Methods for removing overflow
By employing multiple pretreatment steps involving intermittent electrolysis and parameter adjustment, combined with high-pressure water rinsing, the delamination problem in semiconductor packaging material removal was solved, improving product reliability and reducing costs.
Patent Information
- Application Number
- CN202311129834.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-09-01
- Publication Date
- 2026-11-17
- Estimated Expiration
- 2043-09-01
AI Technical Summary
Existing methods for removing overflow from semiconductor packaging structures can easily lead to delamination of the packaging structure, affecting product reliability, and are also costly.
Intermittent electrolysis and parameter adjustment are used to control the amount of gas generation and escape through multiple pretreatment steps, avoiding delamination of the packaging structure, and high-pressure water flushing is used to remove overflow.
It reduces the likelihood of packaging structure delamination, improves product reliability, reduces costs, and enables controllable expansion of the slit, avoiding additional processing steps.
Smart Images

Figure CN117238750B_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of semiconductor packaging, and more particularly to a method for removing overflow. Background Technology
[0002] During the semiconductor packaging process, various adhesive substances, such as flash (also known as burrs or flaking, typically composed of epoxy molding compound), remain on the molded body and leads. These must be removed; otherwise, they can lead to frame deformation, plating defects, and other plating flaws, affecting product reliability, causing open circuits, cold solder joints, and other problems. This can also impact the electrical conductivity of the pins, and in severe cases, result in rework, chip malfunction, or even complete failure. This increases the complexity and cost of the packaging process. Therefore, removing flash is a crucial post-packaging process for semiconductor integrated circuits.
[0003] One process for removing excess material is softening (chemical immersion) followed by high-pressure water jetting. This method has low production efficiency (requiring an additional softening step, taking 2 hours) and relatively high cost (softening equipment, softening chemicals, and waste treatment all incur costs). Furthermore, when multiple iron-nickel substrate products are immersed in a single layer, the product surface is difficult to dry. If the excess material removal process is not completed in time, rust will form on the frame surface, affecting the quality of subsequent electroplating processes.
[0004] Another process for removing overflow is electrolysis, followed by high-pressure water removal. For example, the package structure to be overflowed is used as the cathode, the overflow removal solution as the electrolyte, and stainless steel or titanium alloy as the anode to perform the electrolysis process. This method of overflow removal may cause delamination in the semiconductor package structure. As the application conditions for semiconductor packages become increasingly stringent, many semiconductor package structures require zero delamination (delamination refers to the separation and gaps between different materials at the contact surface) to prevent air, water, or acids / alkalis from entering the semiconductor package structure during use, thereby causing electrical performance failure.
[0005] Therefore, methods for removing overflow that can reduce the probability of semiconductor packaging structure delamination have become the focus of current research. Summary of the Invention
[0006] The technical problem to be solved by the present invention is to provide a method for removing overflow, which can reduce the probability of delamination of the packaging structure and improve the reliability of the packaging structure.
[0007] To address the above problems, the present invention provides a method for removing overflow, comprising:
[0008] Provides a packaging structure for removing overflow;
[0009] Multiple pretreatment steps are performed on the areas of the packaging structure where overflow needs to be removed to loosen the overflow on the packaging structure. Each pretreatment step includes: performing an electrolysis process and continuing for a first time, wherein the parameters of the electrolysis process are adjusted so that the difference between the amount of gas generated and the amount of gas escaped in the first time is less than or equal to a preset value, the preset value being a critical value for the amount of gas that causes the packaging structure to delaminate; stopping the electrolysis process and waiting for a second time to allow residual gas to escape.
[0010] The pre-treated packaging structure is rinsed to remove the overflow.
[0011] In one embodiment, during the pretreatment step, the gas generation rate is greater than the gas escape rate.
[0012] In one embodiment, during the electrolysis process, the amount of gas generated in the first time period is controlled by adjusting the current of the electrolysis process.
[0013] In one embodiment, in the pretreatment step, the parameters of the electrolysis process are adjusted so that the difference between the calculated value of the amount of gas generated in the first time period and the calculated value of the amount of gas emitted in the first time period is less than or equal to the preset value.
[0014] In one embodiment, in the pretreatment step, the parameters of the electrolysis process are adjusted so that the calculated sum of the gas escape amounts in the first time and the second time is greater than or equal to the calculated gas generation amount in the first time.
