A kind of oblique groove etching method based on SiC substrate
By using spin-coated photoresist and electron beam exposure to form a metal mask plate on SiC material, multiple etchings are performed to adjust the inclination angle, and the depth and angle controllable chute etching on SiC material is achieved, solving the existing technology The problem of deep etching and angle requirements cannot be met, which improves the device's withstand voltage and conduction current and enhances the device's reliability.
Patent Information
- Application Number
- CN202311299206.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-10-08
- Publication Date
- 2024-11-26
- Estimated Expiration
- 2043-10-08
AI Technical Summary
The prior art cannot etch chutes with a depth of more than 10μm and controllable angles on SiC materials, which cannot meet the needs of terminal applications of power devices. The traditional wet corrosion process is not suitable for SiC materials.
Using the inclined trench etching method based on SiC substrate, metal mask plate is formed by spin-coating photoresist, electron beam exposure, and metal evaporation, and one-time etching and secondary etching are performed, respectively adjusting the inclination angle to form trapezoidal trench grooves. , SF6 is used as the etching gas to control the etching depth and angle.
A chute with an etching depth of more than 10μm and a controllable angle on SiC material is realized, which can adapt to the needs of different devices, improve the reverse withstand voltage and forward conduction current of the device, and reduce the possibility of breakdown of the trench gate oxygen. improves the reliability of semiconductor devices.
Smart Images

Figure CN117219505B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the field of semiconductor technology, and in particular to a skew groove etching method based on a SiC substrate. Background Art
[0002] Silicon carbide (SiC) is a wide bandgap semiconductor material that has many advantages, such as large bandgap width, high breakdown field strength, radiation resistance, and normal operation at high temperatures of several hundred degrees Celsius. In addition, the epitaxial growth technology of silicon carbide is more mature than other common wide bandgap semiconductors. These factors together determine that SiC is the preferred material for the preparation of various advanced power devices.
[0003] SiC material has high hardness and stable chemical properties, and has strong resistance to chemical corrosion. Therefore, traditional wet etching processes are difficult to apply to the etching of SiC materials. Currently, the etching of SiC materials generally adopts dry etching based on plasma technology, such as reactive ion etching, inductively coupled plasma etching and magnetic neutral loop discharge plasma etching.
[0004] Publication No. CN115527848A provides a SiC groove etching method, which prepares a patterned mask layer on the surface of a silicon carbide substrate, then optimizes the pattern of the mask layer, and finally etches the silicon carbide substrate using the mask layer after the pattern optimization. However, this method is suitable for grooves whose sidewalls are perpendicular to the surface of the SiC substrate, and cannot combine deep etching with controllable angles, and cannot process trapezoidal grooves. The grooves with vertical sidewalls processed by the existing method cannot meet the process requirements for the reverse terminal preparation of existing SiC devices. Therefore, it is necessary to develop a SiC deep etching process technology with an etching depth of more than 10μm and controllable angle to meet the actual needs of power device terminal application scenarios. Summary of the invention
[0005] The object of the present invention is to provide a skew groove etching method based on a SiC substrate to solve the problems raised in the above background technology.
[0006] To achieve the above object, the present invention provides the following technical solutions:
[0007] A method for etching an oblique groove based on a SiC substrate, the specific steps comprising:
[0008] S1: Spin-coating photoresist on the processed end surface of the SiC substrate, exposing the processed end surface with an electron beam to obtain a first required pattern, and evaporating metal onto the processed end surface of the SiC substrate to form a metal mask to obtain a first SiC substrate;
[0009] S2: etching the first required pattern once on the first SiC substrate processing end surface, wherein the etching direction and the second SiC substrate end surface have a first inclination angle, and a first inclined groove in the shape of a parallelogram is obtained;
[0010] S3: washing away the residual metal on the surface of the first SiC substrate with a gold washing solution, re-spinning the photoresist, and then performing secondary exposure on the processed end surface with an electron beam to obtain a second required pattern, and again evaporating the metal onto the processed end surface of the first SiC substrate to form a secondary metal mask to obtain a second SiC substrate;
[0011] S4: A second etching is performed on the second SiC substrate processing end surface according to a second required pattern, and the etching direction and the second SiC substrate end surface have a second inclination angle, which together with the first oblique groove constitute a trapezoidal groove.
[0012] Furthermore, the thickness of the photoresist ranges from 100 μm to 200 μm, the adopted photoresist is polymethyl methacrylate, and the parameters for spin coating the photoresist are 500 revolutions for 6 seconds and then 4000 revolutions for 60 seconds.
