A method for preparing actinide metals from actinide oxides
Actinide borides are prepared by a mixed reduction reaction of actinide oxides and boron sources, followed by molten salt electrolysis. This method solves the problems of high equipment requirements, high cost, and low purity in the preparation of actinide metals in existing technologies, and achieves efficient and environmentally friendly preparation of actinide metals.
Patent Information
- Application Number
- CN202311100556.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-08-29
- Publication Date
- 2026-11-17
- Estimated Expiration
- 2043-08-29
AI Technical Summary
Existing technologies for preparing actinide metals from actinide oxides suffer from problems such as high equipment requirements, high costs, poor environmental performance, and low product purity, especially the hazardous use of hydrogen fluoride gas and the high cost of platinum anode materials.
Actinide borides were prepared by a mixed reduction reaction of actinide oxides and boron sources. Then, the actinide borides were used as anodes for molten salt electrolysis. Actinide metals were prepared by combining high-temperature borothermal reduction and molten salt electrolysis.
The preparation of high-purity actinide metals has been achieved. The process is simple, environmentally friendly, and low-cost, making it suitable for batch and continuous production, and improving the safety and operability of production.
Smart Images

Figure CN117265598B_ABST
Abstract
Description
Technical Field
[0001] This invention belongs to the field of chemical metallurgy technology, and in particular relates to a method for preparing actinide metals from actinide oxides. Background Technology
[0002] Actinide metals are not only important energy materials but also crucial for maintaining national defense security. However, due to their highly reactive chemical properties and strong affinity for oxygen, they are difficult to convert from actinide oxides. Internationally, the common method for industrial production of metallic uranium and plutonium is the metallothermal reduction of uranium tetrafluoride and plutonium using magnesium, calcium, and other metals. However, actinide fluorides are produced by hydrofluorinating actinide oxides with hydrogen fluoride gas in a continuous flow reaction bed. Hydrogen fluoride gas is an extremely dangerous chemical reagent, requiring highly sophisticated reaction equipment and facilities, severely limiting the application of this technology.
[0003] In recent years, with the rapid development of dry reprocessing technology for spent fuel, researchers from various countries have conducted research on the direct dry processing of uranium and plutonium oxides. The dry processing techniques for preparing metals from uranium and plutonium oxides mainly include two routes: metallothermic reduction and molten salt electrochemical reduction. Metallothermic reduction uses reactive metals such as lithium and calcium to remove oxygen, resulting in metallic uranium and plutonium. However, this technology generates large amounts of waste salt, which becomes difficult-to-manage radioactive waste. Molten salt electrochemical reduction uses uranium oxide or plutonium oxide as the cathode and platinum or similar materials as the anode, performing electrolytic reduction in high-temperature alkali metal or alkaline earth metal molten salts to obtain metallic uranium and plutonium. However, this technology suffers from critical problems such as the high cost of platinum anode materials and low uranium and plutonium reduction rates.
[0004] Therefore, existing techniques for preparing actinide metals from actinide oxides need further improvement and development. Summary of the Invention
[0005] This invention addresses the shortcomings of existing technologies by providing a method for preparing actinide metals from actinide oxides. The method involves a reduction reaction of actinide oxides and a boron source to obtain actinide borides, which are then used as the anode in a molten salt electrolysis reaction. This method is simple, stable, requires minimal equipment, is low-cost, environmentally friendly, and can produce actinide metals with high purity.
[0006] Therefore, the present invention provides a method for preparing actinide metals from actinide oxides, comprising: mixing actinide oxides and a boron source to carry out a reduction reaction to obtain actinide borides, and then using the actinide borides as an anode to carry out a molten salt electrolysis reaction.
[0007] This invention prepares actinide borides with metallic conductivity by high-temperature boron thermal reduction of actinide oxides. Then, the actinide borides are used as anodes in molten salt electrolysis. During electrolysis, the boron contained in the anode actinide borides is converted into elemental boron, while the contained actinide elements enter the molten salt in the form of low-valence ions and are deposited at the cathode to obtain actinide metals.
