A copper phosphide / copper phosphate / cobalt phosphide nanowire film catalyst and its application
By growing Cu nanowires in situ on the surface of copper foam and electrodepositing Co(OH)2, combined with high-temperature phosphating, a copper phosphide/copper phosphate/cobalt phosphide nanowire film catalyst was prepared, solving the activity and stability problems of powder catalysts and achieving highly efficient electrocatalytic hydrogen production performance.
Patent Information
- Application Number
- CN202311157999.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-09-08
- Publication Date
- 2026-11-17
- Estimated Expiration
- 2043-09-08
AI Technical Summary
Existing powder catalysts have poor catalytic activity, are complex to separate and recover, and are prone to agglomeration and have complicated synthesis methods, which limit the efficiency and stability of electrocatalytic hydrogen production.
By growing Cu nanowires in situ on the surface of copper foam, depositing Co(OH)2 by electrodeposition, and finally synthesizing copper phosphide/copper phosphate/cobalt phosphide nanowire film catalyst by high-temperature phosphating, the hydrogen production reaction is optimized by utilizing the nanowire structure to enhance mass transfer and heterogeneous interface interaction.
The prepared catalyst is readily available and simple, with nanoparticle immobilization, good stability, and is suitable for large-scale production. It also exhibits excellent electrocatalytic hydrogen production performance under alkaline conditions.
Smart Images

Figure CN117248238B_ABST
Abstract
Description
Technical Field
[0001] This invention relates to a copper phosphide / copper phosphate / cobalt phosphide nanowire film catalyst and its application. Background Technology
[0002] The environmental pollution caused by the large-scale use of fossil fuels such as oil and coal, and the energy crisis resulting from the depletion of traditional fossil fuels, urgently require us to seek green, sustainable, and clean energy sources. Hydrogen energy, due to its high energy density, high conversion efficiency, and clean, pollution-free operation, is considered the most promising green energy source to replace fossil fuels. Electrochemical water splitting for hydrogen production has potential applications due to its simple equipment, lack of high temperature and pressure requirements, environmental friendliness, and zero carbon emissions. However, the slow electrode reaction kinetics and high water molecule dissociation energy barrier result in high energy consumption and low efficiency in water electrolysis for hydrogen production. To reduce energy consumption and improve hydrogen production efficiency, electrocatalysts are often needed to enhance the kinetics of the cathode hydrogen production reaction, aiming to achieve the commercial application of electrochemical water splitting for hydrogen production.
[0003] Currently, noble metal-based catalysts exhibit excellent hydrogen production activity, but their high cost, low reserves, and poor stability greatly limit their widespread application. Although researchers have developed transition metal-based catalytic materials with catalytic performance comparable to noble metals, these materials are mostly powders, and the separation and recovery processes are complex and time-consuming. Furthermore, the preparation of composite materials of copper phosphide, copper phosphate, and transition metal phosphides has not been reported. Based on this, this invention synthesizes a copper phosphide / copper phosphate / cobalt phosphide nanowire film catalyst and applies it to electrocatalytic hydrogen production. Summary of the Invention
[0004] The purpose of this invention is to solve the problems of poor catalytic activity, complex separation and recovery, easy agglomeration of nanoparticles, and complicated synthesis methods of existing powder catalysts, and to provide a copper phosphide / copper phosphate / cobalt phosphide nanowire film catalyst and its application.
[0005] The preparation method of the copper phosphide / copper phosphate / cobalt phosphide nanowire film catalyst of the present invention is carried out according to the following steps:
[0006] Immerse the copper foam in a 1-10% (w / w) HCl solution, sonicate for 5-30 minutes, clean and dry to obtain the treated copper foam.
[0007] 2. The cleaned copper foam was immersed in a mixture of 0.1–2 mol / L alkaline solution and 0.001–0.05 mol / L (NH)4S2O8 and reacted at room temperature for 5–60 min. The resulting blue film was washed and dried in a forced-air drying oven at 150–250 °C to obtain sample A. Then, a three-electrode system was used, with sample A as the working electrode and Ag / AgCl and Pt sheets as the reference and counter electrodes, respectively. Electroreduction was performed in 0.1–2 mol / L alkaline solution at a potential of -1.0–-3.0 V for 0.5–2 h. After the reaction was completed, the sample was washed to obtain Cu nanowires grown on the copper foam. After drying, sample B was obtained.