[0013] Furthermore, the thickness of the metal mask is 50 nm, and the mask metal is one of nickel, chromium and molybdenum.
[0014] Furthermore, the depth of the inclined grooves formed by the first etching and the second etching is the same, and the first inclination angle and the second inclination angle are the same.
[0015] Furthermore, the first demand pattern and the second demand pattern are symmetrically arranged along a center line of the formed trapezoidal groove.
[0016] Furthermore, when the electron beam is exposed to the processed end face, the electron beam exposure system of the micro-nano processing system is used for electron beam exposure, and the electron beam evaporation coating machine is used for metal vapor deposition. When performing the first and second etchings, SF6 is used as the etching gas, the etching power is 90W, and the etching time is 2700s.
[0017] Compared with the prior art, the present invention has the following beneficial effects:
[0018] The present invention adopts a double-side etching method, and the angle of each side can be adjusted according to demand, so as to etch a trapezoidal groove. The inclined grooves with different angles are obtained by etching with controllable angles to meet the actual needs of different devices for the deep groove edge. The inclined grooves with different angles can be helpful for the development and preparation of various SiC devices. At the same time, the inclined grooves with a certain angle can increase the reverse withstand voltage and forward conduction current of the device, reduce the possibility of breakdown of the trench gate oxide, and thus improve the reliability of the semiconductor device. BRIEF DESCRIPTION OF THE DRAWINGS
[0019] Figure 1 It is a schematic diagram of the overall method flow of the present invention;
[0020] Figure 2 Schematic diagram of the processing flow of the SiC substrate in the present invention;
[0021] Figure 3 Characteristic curves of forward voltage applied to the trench processed by the present invention and the semiconductor in the prior art;
[0022] Figure 4 The characteristic curves of the forward voltage applied to the trench processed by the present invention and the semiconductor in the prior art are shown. DETAILED DESCRIPTION
[0023] In order to make the objectives, technical solutions and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with specific embodiments.
[0024] It should be noted that, unless otherwise defined, the technical terms or scientific terms used in the present invention should be understood by people with ordinary skills in the field to which the present invention belongs. The words "first", "second" and similar words used in the present invention do not indicate any order, quantity or importance, but are only used to distinguish different components. "Include" or "comprise" and similar words mean that the elements or objects appearing before the word include the elements or objects listed after the word and their equivalents, without excluding other elements or objects. "Connect" or "connected" and similar words are not limited to physical or mechanical connections, but may include electrical connections, whether direct or indirect. "Up", "down", "left", "right" and the like are only used to indicate relative positional relationships. When the absolute position of the described object changes, the relative positional relationship may also change accordingly.
[0025] Example:
[0026] See also Figure 1 to Figure 2 , the present invention provides a technical solution:
[0027] A method for etching an oblique groove based on a SiC substrate, the specific steps comprising:
[0028] S1: Spin-coat photoresist on the processed end surface of the SiC substrate, use an electron beam to expose the processed end surface to obtain a first required pattern, evaporate metal onto the processed end surface of the SiC substrate to form a metal mask, and obtain a first SiC substrate.
[0029] like Figure 2As shown in steps A to C in the figure, the SiC substrate in this embodiment needs to ensure that its surface is clean. Before processing, it is cleaned and polished to ensure good surface quality. When spin-coating the photoresist, the photoresist is applied to the processed end face of the SiC substrate. During the spin-coating process, the substrate is placed on a rotating table to evenly coat the photoresist on the end face of the substrate. In this embodiment, the thickness of the photoresist ranges from 100μm to 200μm. When the electron beam is exposed to the processed end face, the electron beam exposure system of the micro-nano processing system is used for electron beam exposure.
[0030] During electron beam exposure, an electron beam is used to expose a target area on the photoresist. The control and positioning of the electron beam enables the desired pattern to be formed on the photoresist. The irradiation of the electron beam causes the photoresist to undergo chemical or physical changes in the target area. After electron beam exposure, the photoresist needs to be developed to remove the photoresist in the unexposed area or the exposed area. A developer is used for this purpose. During the development process, only the photoresist structure of the desired pattern is retained.
[0031] During metal evaporation, the required metal source material is heated to the evaporation point of the metal to evaporate into metal vapor, which is deposited on the area exposed by the photoresist and the substrate to form a metal film. The metal mask constructed in this embodiment is used as an etching mask.
[0032] Furthermore, the metal evaporation is continued for a certain time to ensure that the required film thickness is obtained. The photoresist used is polymethyl methacrylate. The parameters for spin coating the photoresist are 500 rpm for 6 seconds and then 4000 rpm for 60 seconds. In this embodiment, an electron beam evaporation coating machine is used for metal evaporation.
