Preparation method and application of supported bimetallic oxide sludge-based mesoporous ceramsite
Through the preparation of loaded bimetal oxide sludge-based mesoporous ceramsite, the problem of insufficient performance of sludge water treatment ceramsite was solved, and efficient removal of COD and total phosphorus in pharmaceutical wastewater was achieved, reducing treatment costs and avoiding Secondary pollution was eliminated, demonstrating the effectiveness and environmental benefits of this technology.
Patent Information
- Application Number
- CN202311225461.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-09-21
- Publication Date
- 2024-10-18
- Estimated Expiration
- 2043-09-21
AI Technical Summary
Existing sludge water treatment ceramsite has limited performance, low interfacial reactivity, and uneven pore structure, making it difficult to efficiently remove COD and total phosphorus in pharmaceutical wastewater. Moreover, traditional treatment methods are costly and prone to secondary pollution.
The preparation method of supported bimetal oxide sludge-based mesoporous ceramsite is used to form ceramics with high reactivity and uniform pore structure through sludge pretreatment, ceramsite raw material preparation, bimetal gradient loading and two-stage sintering. particles, using La3+/Fe3+ ion loading to enhance catalytic and adsorption capabilities.
It achieves efficient removal of COD and total phosphorus in pharmaceutical wastewater, reduces treatment costs, and avoids secondary pollution. The ceramsite has good mechanical strength and stability and is suitable for resource utilization.
Smart Images

Figure CN117263716B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of phosphorus-containing pharmaceutical wastewater treatment, and specifically relates to a preparation method and application of loaded bimetallic oxide sludge-based mesoporous ceramsite. Background Art
[0002] The residual sludge from urban sewage treatment plants is an inevitable by-product of the sewage treatment process. It concentrates and collects 30%-50% of the pollutants and organic matter in the sewage, and also contains a small amount of pathogens, heavy metals and other toxic and harmful substances. It is easy to cause secondary pollution if it is not treated in a standardized manner. The characteristics of sludge such as loose structure, large porosity, and large specific surface area determine its potential advantages as a water treatment material. It can not only solve the problem of residual sludge being difficult to store and causing secondary pollution, and realize the "waste-to-treasure" of sludge; it can also solve the problem of the difficulty of industrial sewage treatment, and realize the "waste-to-waste" of sludge. Therefore, sludge as a water treatment material is a feasible way to utilize sludge resources, and it is an important research direction for the green development of the sewage treatment industry.
[0003] The sludge in the sewage treatment plant is prepared into water treatment ceramsite, which has the characteristics of high porosity, low density, high strength and corrosion resistance, and is applied to the field of environmental protection as filter materials, adsorbent materials, catalytic materials, etc. For example, CN105732076A discloses a method for preparing sludge slag ceramsite, which mixes sewage plant sludge, slag and clay after drying, and then calcines at 1030-1100°C to obtain sludge slag ceramsite, which can be used for biological filter tank method to treat wastewater, and can also be used as building materials. CN106673699A discloses a method for preparing water plant sludge-based porous ceramsite doped with bamboo and wood powder, which mixes powdered sludge and powdered bamboo and wood powder and granulates them, and then washes them with hydrochloric acid and distilled water in turn after calcination, and dries them to obtain sludge-based porous ceramsite, which improves the porosity. However, the performance of the current sludge water treatment ceramsite is very limited. On the one hand, the interfacial reaction activity is not high, the reaction time is long, and the treatment efficiency is low. On the other hand, the pore structure is uneven. If the pores are too large, the actual contact area between small molecule pollutants and ceramsite is small, causing small molecule pollutants to escape; if the pores are too small, large molecule pollutants cannot enter the pores of ceramsite, causing large molecule pollutants to escape. Therefore, taking into account both efficient reaction activity and uniform pore structure is the key technical issue for preparing ceramsite for water treatment from sludge.
[0004] The rapid development of the pharmaceutical industry has led to an increasing discharge of pharmaceutical wastewater. Pharmaceutical wastewater has the characteristics of large changes in water quality and quantity, complex composition, high COD concentration, poor biodegradability, etc. It has certain acute toxicity and microbial inhibition. It is a difficult-to-degrade organic chemical wastewater and seriously pollutes water quality. At the same time, some pharmaceutical companies have introduced a large number of phosphorus-containing agents such as potassium dihydrogen phosphate, phosphorus trichloride, and organophosphorus reagents as auxiliary raw materials. For example, when producing products such as adenine, fosfomycin sodium, and adenosine triphosphate, a large amount of wastewater containing organic and inorganic phosphorus will be produced, resulting in a high total phosphorus concentration in the wastewater. Among the traditional pharmaceutical wastewater treatment methods, physical and chemical methods such as flocculation precipitation, dilution, membrane separation, ion exchange, electrolysis, neutralization and oxidation can treat difficult-to-degrade organic pollutants, but the treatment cost is high and it is also easy to produce secondary pollution; biological methods such as anaerobic biological treatment and advanced oxidation treatment are mainly suitable for wastewater with good biodegradability, and the treatment effect of wastewater containing difficult-to-degrade organic pollutants is not good. COD is one of the most important indicators affecting water pollution, and total phosphorus is the main controlling factor causing eutrophication of water bodies. How to simultaneously and efficiently remove COD and total phosphorus has become a hot issue that needs to be urgently resolved in the field of water treatment. Summary of the invention
[0005] In view of the above technical problems, the present invention provides a preparation method and application of loaded bimetallic oxide sludge-based mesoporous ceramsite. The prepared loaded bimetallic oxide sludge-based mesoporous ceramsite has the advantages of mesoporous structure, developed pores, high reaction activity, high strength, etc., and can also simultaneously and synergistically remove COD and total phosphorus in water.