[0008] 3. Using a three-electrode system, sample B was used as the working electrode, and Ag / AgCl and Pt sheets were used as the reference electrode and counter electrode, respectively. Electrodeposition was carried out in 0.01-1 mol / L Co(NO3)2 solution at a potential of -0.5 to -2.0 V for 30 s to 3600 s. After the reaction was completed, the sample was washed and Co(OH)2 was deposited on Cu nanowires to obtain sample C.
[0009] IV. Place 0.1–2 g of sodium hypophosphite and sample C respectively upstream and downstream of a tube furnace, maintaining a distance of 1–5 cm between them. Raise the temperature to 250–450 °C and hold under a protective atmosphere for 1–5 h. After the reaction is complete, remove the sample, wash it, and dry it to obtain Cu3P / Cu2P4O. 12 / CoP nanowire film catalyst.
[0010] This invention relates to the application of a copper phosphide / copper phosphate / cobalt phosphide nanowire film catalyst as an electrocatalyst for catalytic electrochemical water splitting to produce hydrogen.
[0011] This invention proposes a method for preparing a three-component phosphide heterostructure electrocatalyst for hydrogen production. Specifically, Cu nanowires are grown in situ on a copper foam surface, and Co(OH)₂ is further deposited on the Cu nanowire surface via electrodeposition. Finally, copper phosphide / copper phosphate / cobalt phosphide (Cu₃P / Cu₂P₄O₃) is successfully synthesized via a high-temperature phosphating method. 12 / CoP) nanowires. On the one hand, the unique nanowire structure is used to enhance mass transfer and increase the number of active sites; on the other hand, the strong interactions between heterogeneous interfaces are used to regulate the interfacial electronic structure and optimize the Gibbs free energy of intermediate adsorption during hydrogen production.
[0012] The present invention has the following beneficial effects:
[0013] I. The raw materials used in this invention are readily available, and the preparation process is simple;
[0014] II. This invention is the first to prepare Cu3P / Cu2P4O on the surface of copper foam using a one-step high-temperature phosphating method. 12 / CoP nanowire film catalyst;
[0015] Third, the surface of the film obtained by this invention has many nanowires. The surface of the nanowires is rough and loaded with nanoparticles. By depositing nanoparticles on the surface of the nanowires, the nanoparticles can be immobilized. In addition, this material is synthesized at room temperature, which avoids the material agglomeration problem that exists in the high-temperature synthesis of samples.
[0016] IV. Cu3P / Cu2P4O prepared by this invention 12 The method of using / CoP nanowire membrane catalysts is easy to recycle and reuse. The catalyst prepared in this application is a membrane material. After use, it does not require centrifugation or filtration and can be directly taken out for the next electrocatalytic hydrogen production. It has excellent stability and the synthesis method is relatively simple, thus it has good application prospects.
[0017] V. This invention relates to the preparation of Cu3P / Cu2P4O on copper foam. 12 / CoP nanowire film catalyst, which can be produced on a large scale;
[0018] VI. Cu3P / Cu2P4O prepared by this invention 12 / CoP nanowire film catalyst at 10 mA / cm 2 The alkaline hydrogen production overpotential is 265 mV. Attached Figure Description
[0019] Figure 1 It is the Cu3P / Cu2P4O obtained in step four of Example 1. 12 XRD pattern of / CoP nanowire film catalyst;
[0020] Figure 2 It is the Cu3P / Cu2P4O obtained in step four of Example 1. 12 SEM image of / CoP nanowire film catalyst;
[0021] Figure 3 It is the Cu3P / Cu2P4O obtained in step four of Example 1. 12 Elemental surface scan distribution of / CoP nanowire film catalyst;
[0022] Figure 4 It is the Cu3P / Cu2P4O obtained in step four of Example 1. 12 Polarization curves of alkaline electrocatalytic hydrogen production using / CoP nanowire film catalysts. Detailed Implementation
[0023] The technical solution of the present invention is not limited to the specific embodiments listed below, but also includes any combination of the specific embodiments.
