Co2(OH)3Cl / Ni2(OH)3Cl / multilayer graphene composite material and preparation method thereof

CN117276489BActive Publication Date: 2026-11-10HANGZHOU DIANZI UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310992954.4
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-08-08
Publication Date
2026-11-10
Estimated Expiration
2043-08-08

AI Technical Summary

Technical Problem

然而,多层石墨烯表面没有含氧官能团,因而,在其表面制备复合材料具有非常大的挑战性

Benefits of technology

[0023](1)基底多层石墨烯的制备简单,成本低,不需要对多层石墨烯表面进行活化处理即能沉积Co2(OH)3Cl/Ni2(OH)3Cl。

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN117276489B_ABST
    Figure CN117276489B_ABST
Patent Text Reader

Abstract

This invention discloses a Co2(OH)3Cl / Ni2(OH)3Cl / multilayer graphene composite material and its preparation method. The composite material uses multilayer graphene as a substrate. The multilayer graphene is prepared by ultrasonication of expanded graphite, a simple process with lower preparation cost than graphene oxide. Furthermore, due to the absence of oxidation treatment, the carbon ring structure on the surface of the multilayer graphene is intact, with very few oxygen-containing functional groups, resulting in excellent electrical conductivity. Two phases, Ni2(OH)3Cl and Co2(OH)3Cl, are grown on the surface of the multilayer graphene. Ni2(OH)3Cl forms a nanosheet array, uniformly distributed nearly vertically on the surface of the multilayer graphene. Co2(OH)3Cl consists of cubic particles with a size of 100 nm to 300 nm, uniformly distributed on the surface of the multilayer graphene with a distribution density of approximately 2–3 × 10⁻⁶. 8 pcs / cm 2 The Co2(OH)3Cl cubic particles are composed of even smaller nanoparticles. The composite material prepared by the technical solution of this invention has excellent lithium storage performance and can be used as a negative electrode material for lithium-ion batteries.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of materials technology, and specifically relates to a Co2(OH)3Cl / Ni2(OH)3Cl / multilayer graphene composite material and its preparation method. The material of this invention has potential applications in lithium-ion battery anodes. Background Technology

[0002] The application of lithium-ion batteries is becoming increasingly widespread, especially in power batteries. Currently, commercially available graphite is a commonly used anode material for lithium-ion batteries, but its specific capacity is only 372 mAh / g. Therefore, there is a need to develop a lithium-ion battery anode material with higher capacity. Lithium storage performance based on the redox reaction of transition metal ions can achieve a larger specific capacity. However, the various compounds of transition metal ions used in lithium-ion battery electrodes have poor conductivity. Therefore, the preparation of nanoscale active materials and their composite with carbon materials is currently a hot research topic.

[0003] Currently, the preparation processes for multilayered composite materials are quite complex, with some even employing two-step methods to prepare multiphase composites. Meanwhile, the main metal compounds used are oxides, hydroxides, and sulfides. Hydroxychlorides possess excellent crystal structures, and the presence of chloride ions can improve structural stability and the material's electrical conductivity. Although there has been some research on hydroxychlorides, research on the preparation of hydroxychloride nanomaterials and composites with carbon materials is limited, especially on multiphase composites.

[0004] Multilayer graphene is prepared by ultrasonication of expanded graphite. The preparation process is simple, low-cost, and exhibits good electrical conductivity. However, the surface of multilayer graphene lacks oxygen-containing functional groups, making the preparation of composite materials on its surface extremely challenging. No reports have yet been found regarding the preparation of hydroxyl chlorides and bimetallic hydroxyl chlorides on the surface of multilayer graphene.

[0005] In view of the deficiencies of the existing technology, the present invention proposes a technical solution to solve the technical problems existing in the existing technology. Summary of the Invention

[0006] To address the problems existing in the background technology, this invention uses multilayer graphene as a carbon substrate to directly prepare two hydroxychlorides, Co2(OH)3Cl and Ni2(OH)3Cl, on the surface of multilayer graphene. This composite material has excellent electrochemical performance and can be used as a negative electrode material for lithium-ion batteries.

[0007] To address the technical problems existing in the prior art, the technical solution of the present invention is as follows:

[0008] This invention discloses a Co2(OH)3Cl / Ni2(OH)3Cl / multilayer graphene composite material, wherein the multilayer graphene is obtained by ultrasonication of expanded graphite in a mixed organic solvent. This mechanically exfoliated multilayer graphene exhibits a complete carbon ring structure on its surface, fewer than 100 graphite layers, and very few oxygen-containing functional groups, resulting in excellent electrical conductivity. The Ni2(OH)3Cl is amorphous and uniformly distributed on the surface of the multilayer graphene in a nanosheet array structure.