[0006] In order to achieve the above object, the present invention provides a method for preparing a supported bimetallic oxide sludge-based mesoporous ceramsite, comprising the following steps:
[0007] (1) Sludge pretreatment: The sludge is dried in a natural state until the moisture content is less than 10%, then ground, dried and sieved to obtain sludge powder;
[0008] (2) Preparation of ceramsite raw material: at room temperature, the sludge powder obtained in step (1) is mixed with fly ash and montmorillonite powder, and then granulated and sieved to obtain wet granules, which are then dried to obtain ceramsite raw material;
[0009] (3) First-stage sintering: sintering the ceramsite raw material obtained in step (2) and obtaining a ceramsite masterbatch after cooling;
[0010] (4) Bimetallic gradient loading: Weigh the ceramsite masterbatch obtained in step (3) and mix it with the modified solution in proportion, soak it for a period of time and then let it stand for 8-48 hours. After solid-liquid separation, wash it repeatedly with water until the pH of the filtrate is neutral. Then, dry the solid matter in an oven at 105°C to obtain the loaded La 3+ / Fe 3+ Sludge ceramsite;
[0011] (5) Second stage sintering: The obtained loaded La 3+ / Fe 3+ The sludge ceramsite is sintered and cooled to obtain the loaded bimetallic oxide sludge-based mesoporous ceramsite.
[0012] Preferably, the sludge in step (1) is sludge from a sewage treatment plant with a water content of 40-85%; and the particle size of the sludge powder is 100-200 mesh.
[0013] Preferably, the mass ratio of the sludge powder to the fly ash and montmorillonite powder in step (2) is 40-80:5-30:5-25, the particle sizes of the fly ash and montmorillonite powder are both 200-250 mesh; and the particle size of the ceramsite raw material is 4-6 mm.
[0014] Preferably, the sintering conditions in step (3) are to first heat the temperature to 200-400°C at a rate of 8-15°C / min, preheat for 0.25-3 h, and then heat the temperature for 5-10 h. o C / min to 750-1250℃ and keep it at this temperature for 0.5-2 h.
[0015] Preferably, the modified solution in step (4) is Fe(NO3)3 solution and La(NO3)3 solution, and the mass ratio of ceramsite masterbatch to modified solution is 1:(2-10); the immersion condition is at 25 o C. Immerse for 1-8 h at 200 rpm / min.
[0016] Further preferably, the concentration of the Fe(NO3)3 solution is 0.050-0.150 mol / L, and the concentration of the La(NO3)3 solution is 0.025-0.100 mol / L; the concentration ratio of the Fe(NO3)3 solution to the La(NO3)3 solution is (1-3):1; and the volume ratio is 1:1.
[0017] Preferably, the sintering conditions in step (5) are preheating at 150°C for 30 min, then heating to 300-600°C and sintering for 0.25-2 h.
[0018] The present invention also provides a loaded bimetallic oxide sludge-based mesoporous ceramsite prepared according to the above preparation method.
[0019] The invention also provides application of supported bimetallic oxide sludge-based mesoporous ceramsite in pharmaceutical wastewater.
[0020] Preferably, the pharmaceutical wastewater is phosphorus-containing pharmaceutical wastewater, wherein the COD concentration is 50-500 mg / L and the total phosphorus concentration is 10-50 mg / L.
[0021] The beneficial effects of the present invention are:
[0022] 1. Using a large amount of chemical components such as silicon and iron and a large amount of organic active substances contained in the sludge of the sewage treatment plant as the basic structure of the ceramsite, using the glass, aluminum and a small amount of unburned carbon in the fly ash and the aluminum, silicon and other components contained in the montmorillonite, a stable porous structure is formed after sintering, and pores are formed inside the ceramsite to increase the strength of the ceramsite. At the same time, high-temperature sintering can also fully burn and decompose organic pollutants in the raw materials, and make heavy metals migrate to the flue gas or solidify in the glass phase and lattice, which not only saves precious raw material resources such as clay, but also avoids the accumulation and discharge of sludge and fly ash, reduces environmental pollution, and realizes the resource utilization and harmless utilization of solid waste.
[0023] 2. The sludge ceramsite prepared by the present invention is a more practical molding material, which overcomes the defect that traditional powder materials will form bottom sludge that is difficult to recycle. The sludge prepared into ceramsite is conducive to recycling, that is, it can be directly applied to water bodies, and can also be loaded in reaction carriers for application, and will not cause secondary pollution to the environment.
[0024] 3. Choose bimetallic La 3+ / Fe 3+ When loaded in ceramsite, on the one hand, both Fe ions and La ions are in a stable +3 valence state, which is conducive to reacting with macromolecular organic pollutants in water to form complexes; on the other hand, the radius of La ions is twice that of Fe ions, which makes it easy to achieve uniform dispersion of Fe ions during the loading process, and the three electrons in the 4f orbit of La element are more reactive, which will enhance the catalytic activity of Fe ions. 3+ / Fe 3+ The loading gives the sludge ceramsite a high catalytic degradation ability for macromolecular organic pollutants and an affinity for total phosphorus pollutants, thereby achieving effective degradation of organic pollutants in pharmaceutical wastewater and effective enrichment of total phosphorus pollutants.
[0025] 4. The prepared loaded bimetallic oxide sludge-based mesoporous ceramsite contains rich silicon hydroxyl groups and metal oxides. The hydroxyl groups are easy to coordinate and exchange with the adsorbent to form chemical bonds, which is beneficial to the chemical adsorption of most anionic pollutants, and decompose the large molecular organic pollutants in the sewage into CO2 and H2O. While the CO2 gas is discharged, more abundant reaction sites are released in the ceramsite to further enhance the chemical adsorption of total phosphorus pollutants, achieving the synergistic removal of total phosphorus while efficiently degrading COD.
[0026] 5. There are two sintering processes in the preparation process, and both adopt the method of preheating first and then high-temperature sintering. Preheating can remove the residual crystal water inside the ceramsite, prevent the ceramsite from expanding and rupturing after rapid heating, ensure that the ceramsite has a certain strength, and carbonize and decompose the organic matter inside the ceramsite to improve the expansion performance of the ceramsite. During high-temperature sintering, the organic matter can volatilize and escape to form a porous structure, which has a load effect and improves the mechanical strength of the ceramsite; the second high-temperature sintering removes the crystal water in the modified ceramsite, prevents the ceramsite from expanding and rupturing after rapid heating, and roasting makes La 3+ / Fe 3+ It is converted into oxides and solidified in the pores of the expanded clay, making the pores denser, making it less likely to fall off during use and improving stability.