[0033] S2: etching the first required pattern once on the first SiC substrate processing end surface, wherein the etching direction and the second SiC substrate end surface have a first inclination angle, and a first inclined groove in the shape of a parallelogram is obtained.
[0034] like Figure 2 As shown in step D in the figure, the first required pattern designed in this embodiment is a rectangular area, and the inclination angle during etching is θ1. This embodiment adopts an ion etching method, uses SF6 as an etching gas, has an etching power of 90W, and an etching time of 2700s. The etching power and etching time determine the etching depth.
[0035] S3: The residual metal on the surface of the first SiC substrate is washed away by a gold washing solution, photoresist is re-spin-coated, and the processed end surface is exposed for a second time by an electron beam to obtain a second required pattern, and metal is evaporated again onto the processed end surface of the first SiC substrate to form a secondary metal mask to obtain a second SiC substrate.
[0036] like Figure 2As shown in steps E to G in the embodiment, the gold washing solution in this embodiment is a mixed solution of hydrofluoric acid and nitric acid to remove the oxide, metal layer and organic pollutants on the surface of the first SiC substrate, and the secondary metal mask is hollowed out at the first inclined groove.
[0037] Furthermore, the first requirement pattern and the second requirement pattern are symmetrically arranged along the center line of the formed trapezoidal groove, that is, in this embodiment, the second requirement pattern and the first requirement pattern have the same shape.
[0038] S4: A second etching is performed on the second SiC substrate processing end surface according to a second required pattern, and the etching direction and the second SiC substrate end surface have a second inclination angle, which together with the first oblique groove constitute a trapezoidal groove.
[0039] In this embodiment, the depth of the inclined groove formed by the first etching and the second etching is the same, so the etching parameters such as the etching power and etching time of the first etching and the second etching are also the same. Figure 2 As shown in H in FIG. 1 , the tilt angle during the secondary etching is θ2, and the first tilt angle and the second tilt angle are the same, that is, θ1=θ2.
[0040] Through the double-sided etching method, the angle of each side can be adjusted according to the needs, so as to etch a trapezoidal groove. Through the controllable angle etching, oblique grooves of different angles can be obtained to meet the actual needs of different devices for the deep groove edge. These oblique grooves of different angles can help the development and preparation of various SiC devices.
[0041] In this embodiment, after the processing is completed according to the above method, it is necessary to wash away the remaining metal on the surface with a chemical reagent to obtain a chute structure.
[0042] like Figure 3-4 As shown, it can be seen that the inclined grooves at a certain angle can increase the reverse withstand voltage and forward conduction current of the device, reduce the possibility of trench gate oxide breakdown, and thus improve the reliability of the semiconductor device.
[0043] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.
Claims
1. A method for etching an oblique groove based on a SiC substrate, characterized in that: The specific steps include: S1: Spin-coating photoresist on the processed end surface of the SiC substrate, exposing the processed end surface with an electron beam to obtain a first required pattern, and evaporating metal onto the processed end surface of the SiC substrate to form a metal mask to obtain a first SiC substrate; S2: etching the first required pattern once on the first SiC substrate processing end surface, wherein the etching direction and the first SiC substrate end surface have a first inclination angle, and obtaining a first inclined groove in the shape of a parallelogram; S3: washing away the residual metal on the surface of the first SiC substrate with a gold washing solution, re-spinning the photoresist, and then performing secondary exposure on the processed end surface with an electron beam to obtain a second required pattern, and again evaporating the metal onto the processed end surface of the first SiC substrate to form a secondary metal mask to obtain a second SiC substrate; S4: performing secondary etching on the second SiC substrate processing end surface according to the second required pattern, wherein the etching direction and the second SiC substrate end surface have a second inclination angle, and together with the first oblique groove form a trapezoidal groove; The depth of the inclined groove formed by the first etching and the second etching is the same, the first inclination angle and the second inclination angle are the same, and the first required pattern and the second required pattern are symmetrically arranged along the center line of the formed trapezoidal groove.
2. The method for etching an oblique groove based on a SiC substrate according to claim 1, characterized in that: The thickness of the metal mask is 50nm, and the mask metal is one of nickel, chromium and molybdenum.
3. The method for etching an oblique groove based on a SiC substrate according to claim 1, characterized in that: When the electron beam is exposed to the processed end face, the electron beam exposure system of the micro-nano processing system is used for electron beam exposure, and the electron beam evaporation coating machine is used for metal evaporation. When performing the first etching and the second etching, SF6 is used as the etching gas, the etching power is 90W, and the etching time is 2700s.