[0009] Co2(OH)3Cl particles are cubic with side lengths of approximately 100 nm to 300 nm, and are also distributed on the surface of multilayer graphene with a distribution density of approximately 2 to 3 × 10⁻⁶. 8 pcs / cm 2 The Co2(OH)3Cl cube is composed of well-crystallized, smaller nanoparticles.

[0010] This invention also discloses a method for preparing a Ni2(OH)3Cl nanosheet and multilayer graphene composite material, comprising the following steps:

[0011] Step S10: Measure DMF and deionized water in a volume ratio of 8:2, mix them evenly and use them as a mixed solvent. Weigh out expanded graphite and add it to the mixed solvent. Perform ultrasonic treatment at 200W power for 4 hours to obtain a multilayer graphene dispersion. The concentration of expanded graphite relative to the mixed solvent is 0.5-2 mg / mL.

[0012] Step S20: Weigh nickel chloride hexahydrate, cobalt chloride hexahydrate, and EDTA-2Na and add them to the multilayer graphene solution. Place the magnetic rotor into a glass bottle and stir for 15 minutes at room temperature. The concentration of nickel chloride hexahydrate relative to the mixed solvent is 10-14 mg / mL, the molar number of cobalt chloride hexahydrate is equal to that of nickel chloride hexahydrate, and the concentration of EDTA-2Na relative to the mixed solvent is 1.0-2.5 mg / mL.

[0013] Step S30: Add ammonia water and place it in a water bath at 80-95℃ with magnetic stirring for 5 hours; the volume ratio of ammonia water to the mixed solvent is 0.01-0.025:1.

[0014] In step S40, after cooling the reaction solution, it was washed three times with deionized water and three times with alcohol by centrifugation at a speed of 6000 rpm. After washing, it was placed in an oven at 70°C for 24 hours to dry. After drying, a Co2(OH)3Cl / Ni2(OH)3Cl / multilayer graphene composite material was obtained.

[0015] As a further improvement, multilayer graphene surfaces lack active groups, and Co2(OH)3Cl and Ni2(OH)3Cl are deposited through molecular forces on the surface of multilayer graphene. This differs from the method used in graphene oxide (GO) surfaces, where composite materials are prepared through electrostatic adsorption of oxygen-containing functional groups on the surface to produce metal compounds.

[0016] As a further improvement, the molar ratio of cobalt to nickel is 1:1. Under this molar ratio, the cobalt and nickel ions can interact with EDTA-2Na and ammonia to obtain the composite material.

[0017] As a further improvement, EDTA-2Na exhibits different complexation effects with nickel and cobalt ions, resulting in different morphologies. Strong complexation with nickel ions leads to interconnected complexes, allowing Ni₂(OH)₃Cl to grow into nanosheets that are nearly perpendicular to the multilayer graphene substrate and continuously distributed. Weak complexation with cobalt ions prevents the formation of interconnected sheets, resulting in Co₂(OH)₃Cl growing into nanoparticles that stack into cubic particles.

[0018] As a further improvement, Co2(OH)3Cl and Ni2(OH)3Cl are directly grown on the surface of multilayer graphene and connected to the multilayer graphene through molecular forces. The electron clouds of the carbon atoms in the multilayer graphene and the Co2(OH)3Cl particles and Ni2(OH)3Cl sheets overlap, resulting in low resistance and fast electron movement between them.

[0019] As a further improvement, the larger Co2(OH)3Cl particles increase the gaps between the composite sheets, making it easier for the electrolyte to come into contact with the active material.

[0020] As a further improvement, a multi-layered nanostructure composed of Co2(OH)3Cl, Ni2(OH)3Cl and multilayer graphene improves the capacity, rate performance and cycle performance of the composite material through a synergistic effect.

[0021] As a further improvement, composite materials can be used as anode materials for lithium-ion batteries, exhibiting high capacity density and excellent cycle performance.

[0022] Compared with the prior art, the present invention has the following beneficial effects:

[0023] (1) The preparation of multilayer graphene substrate is simple and low cost. Co2(OH)3Cl / Ni2(OH)3Cl can be deposited without the need for activation treatment of the multilayer graphene surface.

[0024] (2) Co2(OH)3Cl / Ni2(OH)3Cl is connected to the multilayer graphene through molecular forces. The electron clouds of the carbon atoms in the multilayer graphene and Co2(OH)3Cl / Ni2(OH)3Cl overlap, resulting in low resistance and fast movement of electrons between them.