[0008] In some embodiments of the present invention, the molar ratio of boron to actinides when the boron source and actinide oxide are mixed is not less than 2:1. This ensures sufficient boron for the formation of borides such as AnB2 and AnB4, and guarantees the volatilization of oxygen into gaseous substances. The molar ratio of actinide oxide to boron source is not limited to the above ratio, and those skilled in the art can select it according to actual needs.
[0009] In some embodiments of the present invention, the actinide oxides and boron source are further mixed with a carbon source, wherein the molar ratio of carbon to actinide elements is 0.5-5:1 when the carbon source and actinide oxides are mixed. The carbon source can be selectively added; adding carbon can be used for deoxidation, reducing the amount of boron source used and lowering costs. Simultaneously, too little or too much boron and carbon source will not achieve optimal results. Adding too little will result in incomplete oxygen removal, leaving actinide oxides in the product, while adding too much will increase costs and result in high impurity content in the actinide borides.
[0010] In some embodiments of the present invention, the average particle size of the actinide oxide, boron source, and carbon source is no greater than 10,000 nm, preferably 1-10,000 nm. Materials within this particle size range can be thoroughly mixed, thereby significantly increasing the contact area between the actinide oxide, boron source, and carbon source, promoting the reduction reaction and the formation of actinide borides. The particle sizes of the actinide oxide, boron source, and carbon source are not limited to the above ranges, and those skilled in the art can select them according to actual needs.
[0011] In some embodiments of the present invention, the method includes the following specific steps:
[0012] S1: Mix actinide oxides and boron sources evenly in a molar ratio, or mix actinide oxides, boron sources and carbon sources evenly in a molar ratio, and press them into blocks with a certain shape;
[0013] S2: The bulk material obtained in step S1 is subjected to a reduction reaction at 1200-1800℃ under vacuum or inert atmosphere to prepare actinide borides;
[0014] S3: Using the actinide boride obtained in step S2 as the anode and the conductive material as the cathode, a molten salt electrolysis reaction is carried out.
[0015] In some embodiments of the present invention, in step S1, the actinide oxide and boron source are mixed uniformly in a molar ratio, or the actinide oxide, boron source, and carbon source are mixed uniformly in a molar ratio and pressed into a disc-shaped block. In other embodiments, blocks of other shapes can also be pressed. The mixture of actinide oxide, boron source, and carbon source is pressed into a mixed agglomerate with a certain strength, ensuring sufficient contact between the actinide oxide, boron source, and carbon source for smooth subsequent reduction reactions. The pressing conditions are not particularly limited, and those skilled in the art can select them according to actual needs. According to the present invention, the pressing pressure is 10-300 MPa. The mixed agglomerate obtained by pressing under this pressure range has good strength and can meet the requirements of subsequent processes.
[0016] In some embodiments of the present invention, the actinide elements in the actinide oxide include at least one of actinium, thorium, uranium, neptunium, plutonium, americium, and curium.
[0017] In some embodiments of the present invention, the actinide oxides include at least one of AcO2, ThO2, U3O8, UO2, NpO2, PuO2, Am2O3, AmO2, Cm2O3, and CmO2.
[0018] In some embodiments of the present invention, the reduction reaction of actinide oxides and boron source may include the following reactions:
[0019] An₂O₃ + 6B → 2AnB₂ + B₂O₃;
[0020] An₂O₃ + 10B → 2AnB₄ + B₂O₃;
[0021] An₂O₃ + B₄C + 2C → 2AnB₂ + 3CO;
[0022] An₂O₃ + 2B₄C + C → 2AnB₄ + 3CO;
[0023] 3AnO2 + 16B → 3AnB4 + 2B2O3;
[0024] 7AnO2+8B4C→7AnB4+2B2O3+8CO;
[0025] 2AnO2 + B4C + C → AnB4 + 2CO;
[0026] 3An3O8 + 34B → 9AnB2 + 8B2O3;
[0027] 3An3O8 + 52B → 9AnB4 + 8B2O3;
[0028] 2An3O8+3B4C+13C→6AnB2+16CO;
[0029] An3O8 + 3B4C + 5C → 3AnB4 + 8CO.
