for a set time to fluorinate any remaining unstable end groups in the F2 / N2 mixed gas, thus ensuring the product's performance.
[0028] Compared with the prior art, the present invention has the following beneficial effects:
[0029] 1. The process is simple and the raw materials are inexpensive.
[0030] 2. The gas-solid contact reaction is sufficient, and the F2 / N2 / reinforcing gas mixture has strong permeability, resulting in excellent reinforcement effect and good uniformity.
[0031] These features and advantages of the present invention will be disclosed in detail in the following specific embodiments.
Detailed Implementation Methods
[0032] The technical solution of the present invention will be explained and described below with reference to the embodiments of the present invention. However, the following embodiments are only preferred embodiments of the present invention and not all of them. Other embodiments obtained by those skilled in the art based on the embodiments in the implementation methods without creative effort are all within the protection scope of the present invention.
[0033] This invention provides a method for enhancing the mechanical properties of fluoropolymers, comprising the following steps:
[0034] Step 1: In the reactor, a certain amount of oxygen-containing reinforcing gas is used to contact the fluoropolymer at 60-180℃ for a certain period of time.
[0035] The reinforcing gas is any one or more of oxygen, carbon monoxide, nitric oxide, nitrogen dioxide, and sulfur dioxide.
[0036] Step 2: Add F2 / N2 mixture A, and let F2 / N2 / reinforcing gas mixture B contact with fluoropolymer at 150-250℃ for a certain period of time.
[0037] Step 3: Remove the F2 / N2 / enhancing gas mixture B, or replace it with a new reactor and use the F2 / N2 mixture C to contact the fluoropolymer at 150-200℃ for a certain period of time.
[0038] Step one is to enhance the permeation process of the gas. Because fluoropolymers have strong resistance to permeation, in order to enhance the mechanical properties of fluoropolymers through chemical reaction, the reaction gas needs to be permeated first. Otherwise, the reaction uniformity will be poor, affecting the enhancement effect.
[0039] Step two involves the reaction of the F2 / N2 / reinforcing gas mixture. Through chemical reaction, the molecular structure of the fluoropolymer changes, thereby enhancing its mechanical properties.
[0040] Step 3 involves fluorinating the remaining unstable end groups with an F2 / N2 mixed gas to ensure product performance.
[0041] The F2 / N2 mixture A used in step two contains the following components in molar proportions:
[0042] Fluorine gas 5-20 parts; nitrogen gas 80-95 parts.
[0043] The method for enhancing the mechanical properties of fluoropolymers mainly utilizes the molecular chain cross-linking initiated by fluorine gas. Insufficient fluorine gas will prevent the corresponding reaction from occurring, while excessive fluorine gas, due to its high reactivity, will cause the reaction to be too vigorous, potentially destroying the formed cross-linking points and posing significant safety risks. Therefore, the molar fraction of fluorine gas in the F2 / N2 mixture A is controlled between 5% and 20%. Preferably, the molar fraction of fluorine gas in the F2 / N2 mixture A is controlled between 8% and 15%.
[0044] The F2 / N2 mixture C used in step three contains the following components in molar proportions:
[0045] Fluorine gas 15-30 parts; nitrogen gas 70-85 parts.
[0046] Step one enhances the gas permeation process. This step is necessary to ensure the uniformity of the reaction and requires maintaining a specific temperature and time to guarantee the permeation effect. The temperature in step one is controlled between 60-180℃. Too low a temperature results in poor gas permeation, while too high a temperature does not significantly enhance permeation but instead increases energy consumption. The optimal temperature varies depending on the type of fluoropolymer. Preferably, it is 80-120℃ for perfluoroethylene propylene; 100-150℃ for tetrafluoroethylene-perfluoroalkyl vinyl ether copolymer; and 140-180℃ for polytetrafluoroethylene suspension resin.
[0047] Step 1 emphasizes controlling the contact time between the enhanced gas and the fluoropolymer to between 1 minute and 12 hours. Too short a contact time will not achieve uniform gas penetration, while too long a contact time will negatively impact production efficiency and waste energy.