[0025] (3) Ni2(OH)3Cl is in nanosheet form, exhibiting minimal volume change during lithium-ion charge-discharge processes. This improves its structural stability during charge-discharge, thereby enhancing its stability as a lithium-ion battery anode material. Co2(OH)3Cl cubic particles are composed of even smaller nanoparticles. Similarly, they exhibit minimal volume change during lithium-ion charge-discharge processes. The larger size of the Co2(OH)3Cl cubic particles facilitates the entry of particles into the electrolyte. The synergy between these two materials further improves performance.

[0026] (5) The multi-level nanostructured composite material of the present invention is prepared by a one-step method, which has high preparation efficiency.

[0027] (6) The present invention uses a low preparation temperature and does not require the high-pressure equipment required for hydrothermal methods. Therefore, the preparation cost is low. It is suitable for large-scale industrial production. Attached Figure Description

[0028] Figure 1 This is a flowchart illustrating the preparation steps of the Co2(OH)3Cl / Ni2(OH)3Cl / multilayer graphene composite material of the present invention;

[0029] Figure 2 The XRD pattern of the Co2(OH)3Cl / Ni2(OH)3Cl / multilayer graphene composite material prepared in Example 1 of this invention;

[0030] Figure 3 This is a low-magnification scanning electron microscope image of the Co2(OH)3Cl / Ni2(OH)3Cl / multilayer graphene composite material prepared in Example 1 of the present invention;

[0031] Figure 4 This is a high-magnification scanning electron microscope image of the Co2(OH)3Cl / Ni2(OH)3Cl / multilayer graphene composite material prepared in Example 1 of this invention;

[0032] Figure 5 Rate curve of the negative electrode of the Co2(OH)3Cl / Ni2(OH)3Cl / multilayer graphene composite lithium-ion battery prepared in Example 1 of the present invention;

[0033] Figure 6The cycling curve of the Co2(OH)3Cl / Ni2(OH)3Cl / multilayer graphene composite lithium-ion battery anode prepared in Example 1 of the present invention at a charge-discharge current density of 100 mA / g; Detailed Implementation

[0034] To better illustrate the process and solution of the present invention, the following description is provided in conjunction with the accompanying drawings and embodiments. The specific embodiments described herein are merely illustrative of the invention and are not intended to limit the invention.

[0035] To address the technical problems existing in the current technology, see [link to relevant documentation]. Figure 1 The diagram shows a flowchart of the preparation method for uniformly distributing sheet-like nano-iron oxide particles on multilayer graphene, as proposed in this invention, including the following steps:

[0036] Step S10: Measure DMF and deionized water in a volume ratio of 8:2, mix them evenly and use them as a mixed solvent. Weigh out expanded graphite and add it to the mixed solvent. Perform ultrasonic treatment at 200W power for 4 hours to obtain a multilayer graphene dispersion. The concentration of expanded graphite relative to the mixed solvent is 0.5-2 mg / mL.

[0037] Step S20: Weigh nickel chloride hexahydrate, cobalt chloride hexahydrate, and EDTA-2Na and add them to the multilayer graphene solution. Place the magnetic rotor into a glass bottle and stir for 15 minutes at room temperature. The concentration of nickel chloride hexahydrate relative to the mixed solvent is 10-14 mg / mL, the molar number of cobalt chloride hexahydrate is equal to that of nickel chloride hexahydrate, and the concentration of EDTA-2Na relative to the mixed solvent is 1.0-2.5 mg / mL.

[0038] Step S30: Add ammonia water and place it in a water bath at 80-95℃ with magnetic stirring for 5 hours; the volume ratio of ammonia water to the mixed solvent is 0.01-0.025:1.

[0039] In step S40, after cooling the reaction solution, it was washed three times with deionized water and three times with alcohol by centrifugation at a speed of 6000 rpm. After washing, it was placed in an oven at 70°C for 24 hours to dry. After drying, a Co2(OH)3Cl / Ni2(OH)3Cl / multilayer graphene composite material was obtained.

[0040] Example 1:

[0041] DMF and deionized water in a volume ratio of 8:2 were measured and mixed thoroughly to form a mixed solvent. 20 mg of expanded graphite was weighed and added to the mixed solvent, and the mixture was ultrasonically treated at 200 W for 4 hours to obtain a multilayer graphene dispersion. 119 mg of nickel chloride hexahydrate, 119 mg of cobalt chloride hexahydrate, and 15 mg of EDTA-2Na were weighed and added to the multilayer graphene solution. A magnetic rotor was added to a glass bottle, and the mixture was stirred at room temperature for 15 minutes. 200 μL of ammonia water was added, and the mixture was placed in a 90℃ water bath and magnetically stirred for 5 hours. After cooling, the reaction solution was washed three times with deionized water and three times with alcohol by centrifugation at 6000 rpm. After washing, the solution was placed in an oven at 70℃ and dried for 24 hours. The resulting Co2(OH)3Cl / Ni2(OH)3Cl / multilayer graphene composite material was obtained.