[0015] In one embodiment, during the electrolysis process, the amount of gas generated within the first time period is controlled by increasing or decreasing the first time period.
[0016] In one embodiment, during the step of stopping the electrolysis process, the amount of residual gas escaping is controlled by increasing or decreasing the second time.
[0017] In one embodiment, the current used in the electrolysis process is 100–400 A.
[0018] In one embodiment, the method for obtaining the critical value of the amount of gas that causes the encapsulation structure to delaminate includes:
[0019] Multiple encapsulation structure samples are provided, and different encapsulation structure samples have different combinations of parameters;
[0020] An electrolytic process is performed on the packaged structure sample. The amount of gas causing delamination of the packaged structure sample is obtained, and the parameter combinations are correlated with the numerical values to form a database.
[0021] Using the parameter combination of the packaging structure to be removed as an index, the numerical value of the amount of gas corresponding to the parameter combination of the packaging structure to be removed is obtained from the database, and this value is used as the critical value.
[0022] In one embodiment, the parameter combination includes at least one of the following parameters: packaging form of the packaging structure, frame structure, chip size, and molding compound.
[0023] In the method for removing overflow according to the present invention, a pretreatment step is performed on the area of the packaging structure where overflow needs to be removed. Each pretreatment step includes performing an electrolysis process and stopping the electrolysis process. Gas is generated during the electrolysis process, but not during the stopping process. Gas escapes during both the electrolysis and stopping processes. This means the pretreatment step employs an intermittent electrolysis method, allowing the gas generated during the pretreatment step to accumulate to a certain amount and then escape promptly and sufficiently, thus reducing the probability of packaging structure delamination. Furthermore, the method for removing overflow also controls the amount of gas generated during the electrolysis process by adjusting the parameters, ensuring that the total amount of gas near the packaging structure during the electrolysis process (the difference between the amount of gas generated and the amount of gas escaped) does not exceed a critical value that would cause delamination of the packaging structure. This further avoids excessive gas near the packaging structure, thereby further reducing the probability of packaging structure delamination. Meanwhile, the method for removing overflow in this invention requires multiple pre-processing steps, rather than just one, to widen the gap between the overflow and the frame to the required size, thereby achieving controllability of the gap and reducing the probability of delamination of the packaging structure.
[0024] The method for removing overflow in this invention, through intermittent electrolysis and control of electrolysis parameters, can expand the gap between the overflow and the frame to the required size, achieve gap controllability, reduce the probability of delamination of the packaging structure, and reduce costs without adding new processing technology, thus having high applicability. Attached Figure Description
[0025] To more clearly illustrate the technical solutions in the embodiments of the present invention, the accompanying drawings used in the description of the embodiments will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For those skilled in the art, other drawings can be obtained based on these drawings without creative effort.
[0026] Figure 1 This is a schematic diagram of the steps of a method for removing overflow provided in an embodiment of the present invention;
[0027] Figures 2A to 2D This is a schematic flowchart of a method for removing overflow provided in an embodiment of the present invention;
[0028] Figures 3A-3B This is a process flow diagram of an existing method for removing overflow. Detailed Implementation
[0029] The specific embodiments of the method for removing overflow provided by the present invention will be described in detail below with reference to the accompanying drawings.
[0030] Figure 1 This is a schematic diagram illustrating the steps of a method for removing overflow provided in an embodiment of the present invention. Figures 2A to 2D This is a schematic flowchart of a method for removing overflow provided in an embodiment of the present invention. The method for removing overflow provided in an embodiment of the present invention includes:
[0031] Please see Figure 1 and Figure 2A Step S10, providing a packaging structure 200 for removing overflow 230.
[0032] There is overflow 230 at the junction of the edge of the plastic encapsulator 210 and the frame 220 of the encapsulation structure 200. This overflow 230 can cause deformation of the frame 220, plating failure, plating defects, etc. Therefore, it is necessary to remove the overflow 230 from the encapsulation structure 200.