[0048] In this invention, the degree of molecular chain cross-linking is controlled by adjusting the amount of reinforcing gas added. Too little gas will not achieve the desired effect, while too much gas will result in excessive cross-linking, making processing impossible. The amount of reinforcing gas added is controlled to be 0.05%-1% of the total molar fraction of fluorine gas used in step two.
[0049] Step two involves the reaction of a mixture of F2 / N2 and reinforcing gas. The added reinforcing gas, under the influence of fluorine free radicals, promotes cross-linking of the fluoropolymer molecular chains. The temperature in step two is controlled between 150-250℃. Too low a temperature will not achieve the reinforcing effect, while too high a temperature will cause molecular chain breakage and performance degradation. The optimal temperature varies depending on the type of fluoropolymer. Preferably, it is 150-180℃ for perfluoroethylene propylene; 160-200℃ for tetrafluoroethylene-perfluoroalkyl vinyl ether copolymer; and 200-240℃ for polytetrafluoroethylene suspension resin.
[0050] In step two, the contact time between the F2 / N2 / reinforcing gas mixture and the fluoropolymer should be controlled between 1 minute and 36 hours. Too short a contact time results in low cross-linking degree, failing to achieve the reinforcing effect; too long a contact time leads to excessive cross-linking, making the polymer difficult to process.
[0051] Step three involves the fluorination treatment of residual unstable end groups using an F2 / N2 mixed gas to ensure product performance. The added F2 / N2 mixed gas C has a higher fluorine content than the F2 / N2 mixed gas A used in step two to ensure sufficient reaction with the residual unstable end groups. However, the reaction temperature and contact time are lower than in step two to prevent damage to the formed cross-linked structure. The temperature in step three is controlled at 150-200℃, and the contact time is controlled at 1 min-12 h.
[0052] In this invention, there are no particular restrictions on the manufacturing method of the fluoropolymer to be treated, and it can be obtained by any conventional polymerization method.
[0053] In this invention, there are no particular restrictions on the form of the fluoropolymer; it can be in granular or powder form.
[0054] In this invention, there are no limitations on the contact method and reaction site between the mixed gas and the fluoropolymer. Common industrial gas-solid reaction methods can be used, and the reaction apparatus can be a batch reactor, tower reactor, cylindrical reactor, tubular reactor, fixed bed reactor, fluidized bed reactor, or other commonly used industrial reaction apparatus.
[0055] In this invention, the method for treating fluoropolymers with mixed gas can be either batch reaction or continuous reaction.
[0056] One feasible implementation involves initially feeding the fluoropolymer to be treated into a reactor, introducing a certain amount of reinforcing gas, heating the reactor to 60-180°C, and maintaining this temperature for 1 minute to 12 hours to complete step one. Then, a certain amount of F2 / N2 mixed gas is introduced, raising the reactor temperature to 150-250°C, and reacting for 1 minute to 36 hours to complete step two. Next, the system is evacuated, and a certain amount of F2 / N2 mixed gas is introduced, controlling the reactor temperature at 150-200°C to obtain the reinforced fluoropolymer product. Since the gas-solid contact in a batch reactor is insufficient, preferably, the contact time in step one is 8-12 hours, the reaction time in step two is 12-36 hours, and the reaction time in step three is 8-12 hours.
[0057] In one feasible implementation, the fluoropolymer to be treated is introduced into a reaction tube, which is heated to 60-180°C, and a reinforcing gas is continuously introduced for 1 minute to 12 hours to complete step one. Then, a certain amount of F2 / N2 mixture A is mixed into the introduced reinforcing gas, the reaction tube is heated to 150-250°C, and the F2 / N2 / reinforcing gas mixture is continuously introduced for 1 minute to 36 hours to complete step two. Then, the introduction of the F2 / N2 / reinforcing gas mixture is stopped, and an F2 / N2 mixture C is introduced, controlling the reaction tube temperature at 150-200°C, and reacting for 1 minute to 12 hours to obtain the reinforced fluoropolymer product. The tubular reactor enhances the gas-solid contact effect by continuously introducing gas. Preferably, the contact time in step one is 1-3 hours, the reaction time in step two is 4-12 hours, and the reaction time in step three is 2-4 hours.