[0027] 6. Based on the fact that most COD pollutants in pharmaceutical wastewater are mesopores, a loaded bimetallic oxide sludge-based mesoporous ceramsite with a rich mesoporous structure was prepared, so that COD pollutants can be removed inside the pores of the ceramsite, avoiding the problems of too large pore size, too small specific surface area, and low strength, and also avoiding the problem of too small pore size and inability to remove COD pollutants.
[0028] 7. The loaded bimetallic oxide sludge-based mesoporous ceramsite prepared by the present invention is used in the treatment of phosphorus-containing pharmaceutical wastewater. It is a heterogeneous solid catalyst. Compared with the traditional homogeneous Fenton method, it can overcome the problem of secondary pollution of iron sludge solid waste and will not affect the chromaticity of the effluent. It has a good adsorption and removal effect on COD and total phosphorus in actual pharmaceutical wastewater.
[0029] 8. The preparation method of the present invention is simple and easy to operate, and the reaction conditions during modification are mild. The prepared loaded bimetallic oxide sludge-based mesoporous ceramsite is harmless, stable and recyclable. The preparation method is simple, the raw material source is wide, the cost is low, and it has good economic benefits, environmental benefits and social benefits. BRIEF DESCRIPTION OF THE DRAWINGS
[0030] Figure 1 The present invention is a flow chart for preparing the supported bimetallic oxide sludge-based mesoporous ceramsite.
[0031] Figure 2 The N2 adsorption-desorption curves (BET) of the loaded bimetallic oxide sludge-based mesoporous ceramsite prepared in Examples 1-2, wherein (a) is the N2 adsorption-desorption curve (BET) of Example 1, and (b) is the N2 adsorption-desorption curve (BET) of Example 2.
[0032] Figure 3 These are the images of the loaded bimetallic oxide sludge-based mesoporous ceramsite samples prepared in Examples 1-4, wherein (a) is Example 1, (b) is Example 2, (c) is Example 3, and (d) is Example 4.
[0033] Figure 4 The scanning electron microscope (SEM) and energy spectrum scanning diagram (Mapping) of the loaded bimetallic oxide sludge-based mesoporous ceramsite prepared in Example 2, wherein (a) is a scanning electron microscope image of the ceramsite surface, (b) is a magnified scanning electron microscope image of the ceramsite microstructure, (c) is a Si element energy spectrum scanning diagram, (d) is an Al element energy spectrum scanning diagram, (e) is a La element energy spectrum scanning diagram, and (f) is a Fe element energy spectrum scanning diagram.
[0034] Figure 5 This is a diagram of the photochemical reaction device of Example 5, in which 1 is a magnetic stirrer, 2 is a tungsten filament lamp, 3 is a cooling water outlet, 4 is a thermometer, 5 is waste water, 6 is a cooling water inlet, and 7 is a reactor.
[0035] Figure 6 Schematic diagram of the removal of COD and total phosphorus by the loaded bimetallic oxide sludge-based mesoporous ceramsite in the present invention.
[0036] Figure 7 This is the treatment effect of the loaded bimetallic oxide sludge-based mesoporous ceramsite prepared in Example 1 on pharmaceutical wastewater.
[0037] Figure 8 This is a diagram of the fluidized bed reaction device of Example 6, in which 1 is a water inlet pipe, 2 is a drug inlet pipe, 3 is a water inlet peristaltic pump, 4 is a drug inlet peristaltic pump, 5 is a sedimentation bin, 6 is a bottom layer of quartz wool, 7 is a reaction column, 8 is an adsorption layer, 9 is a top layer of quartz wool, 10 is a clean water bin, and 11 is a water outlet pipe. DETAILED DESCRIPTION
[0038] The technical solution of the present invention is further explained below in conjunction with the accompanying drawings and specific embodiments. It is worth noting that the following embodiments are only preferred embodiments of the present invention and should not be understood as limiting the present invention. The protection scope of the present invention shall be based on the contents recorded in the claims. Any modification or replacement made by those skilled in the art to the technical solution of the present invention without creative work shall fall within the protection scope of the present invention.
[0039] Example 1
[0040] according to Figure 1 The process shown is used to prepare the supported bimetallic oxide sludge-based mesoporous ceramsite, and the specific steps are as follows:
[0041] (1) Take the residual sludge with a moisture content of 82.25% from a sewage treatment plant and dry it in a natural state until the moisture content is below 10%. Grind it and dry it at 45°C, then pass it through a 100-mesh sieve to obtain sludge powder;
[0042] (2) Grind fly ash and montmorillonite and pass them through a 200-mesh sieve to obtain powders. Then, mix 25 parts of the sludge powder prepared in step (1), 15 parts of fly ash powder and 10 parts of montmorillonite powder thoroughly. Then, granulate and screen wet granules with a particle size of 4-6 mm. o C and dried to obtain the sludge ceramsite raw material;
[0043] (3) The sludge ceramsite raw material prepared in step (2) is placed in a corundum crucible, and then placed in a muffle furnace, heated to 300°C at a rate of 10°C / min for preheating for 1 h, then heated to 1050°C at a rate of 8°C / min, and calcined at 1050°C for 2 h, and then cooled to obtain a sludge ceramsite masterbatch;
[0044] (4) Weigh 10 g of the sludge ceramsite masterbatch prepared in step (3) and place it in a 150 mL round-bottom flask. Add 25 mL of 0.125 mol / L Fe(NO3)3 solution and 25 mL of 0.050 mol / L La(NO3)3 solution successively. Then place the round-bottom flask in a 25 °C constant temperature water bath and stir and immerse for 4 h at a speed of 200 r / min. After aging for 24 h, separate the solid and liquid through a suction filtration device. Then rinse the filtrate repeatedly with deionized water until the pH of the filtrate is neutral. Dry the filtrate in an oven at 105 °C to obtain the loaded La 3+ / Fe 3+ Sludge ceramsite;
[0045] (5) The loaded La prepared in step (4) 3+ / Fe 3+ The sludge ceramsite was put into a corundum crucible, and then placed in a muffle furnace and heated to 150 ℃ at a rate of 8 ℃ / min for preheating for 30 min, and then heated to 400 ℃ and sintered for 1 h to obtain the loaded bimetallic oxide sludge-based mesoporous ceramsite.