[0033] In existing technologies, electrolysis is typically used to remove the overflow. Specifically, Figures 3A-3B This is a process flow diagram of an existing method for removing overflow. Please refer to [link / reference]. Figure 3A An electrolytic process is performed on the areas of the package structure 300 where overflow 330 needs to be removed. This electrolytic process generates gas 350, which comes into contact with the molding compound 310, the frame 320, and the overflow 330. Please refer to... Figure 3B The generated gas 350, upon contact with the encapsulation body 310, frame 320, and overflow 330, produces a "bursting" effect (the continuous bursting of bubbles generates mechanical force), causing the overflow 330 to loosen from the frame 320, forming a slit 340. This reduces the bonding force between the overflow 330 and the surface of the frame 320. As the amount of gas 350 increases, the slit 340 widens, further loosening the overflow 330 (i.e., achieving a softening effect). After the overflow 330 is loosened, high-pressure water is used to impact the encapsulation structure, thereby removing the loosened overflow 330. Please refer to [link to relevant documentation]. Figure 2D .
[0034] The encapsulation structure 300 formed by removing the overflow 330 using this electrolysis process exhibits delamination. Further research by the inventors revealed that although the effect of removing the overflow 330 improves with increasing electrolysis time, more gas accumulates near the encapsulation structure 300 with increasing electrolysis time. The gas 350 (e.g., hydrogen) generated by electrolysis is a small molecule gas that can continuously collide without direction in the slit 340. The diffusion of a large amount of gas 350 generated in a short time will cause the slit 340 to expand uncontrollably, thus leading to delamination of the encapsulation structure 300.
[0035] In view of this, the present invention provides a pretreatment step for removing overflow, which enables the gas generated in the pretreatment step to accumulate to a certain amount and then escape in a timely and sufficient manner, thereby avoiding excessive gas accumulation that could lead to delamination of the packaging structure and reducing the probability of delamination of the packaging structure.
[0036] Specifically, please refer to Figure 1 , Figure 2B and Figure 2C Step S11 involves performing multiple pretreatment steps on the area of the encapsulation structure 200 where the overflow 230 needs to be removed, to loosen the overflow 230 on the encapsulation structure 200. The pretreatment steps include: performing an electrolysis process and continuing for a first time, wherein the parameters of the electrolysis process are adjusted so that the difference between the amount of gas 250 generated and the amount of gas 250 emitted during the first time is less than or equal to a preset value, the preset value being a critical value for the amount of gas 250 that causes the encapsulation structure 200 to delaminate; stopping the electrolysis process and waiting for a second time to allow the residual gas 250 to escape.
[0037] The amount of gas 250 includes, but is not limited to, the mass or volume of gas 250; the amount of gas 250 generated includes, but is not limited to, the mass or volume of generated gas 250; and the amount of gas 250 emitted includes, but is not limited to, the mass or volume of emitted gas 250.
[0038] In the method for removing overflow 230 of the present invention, a pretreatment step is performed on the area of the packaging structure 200 where overflow 230 needs to be removed. Each pretreatment step includes performing an electrolysis process and stopping the electrolysis process. Gas 250 is generated in the electrolysis process step, but no gas 250 is generated in the stopping electrolysis process step. Gas 250 escapes in both the electrolysis process step and the stopping electrolysis process step. That is, the pretreatment step of the present invention performs an intermittent electrolysis method, so that the gas 250 generated in the pretreatment step (i.e. the gas generated in the electrolysis process) can accumulate to a certain amount and escape in a timely and sufficient manner, thereby reducing the probability of delamination of the packaging structure 200.
[0039] Furthermore, the method for removing overflow 230 of the present invention also controls the amount of gas 250 generated in the electrolysis process by adjusting the parameters of the electrolysis process, so that the total amount of gas 250 near the encapsulation structure 200 during the execution of the electrolysis process (the difference between the amount of gas 250 generated and the amount of gas 250 escaped) does not exceed the critical value of the amount of gas 250 that causes the encapsulation structure 200 to delaminate, thereby further avoiding excessive gas 250 near the encapsulation structure 200, and thus further reducing the probability of delamination of the encapsulation structure 200.