[0058] One feasible implementation uses a series of fluidized bed reactors. In reactor 1, a reinforcing gas and the fluoropolymer to be treated are continuously introduced, ensuring sufficient contact between the fluoropolymer and the reinforcing gas in the reactor bed. The reactor bed temperature is controlled at 60-180°C. The fluoropolymer then enters reactor 2. In reactor 2, an F2 / N2 mixture A is continuously introduced, reacting with the fluoropolymer and reinforcing gas from reactor 1 in the reactor bed. The reactor bed temperature is controlled at 150-250°C. The treated fluoropolymer leaves reactor 2 and enters a separator for gas-solid separation. The resulting fluoropolymer enters reactor 3, where an F2 / N2 mixture C is continuously introduced, ensuring sufficient contact between the fluoropolymer and the F2 / N2 mixture C in the reactor bed. The reactor bed temperature is controlled at 150-200°C, ultimately yielding the reinforced fluoropolymer product. The contact time between the mixture and the fluoropolymer in reactor 1 is 1-5 minutes, the reaction time in reactor 2 is 1-10 minutes, and the reaction time in reactor 3 is 1-5 minutes.
[0059] In this invention, by using a method to enhance the mechanical properties of fluoropolymers, the fluoropolymers are treated to increase the yield strength by more than 10%, the tensile breaking strength by more than 15%, the tensile modulus by more than 15%, and the Shore hardness by more than 10% compared to before treatment.
[0060] This invention also provides a fluoropolymer, including an enhanced fluoropolymer product obtained using the above-described treatment method. When applied in the pump and valve field, it exhibits improved performance, specifically higher strength, hardness, and resistance to deformation.
[0061] The present invention will now be described in detail with reference to specific embodiments. These embodiments will help those skilled in the art to further understand the present invention, but do not limit the invention in any way.
[0062] Unless otherwise stated, all materials used in this invention are commercially available conventional materials.
[0063] The fluoropolymer products used in this invention are tested for yield strength, tensile breaking strength, tensile modulus and Shore hardness according to relevant testing standards before processing. The test data results are shown in the corresponding data table.
[0064] Example 1
[0065] Add 1 kg of polytetrafluoroethylene propylene granules to a 10 L reactor, evacuate the reactor, replace with high-purity nitrogen to control the oxygen content inside the reactor to less than 10 ppm, and continue evacuating the reactor until the absolute pressure inside the reactor is less than 5 Pa.
[0066] Step 1: Raise the temperature of the reactor to 60°C, introduce oxygen until the absolute pressure inside the reactor is 0.36 kPa, and let it stand for 8 hours;
[0067] Step 2: Introduce F2 / N2 mixed gas A until the absolute pressure inside the reactor is 300.36 kPa, the molar content of F2 in F2 / N2 mixed gas A is 12%, raise the reactor temperature to 180℃, and react for 24 hours;
[0068] Step 3: Exhaust the gas inside the reactor, evacuate and replace the evacuation, and introduce F2 / N2 mixed gas B until the absolute pressure inside the reactor is 300 kPa. The molar content of F2 in F2 / N2 mixed gas B is 30%. Control the reactor temperature at 150℃ and react for 10 hours.
[0069] Then, the air is vented, and the material is replaced and cooled to obtain treated perfluoroethylene propylene granules.
[0070] The obtained polytetrafluoroethylene propylene granules were tested for yield strength, tensile breaking strength, tensile modulus and Shore hardness according to relevant testing standards. The test data results are shown in Table 1.
[0071] Example 2
[0072] Under the same conditions as in Example 1, the molar content of F2 in F2 / N2 mixture A was increased to 15%. Specific test results are shown in Table 1.
[0073] Example 3
[0074] Under the same conditions as in Example 1, the molar content of F2 in F2 / N2 mixture A was increased to 20%. Specific test results are shown in Table 1.
[0075] Example 4
[0076] Under the same conditions as in Example 1, the molar content of F2 in F2 / N2 mixture A was reduced to 8%. Specific test results are shown in Table 1.
[0077] Example 5
[0078] Under the same conditions as in Example 1, the molar content of F2 in F2 / N2 mixture A was reduced to 5%. Specific test results are shown in Table 1.
[0079] Example 6
[0080] Under the same conditions as in Example 1, the settling time in step one was extended to 12 hours. Specific test results are shown in Table 1.
