A heat treatment method for additively manufacturing nickel-titanium alloy and its application

By applying high-pressure solution and aging treatment in the airtight container, the problems of pores and microcracks of nickel-titanium alloy parts in additive manufacturing are solved, material densification and performance improvement are achieved, heat treatment process is simplified, and parts are improved. comprehensive mechanical properties and production efficiency.

CN117286440BActive Publication Date: 2024-11-01GUANGDONG INST OF NEW MATERIALS
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202311214641.2
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-09-19
Publication Date
2024-11-01
Estimated Expiration
2043-09-19

AI Technical Summary

Technical Problem

There are difficulties in manufacturing nickel-titanium alloy parts, especially parts with complex shapes, in traditional mechanical processing technology. Internal pores and microcracks generated during additive manufacturing affect the performance of the parts, and the existing heat treatment methods are inefficient.

Method used

Using high-pressure solution treatment and aging treatment method with heating and pressurization in a closed container, uniform isostatic pressure of 900-1200℃ is applied, and the heat and pressure are kept for more than 120 minutes. The cooling rate and air pressure are regulated, residual pores and microcracks are eliminated, and the material is realized. Densification and tissue regulation.

Benefits of technology

Effectively eliminate internal defects of nickel-titanium alloy, improve the comprehensive mechanical properties of the material, avoid pore reopening, simplify the heat treatment process, and improve the performance and production efficiency of the parts.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN117286440B_ABST
    Figure CN117286440B_ABST
Patent Text Reader

Abstract

The present invention discloses a heat treatment method for additive manufacturing of nickel-titanium alloy and its application, and relates to the technical field of heat treatment of metal materials. A heat treatment method for additive manufacturing of nickel-titanium alloy, comprising the following steps: (1) placing the nickel-titanium alloy in a closed container and heating and pressurizing it to a temperature of 900-1200°C and a pressure in the closed container of not less than 120MPa; then keeping the temperature and pressure for more than 120min, and finally cooling it to 250-500°C at a cooling rate of 100-1000°C / min; (2) keeping the nickel-titanium alloy in the closed container for 30-180min, then cooling it to room temperature and taking out the nickel-titanium alloy; the pressure of the closed container after cooling in step (1) and step (2) is ≥80MPa. The method of the present invention can not only eliminate the residual pores and microcracks generated in the additive manufacturing process, but also effectively regulate the material organization properties and improve the preparation efficiency.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of heat treatment of metal materials, and in particular to a heat treatment method for additively manufacturing nickel-titanium alloy and application thereof. Background Art

[0002] Nickel-titanium alloys have shape memory effect, superelasticity, low stiffness, biocompatibility, damping characteristics and corrosion resistance, and are widely used in aerospace and medical equipment. However, due to the activity and resilience of nickel-titanium alloys, it is difficult to manufacture nickel-titanium alloy parts, especially parts with complex shapes, using traditional machining processes.

[0003] In recent years, the rapid development of additive manufacturing technology has provided a new forming technology path for the manufacturing of complex parts. For example, nickel-titanium alloy self-expanding vascular stents, oral orthodontic wires, intervertebral fusion devices, etc. manufactured by selective laser melting technology. However, it should be pointed out that additive manufacturing of nickel-titanium alloys usually requires subsequent heat treatment, such as solution treatment to eliminate the impurities produced during the forming process in order to obtain a single-phase matrix; aging treatment to obtain the second phase precipitation in order to obtain better comprehensive mechanical properties. In addition, since internal pores and microcracks are inevitably generated during the additive manufacturing process, they ultimately affect the performance of the product. Therefore, developing a heat treatment method suitable for additive manufacturing of nickel-titanium alloy parts, while eliminating internal defects, to achieve effective regulation of the material microstructure is of great significance to improving the performance of the product and improving the preparation efficiency. Summary of the invention

[0004] The purpose of the present invention is to overcome the shortcomings of the prior art and provide a heat treatment method for additively manufactured nickel-titanium alloy and its application. The method of the present invention can not only eliminate the residual pores and microcracks generated in the additive manufacturing process, but also effectively regulate the material structure and properties and improve the preparation efficiency.