[0042] The XRD pattern of the Co2(OH)3Cl / Ni2(OH)3Cl / multilayer graphene composite material synthesized in this example is shown below. Figure 2 As shown. The diffraction peaks at 16.4°, 32.2°, and 39.4° belong to the (101), (113), and (024) diffraction peaks of the Co2(OH)3Cl phase. Ni2(OH)3Cl was not observed in the XRD pattern, indicating that Ni2(OH)3Cl has low crystallinity. Low-magnification and high-magnification scanning electron microscope images of the composite material are shown below. Figure 3 and 4 As shown, the nanosheet array observed on the surface of the multilayer graphene is Ni₂(OH)₃Cl, uniformly distributed in a near-vertical manner on the surface of the multilayer graphene. The cubic structures observed on the surface of the multilayer graphene are Co₂(OH)₃Cl. Their side lengths are approximately 100 nm to 300 nm, and their distribution density is approximately 2 to 3 × 10⁻⁶. 8 pcs / cm 2 The Co2(OH)3Cl cube is composed of even smaller nanoparticles.

[0043] The composite material, acetylene black, and PVDF binder (in a mass ratio of 8:1:1) were weighed and stirred evenly with NMP as solvent to obtain a slurry of suitable viscosity. The slurry was coated onto the surface of a copper sheet and dried in a vacuum oven at 100℃ for 12 hours. After removal, it was pressed into a tablet using a tablet press at a pressure of 10 MPa. The resulting composite electrode sheet was then used as the working electrode. The prepared electrode sheet, the separator, lithium hexafluorophosphate (LiPF6) dissolved in a 1:1 weight mixture of ethyl carbonate (EC) and dimethyl carbonate (DMC) as the electrolyte, and a lithium metal sheet as the counter electrode and reference electrode were assembled into a button cell for testing. Figure 5The results show the rate performance test results of the composite material electrode. As can be seen from the figure, the average discharge specific capacity at charge / discharge current densities of 100, 200, 500, 1000, and 2000 mA / g are 828.6, 784.4, 693.1, 583.9, and 401.5 mAh / g, respectively. When the charge / discharge current returns to 100 mA / g, the capacity recovers to 848.5 mA / g. Figure 6 These are the cycle performance test results for the composite electrode. At a charge / discharge current density of 100 mA / g, the initial discharge specific capacity is 1234.3 mAh / g, and the discharge specific capacity after 100 cycles is 913.5 mAh / g. This composite material exhibits excellent rate capability and cycle performance.

[0044] Example 2:

[0045] DMF and deionized water in a volume ratio of 8:2 were measured and mixed thoroughly to form a mixed solvent. 5 mg of expanded graphite was weighed and added to the mixed solvent, and the mixture was ultrasonically treated at 200 W for 4 hours to obtain a multilayer graphene dispersion. 100 mg of nickel chloride hexahydrate, 100 mg of cobalt chloride hexahydrate, and 10 mg of EDTA-2Na were weighed and added to the multilayer graphene solution. A magnetic rotor was added to a glass bottle, and the mixture was stirred at room temperature for 15 minutes. 100 μL of ammonia water was added, and the mixture was placed in an 80℃ water bath and magnetically stirred for 5 hours. After cooling, the reaction solution was washed three times with deionized water and three times with alcohol by centrifugation at 6000 rpm. After washing, the solution was placed in an oven at 70℃ and dried for 24 hours. The resulting Co2(OH)3Cl / Ni2(OH)3Cl / multilayer graphene composite material was obtained.

[0046] Example 3:

[0047] DMF and deionized water in a volume ratio of 8:2 were measured and mixed thoroughly to form a mixed solvent. 10 mg of expanded graphite was weighed and added to the mixed solvent, and the mixture was ultrasonically treated at 200 W for 4 hours to obtain a multilayer graphene dispersion. 140 mg of nickel chloride hexahydrate, 140 mg of cobalt chloride hexahydrate, and 25 mg of EDTA-2Na were weighed and added to the multilayer graphene solution. A magnetic rotor was added to a glass bottle, and the mixture was stirred at room temperature for 15 minutes. 250 μL of ammonia water was added, and the mixture was placed in a 95℃ water bath and magnetically stirred for 5 hours. After cooling, the reaction solution was washed three times with deionized water and three times with alcohol by centrifugation at 6000 rpm. After washing, the solution was placed in an oven at 70℃ for 24 hours to dry. The resulting product was a Co2(OH)3Cl / Ni2(OH)3Cl / multilayer graphene composite material.