[0040] Meanwhile, since the amount of gas 250 generated is controlled, the slit 240 cannot be enlarged to the required size through a single electrolysis process. Therefore, the method for removing the overflow 230 of this invention requires multiple pretreatment steps, rather than just one, to enlarge the slit 240 between the overflow 230 and the frame 220 to the required size, thereby achieving controllability of the slit 240 and reducing the probability of delamination of the packaging structure 200. Figure 2B As shown, this is a schematic diagram after one or more pre-processing steps, where the gap 240 between the overflow 230 and the frame 220 is relatively small; as Figure 2C As shown, it is in Figure 2B The diagram shows the result after performing one or more preprocessing steps on the structure shown, in which the slit 240 between the overflow 230 and the frame 220 becomes larger.
[0041] The method for removing overflow 230 of the present invention can expand the slit 240 between overflow 230 and frame 220 to the required size through intermittent electrolysis and control of electrolysis parameters, thereby achieving controllability of slit 240, reducing the probability of delamination of packaging structure 200, without adding new processing technology, reducing costs, and having high applicability.
[0042] In some embodiments, the step of performing the electrolysis process includes: placing the area of the encapsulation structure 200 from which the overflow 230 needs to be removed in an electrolyte bath, using the area of the encapsulation structure 200 from which the overflow 230 needs to be removed as the cathode, using stainless steel or titanium alloy as the anode, and passing an electric current to perform the electrolysis process. During the electrolysis process, gas 250 is generated in the area of the encapsulation structure 200 from which the overflow 230 needs to be removed. This gas 250, upon contact with the encapsulation body 210, the frame 220, and the overflow 230 of the encapsulation structure 200, can produce a "bursting" effect, causing a slit 240 to form between the overflow 230 and the frame 220. In this embodiment, the electrolyte is an alkaline electrolyte. During the electrolysis process, hydrogen gas is generated in the area of the encapsulation structure 200 where the overflow 230 needs to be removed. When the hydrogen gas comes into contact with the encapsulation body of the encapsulation structure 200 and the overflow 230, it can produce a "bursting" effect, causing a slit 240 to form between the overflow 230 and the frame 220. Furthermore, hydrogen gas is a small molecule gas 250, which can collide in the slit 240 between the overflow 230 and the frame 220, thereby expanding the slit 240.
[0043] During the electrolysis process, the gas 250 generated by the electrolysis process also escapes outward. In some embodiments, during the pretreatment step, the generation rate of gas 250 is greater than the escape rate of gas 250, which can avoid the situation where the amount of gas 250 near the package is too small to form the slit 240 or to enlarge the slit 240 during the electrolysis process.
[0044] In the same electrolyte, the escape rate of gas 250 depends on the properties of the packaging structure 200 itself, such as the bonding force between the encapsulator 210 and the frame 220, and the shape of the packaging structure. Therefore, when the electrolyte and packaging structure 200 are determined, the escape rate of gas 250 is constant. The generation rate of gas 250 depends on the conductivity of the electrolyte, the current density of the electrolysis process, and the amount of charge generated by the electrolysis process. When the electrolyte is determined, the conductivity of the electrolyte is also determined. The current density of the electrolysis process is the ratio of the current to the energized area of the packaging structure 200. When the packaging structure 200 is determined, the energized area of the packaging structure 200 is also determined, and the current density of the electrolysis process depends on the current. The amount of charge generated by the electrolysis process is the product of the current and the energizing time (i.e., the first time). When the energizing time is determined, the amount of charge generated by the electrolysis process depends on the current. For the same packaging structure 200, the generation rate of gas 250 during the electrolysis process in the same time (i.e., the first time) depends on the current of the electrolysis process. Therefore, the generation rate of gas 250 can be controlled by controlling the current of the electrolysis process, thereby making the generation rate of gas 250 greater than the escape rate of gas 250. In some embodiments, when the current of the electrolysis process is determined, the generation rate of gas 250 is a constant value.
[0045] For the same packaging structure 200, the escape rate of gas 250 is constant, and the escape amount of gas 250 is the product of the escape rate and time. Therefore, the escape amount of gas 250 in the first time interval is only related to time, and when the first time interval is constant, the escape amount of gas 250 is also constant. For the same packaging structure 200, the generation rate of gas 250 is related to the current of the electrolysis process. Therefore, in some embodiments, the generation amount of gas 250 in the first time interval can be adjusted by adjusting the current of the electrolysis process, that is, by adjusting the current of the electrolysis process so that the difference between the generation amount of gas 250 and the escape amount of gas 250 in the first time interval is less than or equal to the preset value. In some embodiments, the current of the electrolysis process is 100-400A, thereby controlling the difference between the generation amount of gas 250 and the escape amount of gas 250 in the first time interval to be as close as possible to the preset value, so as to reduce the risk of delamination of the packaging structure 200 while improving the efficiency of the electrolysis process in removing overflow 230.