[0024] Specific Implementation Method 1: The preparation method of a copper phosphide / copper phosphate / cobalt phosphide nanowire film catalyst in this embodiment is carried out according to the following steps: 1. Immerse copper foam in a 1-10% (w / w) HCl solution, sonicate for 5-30 min, clean and dry to obtain the treated copper foam.
[0025] 2. The cleaned copper foam was immersed in a mixture of 0.1–2 mol / L alkaline solution and 0.001–0.05 mol / L (NH)4S2O8 and reacted at room temperature for 5–60 min. The resulting blue film was washed and dried in a forced-air drying oven at 150–250 °C to obtain sample A. Then, a three-electrode system was used, with sample A as the working electrode and Ag / AgCl and Pt sheets as the reference and counter electrodes, respectively. Electroreduction was performed in 0.1–2 mol / L alkaline solution at a potential of -1.0–-3.0 V for 0.5–2 h. After the reaction was completed, the sample was washed to obtain Cu nanowires grown on the copper foam. After drying, sample B was obtained.
[0026] 3. Using a three-electrode system, sample B was used as the working electrode, and Ag / AgCl and Pt sheets were used as the reference electrode and counter electrode, respectively. Electrodeposition was carried out in 0.01-1 mol / L Co(NO3)2 solution at a potential of -0.5 to -2.0 V for 30 s to 3600 s. After the reaction was completed, the sample was washed and Co(OH)2 was deposited on Cu nanowires to obtain sample C.
[0027] IV. Place 0.1–2 g of sodium hypophosphite and sample C respectively upstream and downstream of a tube furnace, maintaining a distance of 1–5 cm between them. Raise the temperature to 250–450 °C and hold under a protective atmosphere for 1–5 h. After the reaction is complete, remove the sample, wash it, and dry it to obtain Cu3P / Cu2P4O. 12 / CoP nanowire film catalyst.
[0028] Specific Implementation Method Two: This implementation method differs from Specific Implementation Method One in that the cleaning in step one involves repeatedly washing with deionized water and ethanol 3 to 6 times. Everything else is the same as in Specific Implementation Method One.
[0029] Specific Implementation Method Three: This implementation method differs from Specific Implementation Method One or Two in that the drying in step one involves placing the item in a vacuum drying oven and drying it at 40-60°C. Everything else is the same as in Specific Implementation Method One or Two.
[0030] Specific Implementation Method Four: This implementation method differs from Specific Implementation Methods One to Three in that the mass ratio of the alkaline solution to (NH)4S2O8 in the mixture in step two is 3.5:1. Everything else is the same as in Specific Implementation Methods One to Three.
[0031] Specific Implementation Method Five: This implementation method differs from Specific Implementation Methods One to Four in that the alkaline solution is NaOH, LiOH, or KOH. Everything else is the same as in Specific Implementation Methods One to Four.
[0032] Specific Implementation Method Six: This implementation method differs from Specific Implementation Methods One to Five in that the cleaning in steps two, three, and four involves rinsing with deionized water 3 to 6 times. Everything else is the same as in Specific Implementation Methods One to Five.
[0033] Specific Implementation Method Seven: This implementation method differs from Specific Implementation Methods One to Six in that the heating rate in step four is 1–10 °C / min. Everything else is the same as in Specific Implementation Methods One to Six.
[0034] Specific Implementation Method Eight: This implementation method differs from Specific Implementation Methods One to Seven in that the protective atmosphere is a mixture of argon, nitrogen, or a mixture of argon and nitrogen in any proportion. Everything else is the same as in Specific Implementation Methods One to Seven.
[0035] Specific Implementation Method Nine: This implementation method describes the application of a copper phosphide / copper phosphate / cobalt phosphide nanowire film catalyst as an electrocatalyst for catalytic electrochemical water splitting to produce hydrogen.