[0081] Example 7
[0082] Under the same conditions as in Example 1, the settling time in step one was shortened to 4 hours. Specific test results are shown in Table 1.
[0083] Example 8
[0084] Under the same conditions as in Example 1, the reaction time in step two was extended to 36 hours. Specific test results are shown in Table 1.
[0085] Example 9
[0086] Under the same conditions as in Example 1, the reaction time in step two was shortened to 12 hours. Specific test results are shown in Table 1.
[0087] Example 10
[0088] Under the same conditions as in Example 1, the reaction time in step two was shortened to 6 hours. Specific test results are shown in Table 1.
[0089] Example 11
[0090] Under the same conditions as in Example 1, oxygen was introduced until the absolute pressure inside the reactor was 0.12 kPa, and in step two, an F2 / N2 mixture A was introduced until the absolute pressure inside the reactor was 300.12 kPa. Specific test results are shown in Table 1.
[0091] Example 12
[0092] Under the same conditions as in Example 1, oxygen was introduced until the absolute pressure inside the reactor was 0.02 kPa, and in step two, an F2 / N2 mixture A was introduced until the absolute pressure inside the reactor was 300.02 kPa. Specific test results are shown in Table 1.
[0093] Example 13
[0094] Under the same conditions as in Example 1, the temperature of the reactor in step one was increased to 80°C. Specific test results are shown in Table 1.
[0095] Example 14
[0096] Under the same conditions as in Example 1, the temperature of the reactor in step one was increased to 120°C. Specific test results are shown in Table 1.
[0097] Example 15
[0098] Under the same conditions as in Example 1, the temperature of the reactor in step one was increased to 150°C. Specific test results are shown in Table 1.
[0099] Example 16
[0100] Under the same conditions as in Example 1, the temperature of the reactor in step two was increased to 200°C. Specific test results are shown in Table 1.
[0101] Example 17
[0102] Under the same conditions as in Example 1, the temperature of the reactor in step two was reduced to 150°C. Specific test results are shown in Table 1.
[0103] Example 18
[0104] Under the same conditions as in Example 1, the temperature of the reactor in step three was increased to 200°C. Specific test results are shown in Table 1.
[0105] Example 19
[0106] Under the same conditions as in Example 1, the molar content of F2 in F2 / N2 mixture B was reduced to 15%. Specific test results are shown in Table 1.
[0107] Example 20
[0108] Under the same conditions as in Example 1, the oxygen introduced in step one was replaced with sulfur dioxide. Specific test results are shown in Table 1.
[0109] Example 21
[0110] In a 10L reactor, add 2kg of tetrafluoroethylene-perfluoroalkyl vinyl ether copolymer granules, evacuate the reactor, replace with high-purity nitrogen to control the oxygen content inside the reactor to less than 10ppm, and continue evacuating the reactor until the absolute pressure inside the reactor is less than 5Pa.
[0111] Step 1: Raise the temperature of the reactor to 100℃, introduce oxygen until the absolute pressure inside the reactor is 0.36kPa, and the molar content of F2 in the F2 / N2 mixed gas A is 12%, and let it stand for 8 hours.
[0112] Step 2: Introduce F2 / N2 mixed gas A until the absolute pressure inside the reactor is 300.36 kPa, raise the reactor temperature to 200℃, and react for 24 hours.
[0113] Step 3: Exhaust the gas inside the reactor, evacuate and replace the evacuation, and introduce F2 / N2 mixed gas B until the absolute pressure inside the reactor is 300 kPa. The molar content of F2 in F2 / N2 mixed gas B is 30%. Control the reactor temperature at 150℃ and react for 10 hours.
[0114] Then, the gas is vented and the mixture is cooled by displacement to obtain treated tetrafluoroethylene-perfluoroalkyl vinyl ether copolymer granules.
[0115] The obtained tetrafluoroethylene-perfluoroalkyl vinyl ether copolymer granules were tested for yield strength, tensile breaking strength, tensile modulus and Shore hardness according to relevant test standards. The test data results are shown in Table 2.
[0116] Example 22
[0117] Under the same conditions as in Example 21, the temperature of the reactor in step one was increased to 150°C. Specific test results are shown in Table 2.