[0046] In some embodiments, the value of the amount of gas 250 generated in the first time period is a calculated value determined based on the current of the electrolysis process and the first time period, and the value of the amount of gas 250 emitted in the first time period is a calculated value determined based on the emission rate of gas 250 and the first time period. Therefore, in the pretreatment step, the difference between the calculated value of the amount of gas 250 generated in the first time period and the calculated value of the amount of gas 250 emitted in the first time period is less than or equal to the preset value by adjusting the parameters of the electrolysis process. Specifically, the difference between the calculated value of the amount of gas 250 generated in the first time period and the calculated value of the amount of gas 250 emitted in the first time period is less than or equal to the preset value by adjusting the current of the electrolysis process.
[0047] The method for removing overflow 230 of the present invention adjusts the parameters of the electrolysis process so that the difference between the amount of gas 250 generated and the amount of gas 250 emitted in the first time period is less than or equal to a preset value. The preset value is a critical value of the amount of gas 250 that causes the encapsulation structure 200 to delaminate, thereby avoiding delamination of the encapsulation structure 200 due to excessive gas 250 during the electrolysis process.
[0048] In the above embodiments, the difference between the amount of gas 250 generated and the amount of gas 250 emitted during the first time period is less than or equal to the preset value by adjusting the current of the electrolysis process. In other embodiments, the amount of gas 250 generated during the first time period is controlled by increasing or decreasing the first time period during the electrolysis process. That is, when the current of the electrolysis process is constant, the amount of gas 250 generated during the first time period can be adjusted by increasing or decreasing the first time period, thereby controlling the difference between the amount of gas 250 generated and the amount of gas 250 emitted during the first time period to be less than or equal to the preset value, for example, to make it as close as possible to the preset value, so as to improve the efficiency of the electrolysis process in removing overflow 230 while reducing the risk of delamination of the packaging structure 200.
[0049] In some embodiments, the step of stopping the electrolysis process includes: stopping the current flow and waiting for a second period of time. During the waiting period of the package structure 200, no gas 250 is generated; only gas 250 escapes. Therefore, by waiting for the package structure 200, residual gas 250 near the package structure 200 can escape, thereby preventing the accumulation of gas 250 generated during multiple electrolysis process steps and further reducing the risk of delamination of the package structure 200.
[0050] In some embodiments, the gas 250 generated in the electrolysis process escapes during both the first and second time periods. Therefore, the sum of the actual amount of gas 250 escaped during the first and second time periods equals the actual amount of gas 250 generated during the first time period. In other embodiments, the sum of the amounts of gas 250 escaped during the first and second time periods is a calculated value determined based on the first time, the second time, and the escape rate of the gas 250. The amount of gas 250 generated during the first time period is a calculated value determined based on the current of the electrolysis process and the first time. Therefore, in the pretreatment step, by adjusting the parameters of the electrolysis process, the calculated value of the sum of the amounts of gas 250 escaped during the first and second time periods is greater than or equal to the calculated value of the amount of gas 250 generated during the first time period. This ensures that all the generated gas 250 escapes after the second time period, further preventing the accumulation of gas 250.
[0051] In some embodiments, the escape rate of gas 250 is a constant value. In the step of stopping the electrolysis process, the amount of residual gas 250 that escapes is controlled by increasing or decreasing the second time, thereby ensuring that all the generated gas 250 can escape after the second time, and further avoiding the accumulation of gas 250.
[0052] In some embodiments, the encapsulation structure 200 is mounted on a fixture, placed in an electrolytic cell, and moves within the electrolytic cell at a set speed, for example, 3-7 m / min. During the movement of the encapsulation structure 200, multiple pretreatment steps are performed to loosen the overflow 230 on the encapsulation structure 200. The sum of a first time and a second time is taken as the total time of one pretreatment step. The time the encapsulation structure 200 is placed in the electrolytic cell is a fixed value (depending on the moving speed of the encapsulation structure 200 and the length of the electrolytic cell). The number of pretreatment steps is the ratio of the time the encapsulation structure 200 is placed in the electrolytic cell to the total time of one pretreatment step. In some embodiments, the electrolyte may be an alkaline electrolyte, such as potassium hydroxide, with a concentration of 60-100 g / L, and the temperature of the electrolyte is 40-60°C.