[0036] Specific Implementation Method Ten: This implementation method differs from Specific Implementation Method Nine in that the application method is as follows: a three-electrode system is used in a 1.0 M KOH solution, with the sample as the working electrode and Pt and Ag / AgCl electrodes as the counter and reference electrodes, respectively. The electrocatalytic hydrogen production performance of the material is evaluated by polarization curves. Everything else is the same as in Specific Implementation Method Nine.
[0037] The beneficial effects of the present invention are verified using the following embodiments:
[0038] Example 1 This embodiment is a Cu3P / Cu2P4O 12 The method for preparing the / CoP nanowire film catalyst is carried out according to the following steps:
[0039] 1. Immerse the copper foam in a 1.0 wt.% HCl solution and sonicate for 30 minutes to remove the surface oxide film. Then, wash it repeatedly with deionized water and ethanol three times in sequence. Finally, dry it in a vacuum drying oven at 40°C.
[0040] 2. The cleaned Cu foam was immersed in a mixture of 2.5 mol / L NaOH and 0.125 mol / L (NH)4S2O8 and reacted at room temperature for 20 min. The resulting blue film was washed three times with deionized water and dried in a forced-air drying oven at 60 °C. Subsequently, a three-electrode system was used, with the dried sample as the working electrode and Ag / AgCl and Pt sheets as the reference and counter electrodes, respectively. Electroreduction was performed in 1.0 mol / L KOH solution at a potential of -1.0 V for 1 h. After the reaction was completed, the sample was washed three times with deionized water to grow Cu nanowires on the copper foam.
[0041] Third, a three-electrode system was used, with the sample dried in the second step as the working electrode, and Ag / AgCl and Pt sheets as the reference and counter electrodes, respectively. Electrodeposition was performed in 0.1 mol / L Co(NO3)2 solution at a potential of -1 V for 300 s. After the reaction was completed, the sample was washed three times with deionized water to deposit Co(OH)2 on Cu nanowires.
[0042] IV. Mix 0.2g of sodium hypophosphite with an area of 0.5–5cm². 2 The samples obtained in step three were placed upstream and downstream of a tube furnace, maintaining a 3 cm gap between them, and heated to 350°C at a rate of 5°C / min, and held at this temperature for 2 hours under an argon atmosphere. After the reaction was complete, the samples were removed, washed three times with deionized water, and dried to obtain Cu3P / Cu2P4O. 12 / CoP nanowire film catalyst.
[0043] Figure 1 The Cu3P / Cu2P4O obtained in this embodiment 12 XRD pattern of / CoP nanowire film catalyst; by Figure 1 It can be seen that the sample contains the phases Cu3P and Cu2P4O. 12 .
[0044] Figure 2 The Cu3P / Cu2P4O obtained in this embodiment 12 SEM image of the / CoP nanowire film catalyst; by Figure 2 It can be seen that the sample exhibits a nanowire structure and has nanoparticles deposited on its surface.
[0045] Figure 3 The Cu3P / Cu2P4O obtained in this embodiment 12 Elemental surface scan distribution of / CoP nanowire film catalyst; by Figure 3 It can be seen that Cu, Co, P and O elements are present in the sample and are uniformly distributed on the sample surface. In addition, it can be inferred that in addition to copper phosphide, cobalt phosphide material is also present in the sample composition.
[0046] The Cu3P / Cu2P4O obtained in this embodiment 12 / CoP nanowire film catalysts are used for alkaline electrocatalytic hydrogen production. The specific method is as follows: a three-electrode system is used in 1.0M KOH solution, with the sample as the working electrode, and Pt and Ag / AgCl electrodes as the counter electrode and reference electrode, respectively. The electrocatalytic hydrogen production performance of the material is evaluated by polarization curves.
[0047] The results are as follows Figure 4 As shown, by Figure 4 It can be seen that at the same potential, Cu3P / Cu2P4O 12 The current density of the / CoP sample is significantly higher than that of the Cu sample, indicating that Cu3P / Cu2P4O 12 The electrocatalytic hydrogen production activity of the / CoP sample was significantly higher than that of the Cu sample.