[0046] Example 2
[0047] (1) The residual sludge with a moisture content of 78.67% from a sewage treatment plant was dried to a moisture content of less than 10% under natural conditions, and then ground and heated at 45 o C is dried and passed through a 100-mesh sieve to obtain sludge powder;
[0048] (2) Grinding fly ash and montmorillonite and passing through a 200-mesh sieve to obtain powders respectively, and then thoroughly mixing 27.5 parts of the sludge powder prepared in step (1), 10 parts of fly ash powder and 12.5 parts of montmorillonite powder, and then granulating and screening wet particles with a particle size in the range of 4-6 mm, and drying at 105°C to obtain sludge ceramsite raw material;
[0049] (3) The sludge ceramsite raw material prepared in step (2) is placed in a corundum crucible, and then placed in a muffle furnace, heated to 300°C at a rate of 10°C / min, preheated for 1 h, then heated to 950°C at a rate of 8°C / min, and calcined at 950°C for 1 h, and then cooled to obtain a sludge ceramsite masterbatch;
[0050] (4) Weigh 10 g of the sludge ceramsite masterbatch prepared in step (3) and place it in a 150 mL round-bottom flask. Add 25 mL of 0.075 mol / L Fe(NO3)3 solution and 25 mL of 0.050 mol / L La(NO3)3 solution successively. Then place the round-bottom flask at 25 o C constant temperature water bath with stirring for 2 h at a speed of 200 r / min, and then allowed to stand for 12 h, solid-liquid separation was performed by suction filtration, and the filtrate was repeatedly rinsed with deionized water until the pH of the filtrate was neutral. o C in an oven to obtain the load La 3+ / Fe 3+ Sludge ceramsite;
[0051] (5) The loaded La prepared in step (4) 3+ / Fe 3+ The sludge ceramsite was placed in a corundum crucible and then placed in a muffle furnace and heated to 150 °C at a rate of 8 °C / min for 30 min, then heated to 400 °C. o C for 2 h to obtain the loaded bimetallic oxide sludge-based mesoporous ceramsite.
[0052] Example 3
[0053] (1) Take the residual sludge with a moisture content of 79.69% from a sewage treatment plant and dry it in a natural state until the moisture content is below 10%. Grind it and dry it at 45℃ and pass it through a 100-mesh sieve to obtain sludge powder;
[0054] (2) Grinding fly ash and montmorillonite and passing through a 200-mesh sieve to obtain powders respectively, and then thoroughly mixing 30 parts of the sludge powder prepared in step (1), 12.5 parts of fly ash powder and 7.5 parts of montmorillonite powder, and then granulating and screening wet particles with a particle size in the range of 4-6 mm, and drying at 105° C. to obtain sludge ceramsite raw material;
[0055] (3) The sludge ceramsite raw material prepared in step (2) was placed in a corundum crucible, and then placed in a muffle furnace and heated to 300°C at a rate of 10°C / min. o C for 1 h, then heated to 1050°C at 8°C / min, and kept at 1050°C for 1 h, and then cooled to obtain the sludge ceramsite masterbatch;
[0056] (4) Weigh 10 g of the sludge ceramsite masterbatch prepared in step (3) and place it in a 150 mL round-bottom flask. Add 25 mL of 0.100 mol / L Fe(NO3)3 solution and 25 mL of 0.050 mol / L La(NO3)3 solution successively. Then place the round-bottom flask in a 25 °C constant temperature water bath and stir and immerse for 4 h at a speed of 200 r / min. After aging for 24 h, separate the solid and liquid through a suction filtration device. Then rinse the filtrate repeatedly with deionized water until the pH of the filtrate is neutral. Dry the filtrate in an oven at 105 °C to obtain the loaded La 3+ / Fe 3+ Sludge ceramsite;
[0057] (5) The loaded La prepared in step (4) 3+ / Fe 3+ The sludge ceramsite was put into a corundum crucible, and then placed in a muffle furnace and heated to 200 ℃ at a rate of 8 ℃ / min for preheating for 30 min, and then heated to 450 ℃ and sintered for 1 h to obtain the loaded bimetallic oxide sludge-based mesoporous ceramsite.
[0058] Example 4
[0059] (1) The residual sludge with a moisture content of 81.33% from a sewage treatment plant was dried naturally to a moisture content of less than 10%, ground and dried at 45°C, and then passed through a 100-mesh sieve to obtain sludge powder;
[0060] (2) Grinding fly ash and montmorillonite and passing through a 200-mesh sieve to obtain powders respectively, and then thoroughly mixing 30 parts of the sludge powder prepared in step (1), 7.5 parts of fly ash powder and 12.5 parts of montmorillonite powder, and then granulating and screening wet particles with a particle size in the range of 4-6 mm, and drying at 105°C to obtain sludge ceramsite raw material;
[0061] (3) The sludge ceramsite raw material prepared in step (2) was placed in a corundum crucible, and then placed in a muffle furnace and heated to 300°C at a rate of 10°C / min. o C for 1 h, then heat to 1050 C at 8 °C / min. o C, and calcined at 1050℃ for 1h, and then cooled to obtain the sludge ceramsite masterbatch;
[0062] (4) Weigh 10 g of the sludge ceramsite masterbatch prepared in step (3) and place it in a 150 mL round-bottom flask. Add 25 mL of 0.050 mol / L Fe(NO3)3 solution and 25 mL of 0.050 mol / L La(NO3)3 solution successively. Then place the round-bottom flask in a 25 °C constant temperature water bath and stir and immerse for 4 h at a speed of 200 r / min. After standing and aging for 12 h, separate the solid and liquid through a suction filtration device. Then rinse the filtrate repeatedly with deionized water until the pH of the filtrate is neutral. Dry the filtrate in an oven at 105 °C to obtain the loaded La 3+ / Fe 3+ Sludge ceramsite;
[0063] (5) The loaded La prepared in step (4) 3+ / Fe 3+ The sludge ceramsite was put into a corundum crucible, and then placed in a muffle furnace and heated to 200°C at a rate of 8°C / min for preheating for 30 min, and then heated to 450°C and sintered for 1 h to obtain the loaded bimetallic oxide sludge-based mesoporous ceramsite.