[0030] In some embodiments of the present invention, the boron source is elemental boron and / or boron carbide.
[0031] In some embodiments of the present invention, the carbon source is at least one selected from graphite, carbon black, activated carbon, carbon powder, amorphous carbon, carbon nanotubes, and organic carbon.
[0032] In some embodiments of the present invention, in step S2, the temperature of the vacuum reduction reaction is 1200-1800℃, the vacuum degree is not greater than 100 Pa, and the reaction time is 1-6 hours; the temperature of the inert atmosphere reduction reaction is 1400-1800℃, the reaction time is 1-6 hours, and the inert atmosphere is argon or helium. The conditions for the reduction reaction are not particularly limited, and those skilled in the art can select them according to actual needs. It should be noted that: if the reaction temperature is too low, the actinides, boron, and carbon will not react chemically or the reaction will be incomplete; if the reaction temperature is too high, the reaction of the actinides, boron, and carbon will proceed fully, but this will result in demanding equipment conditions and wasted energy. A vacuum or inert atmosphere can prevent other gases from disrupting the reaction and also allow the reaction to proceed fully. A reaction time that is too long or too short will not achieve optimal results.
[0033] In some embodiments of the present invention, in step S3, the electrolysis temperature of the molten salt electrolysis reaction is 400-800℃, the cell voltage is 0.8-2.5V, and the current density is 0.01-10.00A / cm². 2 Molten salt electrolysis can be performed in DC mode, constant voltage mode, or a hybrid mode.
[0034] In some embodiments of the present invention, the molten salt electrolysis reaction of the actinide boride may include the following reaction:
[0035] Anode reaction: AnB x →An n+ +ne - +xB;
[0036] Cathode reaction: An n+ +ne - →An;
[0037] Molten salt electrolysis principle and apparatus, such as Figure 4 As shown.
[0038] In some embodiments of the present invention, in step S3, the molten salt for the molten salt electrolysis reaction is a molten salt system composed of alkali metal halides, alkaline earth metal halides, and actinide metal halides. Preferably, it is a molten salt system composed of one or more alkali metal halides, one or more alkaline earth metal halides, and one or more actinide metal halides. Adding a certain amount of actinide to the molten salt system based on alkali metal halides and alkaline earth metal halides is beneficial for increasing the current density and reducing the cell voltage during initial electrolysis. The combination of mixed molten salt systems is not particularly limited, and those skilled in the art can choose according to actual needs. In some embodiments of the present invention, the alkali metal halides, alkaline earth metal halides, and actinide metal halides are preferably alkali metal chlorides, alkaline earth metal chlorides, and actinide metal chlorides. According to the present invention, the molten salt system for the molten salt electrolysis reaction can be, but is not limited to, LiCl-KCl-AnClx or NaCl-KCl-AnClx.
[0039] In some embodiments of the present invention, the cathode conductive material includes molybdenum, tungsten, tantalum, aluminum, zinc, copper, nickel, or graphite. This allows for the deposition of actinide metals generated during electrolysis on the cathode. The selection of the cathode conductive material is not limited to the above-mentioned options; those skilled in the art can select a cathode conductive material that enables the deposition of actinide metals on the cathode according to actual needs.
[0040] In some embodiments of the present invention, after step S3 is completed, the cathode is removed from the molten salt, the adhering molten salt and cathode electrode are removed, and actinide metals are obtained.
[0041] In some embodiments of the present invention, after step S3 is completed, the following operations are specifically included: removing the cathode from the molten salt, washing the molten salt on the metal surface with deionized water or ethanol, or removing the molten salt and cathode on the metal surface by vacuum distillation, collecting actinide metals, and further smelting the collected actinide metals into metal blocks.
[0042] The beneficial effects of this invention are:
[0043] (1) The present invention provides a method for preparing actinide metals from actinide oxides. Actinide borides are prepared by mixing and reducing actinide oxides and boron sources, and then the actinide borides are used as anodes for molten salt electrolysis to prepare actinide metals. This method solves the problem of the difficulty in preparing actinide metals in a simple and efficient way. The prepared actinide metals have high purity and can meet the nuclear industry's demand for high-purity actinide metals. This method has significant progressive significance.