[0053] In some embodiments, during the step of stopping the electrolysis process, the voltage applied to the packaging structure 200 is stopped, the redox reaction stops, and the concentration difference of the electrolyte caused by the redox reaction disappears, that is, the concentration of the electrolyte returns to the initial state. This is beneficial for the replenishment of electrolyte when the electrolysis process is performed again in a subsequent manner, and can further improve the electrolysis efficiency.
[0054] In the method for removing overflow 230 of the present invention, the preset value is a critical value of the amount of gas 250 that causes the encapsulation structure 200 to delaminate. Therefore, an embodiment of the present invention also provides a method for obtaining the critical value of the amount of gas 250 that causes the encapsulation structure 200 to delaminate. The method includes:
[0055] Multiple package structure samples are provided, with different package structure samples having different parameter combinations. The parameter combinations include at least one of the following: package type, frame structure, chip size, and molding compound. The parameters in the parameter combinations are known parameters. In this step, package structure samples with the same parameter combination may include multiple sub-samples to further improve the accuracy of the obtained critical values.
[0056] An electrolysis process is performed on the packaged structure sample to obtain the numerical value of the amount of gas that causes the packaged structure sample to delaminate, and the parameter combination is associated with the numerical value to form a database.
[0057] In this step, the encapsulated structure sample is placed in an electrolyte bath for electrolysis. In some embodiments, to make the critical value referential, the composition and concentration of the electrolyte in this step are the same as the composition and concentration of the electrolyte in the step of performing the electrolysis process in the method for removing overflow of the present invention.
[0058] In this step, multiple sub-samples of a package structure sample with the same parameter combination can be electrolyzed using different electrolysis process parameters (e.g., the current of the electrolysis process), and the electrolyzed sub-samples are measured to obtain the electrolysis process parameters corresponding to the stratified sub-samples. Then, based on these parameters, the value of the amount of gas that causes the sub-sample to stratify is obtained (i.e., the critical value of the amount of gas that causes the package structure with this parameter combination to stratify).
[0059] In this step, the parameter combination value is associated with a critical value. For example, the critical value is associated with the parameter combination in a list, with one parameter combination corresponding to one critical value.
[0060] In performing multiple preprocessing steps on the area of the encapsulation structure 200 where overflow 230 needs to be removed, the parameter combination of the encapsulation structure 200 to which overflow 230 needs to be removed is used as an index to obtain the numerical value of the gas quantity corresponding to the parameter combination of the encapsulation structure to which overflow 230 needs to be removed from the database, and this value is used as the critical value. For example, if the parameter combination of the encapsulation structure is a combination of encapsulation form and frame structure, then the encapsulation type and frame 220 structure of the encapsulation structure 200 to which overflow 230 needs to be removed are used as indexes to obtain the numerical value of the gas quantity corresponding to the parameter combination with that encapsulation type and frame structure from the database, and this value is used as the critical value.
[0061] At this point, the preprocessing step is complete, and the packaging structure 200 can be transferred to other devices for further processing.
[0062] Please continue reading. Figure 1 and Figure 2D In step S12, the pre-treated packaging structure 200 is rinsed to remove the overflow 230. In this step, the loose overflow 230 is removed by rinsing.
[0063] In some embodiments, high-pressure flushing can be used to remove the overflow 230 by utilizing the high pressure of the flushing fluid. The pressure of the flushing fluid is 100-500 kgf / cm². 2 For example, in this embodiment, high-pressure water is used to impact the loose overflow material 230 on the frame 220, with the water pressure being 100-500 kgf / cm². 2 .
[0064] In some embodiments, after rinsing the pretreated packaging structure 200, a drying step is further included to dry the water marks on the product surface and prevent oxidation.