[0064] Results test:
[0065] The loaded bimetallic oxide sludge-based mesoporous ceramsite prepared in Examples 1-4 was tested for strength, chemical composition, structural parameters, heavy metal leaching content, and N2 adsorption and desorption. The results are shown in Tables 1 and 2, respectively. The strength detection method refers to the molecular sieve crushing resistance test method (HG / T 2783-2020), and the structural parameter detection is carried out using the automatic surface analyzer (Belsorp-minII) of Japan's Mychik Bayer Company, which is mainly used to determine the specific surface area, pore volume, pore size distribution and nitrogen adsorption and desorption curve of the ceramsite; the detection method of heavy metal leaching content refers to the identification standard for hazardous waste leaching toxicity identification (GB 5085.3-2007) for detection.
[0066] Table 1 Raw material dosage and strength of supported bimetallic oxide sludge-based mesoporous ceramsite
[0067]
[0068] Table 2 Chemical composition of supported bimetallic oxide sludge-based mesoporous ceramsite / (%)
[0069]
[0070] Table 3 Pore structure parameters of supported bimetallic oxide sludge-based mesoporous ceramsite
[0071]
[0072] Table 4 Heavy metal leaching content of supported bimetallic oxide sludge-based mesoporous ceramsite (mg·L -1 )
[0073]
[0074] It can be seen from the above data that when the mass ratio of sludge to fly ash and montmorillonite is 5:3:2 (Example 1), the strength of the supported bimetallic oxide sludge-based mesoporous ceramsite prepared by calcining at 1050°C for 2h is the highest, which is 4.55MPa, while when the mass ratio is 5.5:2:2.5 (Example 2), the strength of the supported bimetallic oxide sludge-based mesoporous ceramsite prepared by calcining at 950°C for 2h is the highest, which is 4.55MPa. o The product prepared by calcining at 40 °C for 1 h has the lowest strength, which is 3.68 MPa. This shows that when the mass ratio of sludge, fly ash and montmorillonite does not change significantly, the strength of ceramsite is related to the calcination temperature and time. The higher the calcination temperature and the longer the calcination time, the greater the strength of ceramsite. 3+ / Fe 3+ With the increase of concentration ratio, the iron content in the ceramsite prepared in Example 1-4 increased (Fe2O3 content increased from 6.27 to 8.24), and the lanthanum content decreased relatively (La2O3 content decreased from 1.14 to 0.96). 3+ / Fe 3+ When the concentration ratio is 1:2, the modified metal loading rate is the most efficient.
[0075] The structural parameters of the supported bimetallic oxide sludge-based mesoporous ceramsite prepared under different raw materials, calcination temperatures and different modified concentration ratios are also different. Under the premise that the particle size is 4-6 mm, the S of the product prepared in Example 2 is BET The single pore volume and total pore volume are the highest, which are 52850 cm 2 / g, 0.619cm 3 / g and 0.0083 cm 3 / g, the lowest average pore size is 13.868 nm; followed by Example 3; the largest average pore size is 16.627 nm for the loaded bimetallic oxide sludge-based mesoporous ceramsite prepared in Example 1. The above results show that when the calcination temperature is 950°C, the liquid phase viscosity is low, the crystal melting rate is low, and the pore size is large. As the sintering temperature increases and the calcination time prolongs, the glassy melt in the ceramsite increases, the structure collapses, and the pore size decreases. As the modified concentration ratio increases, the content of iron and lanthanum in the ceramsite increases, proving that the loading of iron and lanthanum will also increase the specific surface area of the ceramsite.
[0076] In the heavy metal leaching experiment, it can be seen from Examples 2, 4 and 1, 4 that when the calcination temperature is low or the calcination time is short, the solidification effect of heavy metals is poor, and as the calcination temperature and time increase, the heavy metal leaching rate becomes smaller and smaller. The leaching amounts of Cu, Zn, Pb, Cd, Cr, and Ni of the supported bimetallic oxide sludge-based mesoporous ceramsite prepared in Examples 1-4 are far less than the provisions of GB 5085.3-2007, indicating that the supported bimetallic oxide sludge-based mesoporous ceramsite prepared in Examples 1-4 has low heavy metal leaching content and little pollution to the environment, and can be used in the field of sewage treatment.
[0077] The N2 adsorption and desorption curves of the supported bimetallic oxide sludge-based mesoporous ceramsite prepared in Example 1-2 are as follows: Figure 2 As shown, the adsorption / desorption curve of the ceramsite is of Tape (III) type, all showing the characteristics of increased adsorption volume and hysteresis, and the hysteresis loop in the isotherm belongs to the type II line in the H3 hysteresis loop. When the calcination temperature is low, the specific surface area of Example 2 is larger than that of Example 1. The above results show that the ceramsite is formed by particle aggregation, resulting in an interconnected irregular pore structure, which increases the specific surface area and is beneficial to improving the adsorption performance of the ceramsite.
[0078] The appearance of the supported bimetallic oxide sludge-based mesoporous ceramsite prepared in Example 1-4 is as follows Figure 3 As shown, when the calcination temperature is low (Example 2), the ceramsite is light yellow ( Figure 3 b), when the calcination temperature is higher (Examples 1, 3 and 4), it is brown ( Figure 3 a\c and d), which proves that the ceramsite components will undergo chemical reactions under calcination conditions. The reaction is not complete when the temperature is low, and the dark color indicates that the temperature is too high or the calcination time is too long and the particles are burned.