[0044] (2) The present invention provides a method for preparing actinide metals from actinide oxides. The high-temperature boronothermic reduction reaction process is simple, the raw materials are readily available and inexpensive, the product is single, and it has good environmental friendliness.
[0045] (3) The present invention provides a method for preparing actinide metals from actinide oxides. Actinide borides are used as anodes and molten salt electrolysis is used to prepare actinide metals. The process is simple, can be continuously electrolyzed for a long time, will not cause short circuit in the electrolytic cell, and is conducive to product recovery. It greatly improves the safety and operability of the process, has low equipment requirements, good stability, and can realize batch and continuous production. It has good application prospects and is worth promoting and applying on a large scale. Attached Figure Description
[0046] Figure 1 The image shows the XRD characterization pattern of metallic uranium prepared in Example 1.
[0047] Figure 2 The image shows the XRD characterization pattern of uranium boride prepared in Example 2.
[0048] Figure 3 This is a diagram of the metallic uranium product prepared by molten salt electrolysis in Example 2.
[0049] Figure 4 This is a schematic diagram of the molten salt electrolysis principle and apparatus of the present invention. Detailed Implementation
[0050] To make the present invention easier to understand, the present invention will be described in detail below with reference to embodiments. These embodiments are for illustrative purposes only and are not limited to the scope of application of the present invention.
[0051] Example 1
[0052] This embodiment provides a method for preparing actinide metals from actinide oxides, including the following specific steps:
[0053] S1: Uranium dioxide and boron are mixed in a molar ratio of 3:10.5 to obtain a mixture. The mixture is then pressed under a pressure of 200MPa to form a disc-shaped mixture block.
[0054] S2: The mixed block obtained in step S1 is subjected to a vacuum reduction reaction in a vacuum reactor. The reaction conditions are: reduction temperature 1800℃, vacuum degree 100Pa, reaction time 3h. After the reaction is completed, uranium boride is obtained.
[0055] S3: Using the uranium boride obtained in step S2 as the anode and the tungsten rod as the cathode, molten salt electrolysis was carried out in a LiCl-KCl-UCl3 molten salt system under inert gas protection. The electrolysis conditions were: electrolysis temperature 500℃, cell voltage 1.8V, and electrolysis time 24h.
[0056] S4: After electrolysis, the cathode product is removed, cooled, and washed with deionized water to remove the molten salt, yielding metallic uranium. The results are as follows: Figure 1As shown, the analysis results indicate that the electrodeposited material is metallic uranium with a purity of 99.9%.
[0057] Example 2
[0058] This embodiment provides a method for preparing actinide metals from actinide oxides, including the following specific steps:
[0059] S1: Uranium oxide octoxide, boron carbide and graphite powder are mixed in a molar ratio of U3O8:B4C:C = 1:3.1:5. After being mixed evenly, the mixture is pressed and shaped into a disc-shaped block under a pressure of 100 MPa.
[0060] S2: The mixed block obtained in step S1 was subjected to a vacuum reduction reaction in a vacuum reactor. The reaction conditions were: reduction temperature 1500℃, vacuum degree 10Pa, and reaction time 4h. After the reaction, uranium boride was obtained. The XRD characterization pattern of uranium boride is shown below. Figure 2 As shown.
[0061] S3: Using the uranium boride obtained in step S2 as the anode and the molybdenum rod as the cathode, molten salt electrolysis was carried out in a LiCl-KCl-UCl3 molten salt system under inert gas protection. The electrolysis conditions were: electrolysis temperature 450℃, cell voltage 1.5V, and electrolysis time 48h.
[0062] S4: After electrolysis, the cathode product is removed, cooled, and washed with deionized water to remove the molten salt, yielding metallic uranium. The obtained metallic uranium product is shown in the image below. Figure 3 As shown in the figure. Analysis results indicate that the electrodeposited material is metallic uranium with a purity of 99.9%.