[0065] The packaging structure obtained by the method of removing overflow 230 of the present invention can effectively reduce the delamination caused by electrolytic overflow removal. The delamination ratio of the packaging structure is greatly reduced, and some packaging structures can even achieve zero delamination. This can reduce a series of quality problems caused by the delamination between the frame and the molding compound and improve product reliability.
[0066] It should be noted that the terms "comprising" and "having," and their variations, used in this invention document are intended to cover non-exclusive inclusion. The terms "first," "second," etc., are used to distinguish similar objects and are not necessarily used to describe a specific order or sequence, unless explicitly indicated by the context; it should be understood that such use of data can be interchanged where appropriate. The term "one or more" depends at least in part on the context and can be used to describe features, structures, or characteristics in a singular sense, or in a plural sense to describe combinations of features, structures, or characteristics. The term "based on" can be understood as not necessarily intended to express an exclusive set of factors, but can instead, also at least in part on the context, allow for the presence of other factors that are not necessarily explicitly described. Furthermore, embodiments and features in embodiments of this invention can be combined with each other without conflict. In addition, descriptions of well-known components and technologies have been omitted in the above description to avoid unnecessarily obscuring the concepts of this invention. In the various embodiments described above, each embodiment focuses on its differences from other embodiments; similar / identical parts between embodiments can be referred to mutually.
[0067] The above description is only a preferred embodiment of the present invention. It should be noted that those skilled in the art can make several improvements and modifications without departing from the principle of the present invention, and these improvements and modifications should also be considered within the scope of protection of the present invention.
Claims
1. A method of removing flash, characterized by, include: Provides a packaging structure for removing overflow; Multiple pretreatment steps are performed on the areas of the packaging structure where overflow needs to be removed to loosen the overflow on the packaging structure. Each pretreatment step includes: performing an electrolysis process and continuing for a first time, wherein the parameters of the electrolysis process are adjusted so that the difference between the amount of gas generated and the amount of gas escaped in the first time is less than or equal to a preset value, the preset value being a critical value for the amount of gas that causes the packaging structure to delaminate; stopping the electrolysis process and waiting for a second time to allow residual gas to escape. The pre-treated packaging structure is rinsed to remove the overflow.
2. The method of removing flash according to claim 1, wherein, In the pretreatment step, the gas generation rate is greater than the gas escape rate.
3. The method for removing overflow according to claim 1, characterized in that, In the electrolysis process, the amount of gas generated in the first time period is controlled by adjusting the current of the electrolysis process.
4. The method for removing overflow according to claim 1, characterized in that, In the pretreatment step, the parameters of the electrolysis process are adjusted so that the difference between the calculated value of the amount of gas generated in the first time period and the calculated value of the amount of gas emitted in the first time period is less than or equal to the preset value.
5. The method for removing overflow according to claim 1, characterized in that, In the pretreatment step, the parameters of the electrolysis process are adjusted so that the calculated sum of the gas escape amounts in the first time and the second time is greater than or equal to the calculated gas generation amount in the first time.
6. The method for removing overflow according to claim 1, characterized in that, In the electrolysis process, the amount of gas generated within the first time period is controlled by increasing or decreasing the first time period.
7. The method for removing overflow according to claim 1, characterized in that, In the step of stopping the electrolysis process, the amount of residual gas escaping is controlled by increasing or decreasing the second time.
8. The method for removing overflow according to claim 1, characterized in that, In the electrolysis process, the current is 100–400 A.
9. The method for removing overflow according to claim 1, characterized in that, The method for obtaining the critical value of the amount of gas that causes the encapsulation structure to delaminate includes: Multiple encapsulation structure samples are provided, and different encapsulation structure samples have different parameter combinations; an electrolysis process is performed on the encapsulation structure samples to obtain the numerical values of the amount of gas that causes the encapsulation structure samples to delaminate, and the parameter combinations are associated with the numerical values to form a database; Using the parameter combination of the packaging structure to be removed as an index, the numerical value of the amount of gas corresponding to the parameter combination of the packaging structure to be removed is obtained from the database, and this value is used as the critical value.
10. The method for removing overflow according to claim 9, characterized in that, The parameter combination includes at least one of the following: packaging form, frame structure, chip size, and molding compound.
Citation Information
Patent Citations
Method for cleaning the surface of a silicon substrate
CN102648533A
Electrolyte composition for removing burr and method of removing burr
CN105986308A