[0079] The scanning electron microscope photo and energy spectrum scanning diagram of the supported bimetallic oxide sludge-based mesoporous ceramsite prepared in Example 2 are as follows: Figure 4 As shown by Figure 4 From (a) and (b) in the figure, it can be seen that the modified ceramsite has obvious holes. After zooming in, it can be seen that there are obvious sediments attached to the surface of the ceramsite, and the surface becomes rough, indicating that iron and lanthanum are successfully loaded onto the surface of the ceramsite. From the EDS-Mapping diagram ( Figure 4 From (c), (d), (e) and (f) in the figure, we can see that the expanded clay contains a large amount of silicon and aluminum elements, as well as iron and lanthanum elements, which further verifies that lanthanum and iron are successfully loaded onto the surface of the expanded clay.
[0080] Comparative Example 1
[0081] (1) Take the residual sludge with a moisture content of 78.67% from a sewage treatment plant and dry it in a natural state until the moisture content is below 10%. Grind it and dry it at 45°C, then pass it through a 100-mesh sieve to obtain sludge powder.
[0082] (2) Grinding fly ash and montmorillonite and passing through a 200-mesh sieve to obtain powders respectively, and then thoroughly mixing 30 parts of the sludge powder prepared in step (1), 12.5 parts of fly ash powder and 7.5 parts of montmorillonite powder, and then granulating and screening wet particles with a particle size in the range of 4-8 mm, and drying at 105° C. to obtain sludge ceramsite raw material;
[0083] (3) The sludge ceramsite raw material prepared in step (2) is placed in a corundum crucible, and then placed in a muffle furnace, heated to 300 °C at a rate of 10 °C / min, preheated for 1 h, then heated to 1050 °C at 8 °C / min, and sintered at 1050 °C for 1 h, and then cooled to obtain sludge ceramsite.
[0084] Comparative Example 2
[0085] (1) Take the residual sludge with a moisture content of 78.67% from a sewage treatment plant and dry it in a natural state until the moisture content is below 10%. Grind it and dry it at 45°C, then pass it through a 100-mesh sieve to obtain sludge powder.
[0086] (2) Grinding fly ash and montmorillonite and passing through a 200-mesh sieve to obtain powders respectively, and then thoroughly mixing 30 parts of the sludge powder prepared in step (1), 12.5 parts of fly ash powder and 7.5 parts of montmorillonite powder, and then granulating and screening wet particles with a particle size in the range of 4-8 mm, and drying at 105° C. to obtain sludge ceramsite raw material;
[0087] (3) The sludge ceramsite raw material prepared in step (2) is placed in a corundum crucible, and then placed in a muffle furnace, heated to 300°C at a rate of 10°C / min, preheated for 1 h, then heated to 1050°C at a rate of 8°C / min, and fired at 1050°C for 1 h, and then cooled to obtain sludge ceramsite.
[0088] (4) Weigh 10 g of the sludge ceramsite masterbatch prepared in step (3) and place it in a 150 mL round-bottom flask. Add 25 mL of a 0.100 mol / L Fe(NO3)3 solution. Then place the round-bottom flask in a 25°C constant temperature water bath and stir for 4 h at a speed of 200 r / min. After aging for 12 h, separate the solid and liquid through a suction filtration device. Then rinse the filtrate repeatedly with deionized water until the pH of the filtrate is neutral. Dry the filtrate in an oven at 105°C to obtain a Fe-loaded ceramsite. 3+ Sludge ceramsite;
[0089] (5) The loaded La prepared in step (4) 3+The sludge ceramsite was put into a corundum crucible, and then placed in a muffle furnace and heated to 200 °C at a rate of 8 °C / min for preheating for 30 min, and then heated to 450 °C and sintered for 1 h to obtain the loaded iron metal oxide sludge-based mesoporous ceramsite.
[0090] Comparative Example 3
[0091] (1) Take the residual sludge with a moisture content of 78.67% from a sewage treatment plant and dry it in a natural state until the moisture content is below 10%. Grind it and dry it at 45℃, then pass it through a 100-mesh sieve to obtain sludge powder;
[0092] (2) Grind fly ash and montmorillonite and pass them through a 200-mesh sieve to obtain powders. Then, 30 parts of the sludge powder prepared in step (1), 12.5 parts of fly ash powder and 7.5 parts of montmorillonite powder are thoroughly mixed. Then, wet granules with a particle size of 4-8 mm are sieved and granulated at 105 o C and dried to obtain the sludge ceramsite raw material;
[0093] (3) The sludge ceramsite raw material prepared in step (2) was placed in a corundum crucible, and then placed in a muffle furnace, and heated to 300 °C at a rate of 10 °C / min, preheated for 1 h, and then heated for 8 h. o The temperature was raised to 1050 ℃ at 1050 ℃ at a speed of 1000 ℃ / min, and the mixture was fired at 1050 ℃ for 1 h. After cooling, the sludge ceramsite was obtained.
[0094] (4) Weigh 10 g of the sludge ceramsite masterbatch prepared in step (3) and place it in a 150 mL round-bottom flask, add 25 mL of 0.050 mol / L La(NO3)3 solution, and then place the round-bottom flask in a 25 °C constant temperature water bath and stir for 4 h at a speed of 200 r / min. After aging for 12 h, separate the solid and liquid through a suction filtration device, and then repeatedly rinse the filtrate with deionized water until the pH of the filtrate is neutral. Place the filtrate in an oven at 105 °C to dry to obtain the loaded La 3+ Sludge ceramsite;
[0095] (5) The loaded La prepared in step (4) 3+ The sludge ceramsite was put into a corundum crucible, and then placed in a muffle furnace and heated to 200 °C at a rate of 8 °C / min for preheating for 30 min, and then heated to 45 °C and kept at this temperature for 1 h to obtain lanthanum metal oxide-loaded sludge-based mesoporous ceramsite.