[0048] Example 4:

[0049] DMF and deionized water in a volume ratio of 8:2 were measured and mixed thoroughly to form a mixed solvent. 20 mg of expanded graphite was weighed and added to the mixed solvent, and the mixture was ultrasonically treated at 200 W for 4 hours to obtain a multilayer graphene dispersion. 130 mg of nickel chloride hexahydrate, 130 mg of cobalt chloride hexahydrate, and 17 mg of EDTA-2Na were weighed and added to the multilayer graphene solution. A magnetic rotor was added to a glass bottle, and the mixture was stirred at room temperature for 15 minutes. 220 μL of ammonia water was added, and the mixture was placed in a 90℃ water bath and magnetically stirred for 5 hours. After cooling, the reaction solution was washed three times with deionized water and three times with alcohol by centrifugation at 6000 rpm. After washing, the solution was placed in an oven at 70℃ and dried for 24 hours. The resulting Co2(OH)3Cl / Ni2(OH)3Cl / multilayer graphene composite material was obtained.

[0050] The above description of the disclosed embodiments enables those skilled in the art to make or use the invention. Various modifications to these embodiments will be readily apparent to those skilled in the art, and the general principles defined herein may be implemented in other embodiments without departing from the spirit or scope of the invention. Therefore, the invention is not to be limited to the embodiments shown herein, but is to be accorded the widest scope consistent with the principles and novel features disclosed herein.

Claims

1. A method for preparing a Co2(OH)3Cl / Ni2(OH)3Cl / multilayer graphene composite material, characterized in that, Includes the following steps: Step S10: Measure DMF and deionized water in a volume ratio of 8:2, mix them evenly and use them as a mixed solvent. Weigh out expanded graphite and add it to the mixed solvent. Perform ultrasonic treatment at 200W power for 4 hours to obtain a multilayer graphene dispersion. The concentration of expanded graphite relative to the mixed solvent is 0.5~2mg / mL. Step S20: Weigh nickel chloride hexahydrate, cobalt chloride hexahydrate, and EDTA-2Na and add them to the multilayer graphene solution. Add the magnetic rotor to the glass bottle and stir for 15 minutes at room temperature. The concentration of nickel chloride hexahydrate relative to the mixed solvent is 10-14 mg / mL, the molar number of cobalt chloride hexahydrate is equal to that of nickel chloride hexahydrate, and the concentration of EDTA-2Na relative to the mixed solvent is 1.0-2.5 mg / mL. Step S30: Add 25-28 wt% ammonia water and place it in a water bath at 80-95℃ with magnetic stirring for 5 hours; the volume ratio of ammonia water to the mixed solvent is 0.01-0.025:

1. In step S40, after the reaction solution is cooled, it is washed three times with deionized water and three times with alcohol by centrifugation at a speed of 6000 rpm. After washing, it is placed in an oven at 70°C for 24 hours to dry. After drying, Co2(OH)3Cl / Ni2(OH)3Cl / multilayer graphene composite material is obtained.

2. The method for preparing the composite material according to claim 1, characterized in that, The molar ratio of cobalt to nickel is 1:

1. Under this molar ratio, cobalt ions and nickel ions interact with EDTA-2Na and ammonia to obtain the composite material.

3. The method for preparing the composite material according to claim 1, characterized in that, This composite material is used as a negative electrode material for lithium-ion batteries, exhibiting high capacity density and excellent cycle performance.

4. The Co2(OH)3Cl / Ni2(OH)3Cl / multilayer graphene composite material prepared by the method of claim 1, characterized in that, include: Multilayer graphene is obtained by ultrasonication of expanded graphite in a mixed organic solvent. The mechanically exfoliated multilayer graphene has an intact carbon ring structure on its surface, fewer than 100 graphite layers, very few oxygen-containing functional groups on its surface, and good electrical conductivity. Ni2(OH)3Cl is amorphous and is uniformly distributed on the surface of multilayer graphene in a nanosheet array structure; Co2(OH)3Cl consists of cubic particles composed of well-crystallized, smaller nanoparticles with side lengths ranging from 100 nm to 300 nm. These particles are also distributed on the surface of multilayer graphene at a density of 2–3 × 10⁻⁶. 8 pcs / cm 2 .