[0063] Example 3
[0064] This embodiment provides a method for preparing actinide metals from actinide oxides, including the following specific steps:
[0065] S1: Thorium dioxide, boron carbide and graphite powder are mixed in a molar ratio of ThO2:B4C:C = 2:1.05:1 to obtain a mixture. The mixture is then pressed under a pressure of 50 MPa to form a disc-shaped mixed block.
[0066] S2: The mixed block obtained in step S1 is subjected to vacuum reduction reaction in a vacuum reactor. The reaction conditions are: reduction temperature 1600℃, vacuum degree 10Pa, reaction time 6h. Thorium boride is obtained after the reaction is completed.
[0067] S3: Using the thorium boride obtained in step S2 as the anode and the graphite rod as the cathode, molten salt electrolysis was carried out in a NaCl-KCl-ThCl4 molten salt system under inert gas protection. The electrolysis conditions were: electrolysis temperature 750℃, cell voltage 2.0V, and electrolysis time 24h.
[0068] S4: After electrolysis, the cathode product was removed, cooled, and washed with deionized water to remove the molten salt, yielding metallic thorium. Analysis showed that the electrodeposited product was metallic thorium with a purity of 99.9%.
[0069] It should be noted that the embodiments described above are only for explaining the present invention and do not constitute any limitation on the present invention. The present invention has been described with reference to typical embodiments, but it should be understood that the words used therein are descriptive and explanatory terms, not limiting terms. Modifications can be made to the present invention within the scope of the claims, and revisions can be made to the present invention without departing from the scope and spirit of the present invention. Although the present invention described herein relates to specific methods, materials, and embodiments, it does not mean that the present invention is limited to the specific examples disclosed herein; on the contrary, the present invention can be extended to all other methods and applications with the same function.
Claims
1. A method for preparing actinide metals from actinide oxides, characterized in that, Actinide borides are prepared by mixing actinide oxides and boron sources and carrying out a reduction reaction. Then, the actinide borides are used as anodes for molten salt electrolysis. The specific steps include the following: S1: Mix actinide oxides and boron source evenly in a molar ratio, with the molar ratio of boron to actinide elements not less than 2:1, and press into a block with a certain shape; Alternatively, actinide oxides, boron sources, and carbon sources can be mixed evenly in a molar ratio, with the molar ratio of carbon to actinide elements being 0.5-5:1, and then pressed into blocks of a certain shape. S2: The bulk material obtained in step S1 is subjected to a reduction reaction at 1200-1800℃ under vacuum or inert atmosphere to prepare actinide borides; S3: Using the actinide boride obtained in step S2 as the anode and the conductive material as the cathode, a molten salt electrolysis reaction is carried out; The actinide elements in the actinide oxides are at least one of actinium, thorium, uranium, neptunium, plutonium, americium, and curium.
2. The method according to claim 1, characterized in that, The boron source is elemental boron and / or boron carbide; And / or, the carbon source is at least one of graphite, carbon black, activated carbon, carbon powder, amorphous carbon, carbon nanotubes, and organic carbon.
3. The method according to claim 1, characterized in that, In step S2, the temperature of the vacuum reduction reaction is 1200-1800℃, the vacuum degree is not greater than 100Pa, and the reaction time is 1-6h; the temperature of the inert atmosphere reduction reaction is 1400-1800℃, the reaction time is 1-6h, and the inert atmosphere is argon or helium.
4. The method according to claim 1, characterized in that, In step S3, the electrolysis temperature of the molten salt electrolysis reaction is 400-800℃, the cell voltage is 0.8-2.5V, and the current density is 0.01-10.00A / cm². 2 .
5. The method according to claim 1, characterized in that, In step S3, the molten salt in the molten salt electrolysis reaction is a molten salt system composed of alkali metal halides, alkaline earth metal halides, and actinide metal halides. And / or, the cathode conductive material includes molybdenum, tungsten, tantalum, aluminum, zinc, copper, nickel, or graphite.
6. The method according to claim 1, characterized in that, After step S3 is completed, the cathode is removed from the molten salt, the adhering molten salt and cathode electrode are removed, and actinide metals are obtained.
Citation Information
Patent Citations
Preparation method of UCl3-containing high-purity chloride molten salt system, molten salt system and application
CN106498445A