[0096] Comparative Example 4
[0097] (1) Take the residual sludge with a moisture content of 78.67% from a sewage treatment plant and dry it in a natural state until the moisture content is below 10%. Grind it and dry it at 45℃, then pass it through a 100-mesh sieve to obtain sludge powder;
[0098] (2) Weigh 10 g of sludge powder and place it in a 150 mL round-bottom flask, add 25 mL of 0.100 mol / L Fe(NO3)3 solution and 25 mL of 0.050 mol / L La(NO3)3 solution, then place the round-bottom flask in a 25 °C constant temperature water bath and stir for 4 h at a speed of 200 r / min. After aging for 12 h, separate the solid and liquid through a suction filtration device, then rinse the filtrate repeatedly with deionized water until the pH of the filtrate is neutral, and dry the filtrate in a 105 °C oven to obtain the loaded La 3+ / Fe 3+ sludge.
[0099] Table 5 Sludge parameters of different loaded metal oxides
[0100]
[0101] Table 6 Heavy metal leaching content of sludge with different supported metal oxides (mg·L -1 )
[0102]
[0103] The results show that after single metal loading modification, the specific surface area of ceramsite increases relative to that of unmodified ceramsite, and the specific surface area of bimetallic modified ceramsite is larger than that of single metal modified ceramsite, indicating that the more types or quantities of loaded metals, the more obvious the effect on the increase of ceramsite surface area.
[0104] Under the conditions of certain material ratio and primary calcination temperature, the leaching toxicity of zinc and chromium in the modified sludge powder (Comparative Example 4) exceeded the standard, while the leaching toxicity of heavy metals in the calcined ceramsite was greatly reduced. This may be because zinc and copper are more distributed in silicate minerals after calcination and can be well dissolved in ceramsite. Other volatile elements such as cadmium generate gaseous products during the calcination process and volatilize or convert into other insoluble salts. This shows that after calcination, the ceramsite allows heavy metals to migrate into the flue gas or solidify in the glass phase and lattice, which is harmless and stable.
[0105] Only sludge powder materials modified with metal oxides are used. Although the specific surface area of the powder material is larger, it is not conducive to recycling in actual production applications and is prone to secondary pollution such as sludge. When it is filled in the device for use, it is also prone to blockage, requiring frequent replacement and maintenance, and other problems.
[0106] Example 5
[0107] The supported bimetallic oxide sludge-based mesoporous ceramsite prepared in Example 1 and Example 2 was used to statically remove COD and total phosphorus from a pharmaceutical wastewater, wherein the pH of the pharmaceutical wastewater was 6.35±0.05, the COD concentration was 438 mg / L, and the total phosphorus concentration was 22 mg / L. The specific method is as follows:
[0108] (1) Construct a photochemical reaction device, such as Figure 5 The magnetic stirrer 1 shown is provided with a reactor 7 on the upper part, a cooling water inlet 6 is provided on the lower part of one side of the reactor 7, and a cooling water outlet 3 is provided on the upper part of the other side; a tungsten filament lamp 2 and a thermometer 4 are fixed inside the reactor 7;
[0109] (2) Take 50 mL of pharmaceutical wastewater and place it in reactor 7 in the photochemical reaction device. Perform magnetic stirring at the same time. Stir for 30 min in a dark environment at a speed of 100 r / min.
[0110] (3) Add 1 g / L potassium peroxymonosulfonate and turn on tungsten lamp 2 as the starting point of the reaction. Take 1 mL of supernatant sample at 10, 20, 40, 60, 120, 240, and 480 min in sequence.
[0111] (4) The supernatant prepared in step (2) was filtered through a 0.45 µm filter membrane, and then the COD concentration was determined by referring to the National Standard of the People's Republic of China (GB11914-89) "Determination of COD in Water Quality - Potassium Dichromate Method"; the total phosphorus concentration was determined by referring to the National Standard of the People's Republic of China (GB11893-89) "Determination of Total Phosphorus in Water Quality - Ammonium Molybdate Spectrophotometry". The principle of removing COD and total phosphorus from the loaded bimetallic oxide sludge-based mesoporous ceramsite is as follows: Figure 6 The results are shown in Table 7:
[0112] Table 7 Effect of loaded bimetallic oxide sludge-based mesoporous ceramsite on static treatment of pharmaceutical wastewater
[0113]
[0114] The results show that after the sludge ceramsite is modified with lanthanum / iron metal oxide, the removal capacity of COD and total phosphorus is significantly improved (Examples 1-4). The main reason is that the lanthanum / iron metal oxide on the surface of the sludge ceramsite plays an important adsorption role in the reaction, provides reaction active sites, and improves the catalytic performance and adsorption capacity of the ceramsite. On the one hand, lanthanum stimulates the activity of iron oxide, prompting the potassium peroxymonosulfonate solution to catalytically degrade organic pollutants. On the other hand, lanthanum metal oxide itself has strong adsorption capacity, providing abundant adsorption active sites for phosphorus removal of ceramsite, and has outstanding adsorption performance for total phosphorus pollutants. Unmodified (Comparative Example 1) or single metal oxide loaded sludge ceramsite (Comparative Examples 2 and 3) cannot achieve the synergistic removal function of COD and total phosphorus. It is proved that the ceramsite loaded with bimetallic has high catalytic degradation ability for macromolecular organic pollutants and affinity for total phosphorus pollutants, and can effectively degrade organic pollutants in pharmaceutical wastewater and effectively enrich total phosphorus pollutants.
[0115] like Figure 7 As shown, with the extension of time, the removal rate of COD and total phosphorus by the loaded bimetallic oxide sludge-based mesoporous ceramsite prepared in Example 1 showed a gradually increasing trend.