[0118] Example 23
[0119] Under the same conditions as in Example 21, the temperature of the reactor in step one was increased to 180°C. Specific test results are shown in Table 2.
[0120] Example 24
[0121] Under the same conditions as in Example 21, the temperature of the reactor in step one was reduced to 70°C. Specific test results are shown in Table 2.
[0122] Example 25
[0123] Under the same conditions as in Example 21, the temperature of the reactor in step two was increased to 220°C. Specific test results are shown in Table 2.
[0124] Example 26
[0125] Under the same conditions as in Example 21, the temperature of the reactor in step two was reduced to 160°C. Specific test results are shown in Table 2.
[0126] Example 27
[0127] Under the same conditions as in Example 21, the temperature of the reactor in step two was reduced to 140°C. Specific test results are shown in Table 2.
[0128] Example 28
[0129] A series of fluidized bed reactors were used. The feed rate of polytetrafluoroethylene suspension resin fine powder was 100 g / h. The bed temperature of reactor 1 was 140℃, the oxygen flow rate was 96 ml / min, and the residence time of the resin in reactor 1 was 1 min. The bed temperature of reactor 2 was 240℃, the flow rate of F2 / N2 mixed gas A was 80 L / min, the molar content of F2 in F2 / N2 mixed gas A was 12%, and the residence time of the resin in reactor 2 was 2 min.
[0130] Then, after cyclone separation, the resin powder enters the collection tank and continues to be fed into reactor 3. The bed temperature of reactor 3 is 150℃, the flow rate of F2 / N2 mixed gas B is 80L / min, the molar content of F2 in F2 / N2 mixed gas A is 30%, and the residence time of the resin in reactor 3 is 2min.
[0131] The product is separated by cyclone separator and enters a collection tank. After system displacement and cooling, the treated polytetrafluoroethylene suspension resin fine powder is obtained.
[0132] The obtained polytetrafluoroethylene suspension resin fine powder was tested for yield strength, tensile breaking strength, tensile modulus and Shore hardness according to relevant testing standards. The test data results are shown in Table 3.
[0133] Example 29
[0134] Under the same conditions as in Example 28, the bed temperature in reactor 1 was increased to 180°C. Specific test results are shown in Table 3.
[0135] Example 30
[0136] Under the same conditions as in Example 28, the bed temperature of reactor 1 was reduced to 100°C. Specific test results are shown in Table 3.
[0137] Example 31
[0138] Under the same conditions as in Example 28, the resin feeding rate was adjusted to 20 g / h, the oxygen injection flow rate was 19.2 ml / min, the F2 / N2 mixed gas A flow rate was adjusted to 16 L / min, the resin residence time in reactor 1 was 5 min, and the resin residence time in reactor 2 was 10 min. Specific test results are shown in Table 3.
[0139] Example 32
[0140] Under the same conditions as in Example 28, the bed temperature in reactor 2 was reduced to 200°C. Specific test results are shown in Table 3.
[0141] Example 33
[0142] Under the same conditions as in Example 28, the bed temperature in reactor 2 was reduced to 180°C. Specific test results are shown in Table 3.
[0143] Example 34
[0144] Under the same conditions as in Example 28, the oxygen injection flow rate was 4.8 ml / min. Specific test results are shown in Table 3.
[0145] Comparative Example 1
[0146] Under the same conditions as in Example 1, the molar content of F2 in F2 / N2 mixture A was reduced to 4%. Specific test results are shown in Table 1.
[0147] Comparative Example 2
[0148] Under the same conditions as in Example 1, the settling process in step one was omitted. Specific test results are shown in Table 1.
[0149] Comparative Example 3
[0150] Under the same conditions as in Example 1, the oxygen introduced in step one was omitted. Specific test results are shown in Table 1.
[0151] Comparative Example 4
[0152] Under the same conditions as in Example 1, the molar content of F2 in F2 / N2 mixture B was reduced to 12%. Specific test results are shown in Table 1.
[0153] Comparative Example 5
[0154] Under the same conditions as in Example 1, the molar content of F2 in the F2 / N2 mixture B was increased to 35%. Specific test results are shown in Table 1.