Claims
1. A method for preparing a copper phosphide / copper phosphate / cobalt phosphide nanowire film catalyst, characterized in that... This method is performed in the following steps: Immerse the copper foam in a 1-10% (w / w) HCl solution, sonicate for 5-30 minutes, clean and dry to obtain the treated copper foam.
2. The cleaned copper foam was immersed in a mixture of 0.1–2 mol / L alkaline solution and 0.001–0.05 mol / L (NH)4S2O8 and reacted at room temperature for 5–60 min. The resulting blue film was washed and dried in a forced-air drying oven at 150–250 °C to obtain sample A. Then, a three-electrode system was used, with sample A as the working electrode and Ag / AgCl and Pt sheets as the reference and counter electrodes, respectively. Electroreduction was performed in 0.1–2 mol / L alkaline solution at a potential of -1.0–-3.0 V for 0.5–2 h. After the reaction was completed, the sample was washed to obtain Cu nanowires grown on the copper foam. After drying, sample B was obtained.
3. Using a three-electrode system, sample B was used as the working electrode, and Ag / AgCl and Pt sheets were used as the reference electrode and counter electrode, respectively. Electrodeposition was carried out in 0.01-1 mol / L Co(NO3)2 solution at a potential of -0.5 to -2.0 V for 30 s to 3600 s. After the reaction was completed, the sample was washed and Co(OH)2 was deposited on Cu nanowires to obtain sample C. IV. Place 0.1–2 g of sodium hypophosphite and sample C respectively upstream and downstream of a tube furnace, maintaining a distance of 1–5 cm between them. Raise the temperature to 250–450 °C and hold under a protective atmosphere for 1–5 h. After the reaction is complete, remove the sample, wash it, and dry it to obtain Cu3P / Cu2P4O. 12 / CoP nanowire film catalyst.
2. The method for preparing a copper phosphide / copper phosphate / cobalt phosphide nanowire film catalyst according to claim 1, characterized in that, In step one, the cleaning process involves repeatedly washing with deionized water and ethanol 3 to 6 times.
3. The method for preparing a copper phosphide / copper phosphate / cobalt phosphide nanowire film catalyst according to claim 1, characterized in that, The drying process in step one involves placing the item in a vacuum drying oven and drying it at 40–60°C.
4. The method for preparing a copper phosphide / copper phosphate / cobalt phosphide nanowire film catalyst according to claim 1, characterized in that, In step two, the mass ratio of alkaline solution to (NH)4S2O8 in the mixed solution is 3.5:
1.
5. The method for preparing a copper phosphide / copper phosphate / cobalt phosphide nanowire film catalyst according to claim 1, characterized in that, The alkaline solution is NaOH, LiOH, or KOH.
6. The method for preparing a copper phosphide / copper phosphate / cobalt phosphide nanowire film catalyst according to claim 1, characterized in that, The cleaning in steps two, three, and four involves rinsing with deionized water 3 to 6 times.
7. The method for preparing a copper phosphide / copper phosphate / cobalt phosphide nanowire film catalyst according to claim 1, characterized in that, The heating rate in step four is 1–10 °C / min.
8. The method for preparing a copper phosphide / copper phosphate / cobalt phosphide nanowire film catalyst according to claim 1, characterized in that, The protective atmosphere is a mixture of argon, nitrogen, or argon and nitrogen in any proportion.
9. The application of the copper phosphide / copper phosphate / cobalt phosphide nanowire film catalyst prepared according to claim 1 as an electrocatalyst for catalytic electrochemical water splitting to produce hydrogen.
10. The application according to claim 9, characterized in that, The application method is as follows: a three-electrode system is used in 1.0M KOH solution, with the sample as the working electrode and Pt and Ag / AgCl electrodes as the counter electrode and reference electrode, respectively, and the electrocatalytic hydrogen production performance of the material is evaluated by polarization curves.
Citation Information
Patent Citations
Phosphorus-doped cobalt hydroxide / copper nanowire, preparation method thereof and zinc-nitrate battery
CN120288815A