[0116] Example 6
[0117] The supported bimetallic oxide sludge-based mesoporous ceramsite prepared in Example 3 and Example 4 was used to statically remove COD and total phosphorus from a pharmaceutical wastewater, wherein the pH of the pharmaceutical wastewater was 6.35±0.05, the COD concentration was 438 mg / L, and the total phosphorus concentration was 22 mg / L. The specific method is as follows:
[0118] (1) Construct Figure 8 The fluidized reaction device shown in the figure has a reaction column 7 with a height of 25 cm and an inner diameter of 6 cm. A top layer of quartz wool 9 is arranged at the upper end of the reaction column 7, and a bottom layer of quartz wool 6 is arranged at the lower layer to prevent the loss of filling materials; a sedimentation bin 5 is arranged below the bottom layer of quartz wool 6, and the sedimentation bin 5 is connected to the water inlet pipe 1 and the drug inlet pipe 2, and a water inlet peristaltic pump 3 is arranged on the water inlet pipe 1, and a drug inlet peristaltic pump 4 is arranged on the drug inlet pipe 2; a clean water bin 10 is arranged above the top layer of quartz wool 9, and the clean water in the clean water bin 10 is discharged through the outlet pipe 11; the reaction column 7 contains an adsorption layer 8, which is specifically the prepared loaded bimetallic oxide sludge-based mesoporous ceramsite;
[0119] (2) Fill the reaction column 7 with 400 g of loaded bimetallic oxide sludge-based mesoporous ceramsite, then let the pharmaceutical wastewater enter through the water inlet pipe 1, and set the peristaltic pump 3 at an inlet flow rate of 1 mL / min; potassium peroxymonosulfonate solution (1 g / L) passes through the drug inlet pipe 2, and set the peristaltic pump 4 at an inlet flow rate of 0.2 mL / min; inject from the water inlet at the lower end of the reaction column 7, and sample at the water outlet 11;
[0120] (3) The residual COD and total phosphorus concentrations of the samples were measured. The sample solution was filtered using a 0.45 µm filter membrane. The COD concentration was measured in accordance with the National Standard of the People's Republic of China (GB11914-89) "Determination of COD in Water - Potassium Dichromate Method"; the total phosphorus concentration was measured in accordance with the National Standard of the People's Republic of China (GB11893-89) "Determination of Total Phosphorus in Water - Ammonium Molybdate Spectrophotometric Method". The results are shown in Table 8:
[0121] Table 8 Effect of loaded bimetallic oxide sludge-based mesoporous ceramsite on dynamic treatment of pharmaceutical wastewater
[0122]
[0123] The results show that during dynamic treatment, the ceramsite prepared in Examples 1-4 still maintains a high level of removal capacity for COD and total phosphorus, and still has good selectivity and adsorption. After treatment, the ceramsite wear rate and acid solubility rate slightly decrease, proving that the ceramsite has good stability under the action of water flow. The treatment capacity of the unmodified ceramsite prepared in Comparative Example 1 and the single metal-modified ceramsite prepared in Comparative Examples 2-3 also decreases, proving that the loaded bimetallic oxide sludge-based mesoporous ceramsite has excellent wastewater treatment capacity.
Claims
1. A method for preparing supported bimetallic oxide sludge-based mesoporous ceramsite, characterized in that: The following steps are involved: (1) Sludge pretreatment: The sludge is dried in a natural state until the moisture content is less than 10%, then ground, dried and sieved to obtain sludge powder; (2) Preparation of ceramsite raw material: at room temperature, the sludge powder obtained in step (1) is mixed with fly ash and montmorillonite powder, and then granulated and sieved to obtain wet granules, which are then dried to obtain ceramsite raw material; (3) First-stage sintering: sintering the ceramsite raw material obtained in step (2) and obtaining a ceramsite masterbatch after cooling; (4) Bimetallic gradient loading: Weigh the ceramsite masterbatch obtained in step (3) and mix it with the modified solution in proportion, soak it for a period of time and then let it stand for 8-48 hours. After solid-liquid separation, wash it repeatedly with water until the pH of the filtrate is neutral. Then, dry the solid matter in an oven at 105°C to obtain the loaded La 3+ / Fe 3+ Sludge ceramsite; (5) Second stage sintering: The obtained loaded La 3+ / Fe 3+ The sludge ceramsite is sintered and cooled to obtain the loaded bimetallic oxide sludge-based mesoporous ceramsite; The mass ratio of the sludge powder to the fly ash and montmorillonite powder in step (2) is 40-80:5-30:5-25; The modified solution in step (4) is Fe(NO3)3 solution and La(NO3)3 solution, and the mass ratio of ceramsite masterbatch to modified solution is 1:(2-10); the immersion conditions are immersion at 25°C and 200 rpm / min for 1-8 h; The concentration of the Fe(NO3)3 solution is 0.050-0.150 mol / L, and the concentration of the La(NO3)3 solution is 0.025-0.100 mol / L; the concentration ratio of the Fe(NO3)3 solution to the La(NO3)3 solution is (1-3):1; and the volume ratio is 1:
1.
2. The preparation method according to claim 1, characterized in that: The sludge in step (1) is sludge from a sewage treatment plant with a water content of 40-85%; the particle size of the sludge powder is 100-200 mesh.
3. The preparation method according to claim 1, characterized in that: The particle sizes of the fly ash and montmorillonite powder in step (2) are both 200-250 mesh; the particle size of the ceramsite raw material is 4-6 mm.
4. The preparation method according to claim 1, characterized in that: The sintering conditions in step (3) are to first heat the material to 200-400°C at a rate of 8-15°C / min, preheat the material for 0.25-3 h, then heat the material to 750-1250°C at a rate of 5-10°C / min, and sinter the material at this temperature for 0.5-2 h.
5. The preparation method according to claim 1, characterized in that: The sintering conditions in step (5) are preheating at 150°C for 30 min, then heating to 300-600°C and sintering for 0.25-2 h.
6. A supported bimetallic oxide sludge-based mesoporous ceramsite prepared by the preparation method according to any one of claims 1 to 5.
7. Use of the supported bimetallic oxide sludge-based mesoporous ceramsite as claimed in claim 6 in pharmaceutical wastewater.
8. The use according to claim 7, characterized in that: The pharmaceutical wastewater is phosphorus-containing pharmaceutical wastewater, wherein the COD concentration is 50-500 mg / L and the total phosphorus concentration is 10-50 mg / L.
Citation Information
Patent Citations
Preparation method of sludge-furnace slag haydite
CN105732076A
Preparation method of waterworks sludge-base porous ceramsite doped with bamboo powder
CN106673699A
Lanthanum-iron modified zeolite phosphorus removal adsorbent and preparation method and application thereof
CN109847691A
Preparation method and application of mesoporous lanthanum modified mineral-based efficient phosphorus removal ceramsite
CN115739017A