[0155] Comparative Example 6
[0156] Under the same conditions as in Example 1, the F2 / N2 mixture B introduced in step three was omitted. Specific test results are shown in Table 1.
[0157] Comparative Example 7
[0158] Poly(fluoroethylene propylene) resin was treated with carbon fiber reinforcement, with a carbon fiber addition amount of 2%. Specific test results are shown in Table 1.
[0159] Table 1. Test results of poly(fluoroethylene propylene) granules before treatment, Examples 1-20, and Comparative Examples 1-7
[0160]
[0161]
[0162] Table 2. Test results of tetrafluoroethylene-perfluoroalkyl vinyl ether copolymer granules before treatment, Examples 21-27
[0163]
[0164] Table 3. Test results of polytetrafluoroethylene suspension resin powder before treatment, Examples 28-34
[0165]
[0166] The above embodiments further illustrate the correlation between the implementation methods described in this invention and the reinforcing effect on fluoropolymers. By controlling the temperature and contact time in the first infiltration stage, sufficient contact between the reinforcing gas and the fluoropolymer is ensured. By controlling the concentration, temperature, and reaction time of the fluorine gas in the second step, the cross-linking effect of the reinforcing gas is ensured, thereby achieving the expected reinforcing effect. By controlling the concentration and temperature of the fluorine gas in the third step, the unstable end groups are controlled to ensure the material's performance without causing the cross-linked structure to break or the material to degrade.
[0167] The above description is merely a specific embodiment of the present invention, but the scope of protection of the present invention is not limited thereto. Those skilled in the art should understand that the present invention includes, but is not limited to, the content described in the above specific embodiments. Any modifications that do not depart from the functional and structural principles of the present invention will be included within the scope of the claims.
Claims
1. A method for enhancing the mechanical properties of fluoropolymers, characterized in that, Includes the following steps: Step 1: In the reactor, the fluoropolymer is brought into contact with the oxygen-containing reinforcing gas at 60-180°C for a set time t1, where t1 ≥ 1 min. The reinforcing gas is any one or any combination of oxygen and sulfur dioxide. Step 2: Add F2 / N2 mixture A to the reactor, and contact the fluoropolymer with the F2 / N2 / reinforcing gas mixture B at 150-250℃ for a set time t2, where t2 ≥ 1 min. The F2 / N2 mixture A contains the following components in molar proportions: 5-20 parts of fluorine gas; 80-95 parts of nitrogen gas. Step 3: After removing the F2 / N2 / enhancing gas mixture B from the reactor, or replacing it with a new reactor, add the F2 / N2 mixture C to the reactor. The fluoropolymer and the F2 / N2 mixture C are then contacted at 150-200℃ for a set time t3, where t3 ≥ 1 min. The F2 / N2 mixture C contains the following molar amounts of components: 15-30 parts fluorine and 70-85 parts nitrogen.
2. The method for enhancing the mechanical properties of fluoropolymers according to claim 1, characterized in that, In step one, 1h≤t1≤6h; and / or, the fluoropolymer is contacted with the reinforcing gas containing oxygen atoms at 90-150℃.
3. The method for enhancing the mechanical properties of fluoropolymers according to claim 1, characterized in that... In step two, 1h≤t2≤6h; and / or, the fluoropolymer is contacted with the mixture B of F2 / N2 / reinforcing gas at 180-220℃.
4. The method for enhancing the mechanical properties of fluoropolymers according to claim 1, characterized in that... In step three, 1h ≤ t3 ≤ 6h.
5. The method for enhancing the mechanical properties of fluoropolymers according to claim 1, characterized in that, The fluoropolymer is any one of perfluoroethylene propylene, tetrafluoroethylene-perfluoroalkyl vinyl ether copolymer, and polytetrafluoroethylene suspension resin.
6. A fluoropolymer, characterized in that, The fluoropolymer is obtained by treating it with the method described in any one of claims 1 to 5, thereby enhancing the mechanical properties of the fluoropolymer.
Citation Information
Patent Citations
Resin composition, molding produced using the same, and process for producing the same
EP0857756A1
Process for producing fluorination-treated perfluoropolymer
US20100063214A1
Polymeric materials having controlled physical properties
US4833205A