[0005] To achieve the above object, the technical solution adopted by the present invention is:

[0006] In a first aspect, the present invention provides a method for heat treatment of nickel-titanium alloy in additive manufacturing, comprising the following steps:

[0007] (1) placing the nickel-titanium alloy in a sealed container and heating and pressurizing it to a temperature of 900-1200° C. and a pressure in the sealed container of not less than 120 MPa; then maintaining the temperature and pressure for more than 120 minutes, and finally cooling it to 250-500° C. at a cooling rate of 100-1000° C. / min;

[0008] (2) The nickel-titanium alloy in the sealed container is kept at a temperature and pressure for 30-180 minutes, then cooled to room temperature and the nickel-titanium alloy is taken out; the pressure in the sealed container after the temperature is reduced in step (1) and step (2) is ≥80 MPa.

[0009] The present invention simultaneously completes the densification and heat treatment of the additively manufactured nickel-titanium alloy material in a closed container. The present invention effectively eliminates the residual internal pores and microcracks of the material during the additive manufacturing process by applying a uniform isostatic pressure of not less than 120MPa to the nickel-titanium alloy at 900-1200°C and keeping the temperature and pressure for not less than 120min. At the same time, the above-mentioned high-pressure solid solution treatment can fully dissolve the impurities generated in the additive manufacturing process into the matrix, thereby obtaining a uniform single-phase matrix structure, i.e., the NiTi phase; and by adjusting the cooling rate at the end of the solid solution treatment, the precipitation of the second phase inside the nickel-titanium alloy is regulated. In addition, the present invention further regulates the introduction and growth of the second phase in the nickel-titanium alloy by adjusting the temperature of the aging treatment and the insulation and pressure holding time. In addition, since both the solid solution treatment and the aging treatment are carried out at a pressure of not less than 80MPa, the nickel-titanium alloy can effectively avoid the reopening of pores during the heat treatment process. The present invention can not only effectively improve the comprehensive mechanical properties of the nickel-titanium alloy material, but also combine the original multi-step heat treatment, thereby improving the production efficiency of nickel-titanium alloy parts.

[0010] Preferably, the temperature after heating and pressurizing in step (1) is 1050-1200° C., and the gas pressure in the sealed container is 120-150 MPa.

[0011] More preferably, in step (1), the heating temperature is 1100° C., the gas pressure is 130 MPa, and the heat and pressure holding time is 210 min.

[0012] Preferably, the time of heat preservation and pressure preservation in step (1) is 180-240 minutes.

[0013] The present invention adopts the temperature and air pressure within the above range and the heat and pressure holding time, so that the residual internal pores and microcracks of the nickel-titanium alloy during the additive manufacturing process are better eliminated, thereby further improving the comprehensive mechanical properties of the nickel-titanium alloy.

[0014] Preferably, the temperature during heat preservation and pressure preservation in step (2) is 350-500° C., and the air pressure in the sealed container is 80-120 MPa.

[0015] Preferably, the time of heat preservation and pressure preservation in step (2) is 60-120 minutes.

[0016] More preferably, the temperature during the heat preservation and pressure preservation in step (2) is 400° C., the air pressure in the sealed container is 100 MPa, and the heat preservation and pressure preservation time is 80 min.

[0017] The present invention adopts the temperature and pressure within the above range and the heat preservation and pressure holding time, so that the pores of the nickel-titanium alloy are less likely to be reopened during the heat treatment process, which is beneficial to further improve the comprehensive mechanical properties of the nickel-titanium alloy.

[0018] Preferably, the cooling rate in step (1) is 800-1000° C. / min.

[0019] More preferably, the cooling rate in step (1) is 900° C. / min.

[0020] Preferably, the closed container is a hot isostatic pressing cylinder.

[0021] In a second aspect, the present invention provides an additively manufactured nickel-titanium alloy, wherein the additively manufactured nickel-titanium alloy is obtained by the above-mentioned thermal method.

[0022] In a third aspect, the present invention provides an application of additively manufactured nickel-titanium alloy in the fields of aerospace and biomedicine.

[0023] Compared with the prior art, the present invention has the following beneficial effects:

[0024] (1) The present invention effectively eliminates residual internal pores and microcracks in the material during the additive manufacturing process by applying a uniform isostatic pressure of not less than 120 MPa to the material at 900-1200° C. and maintaining the temperature and pressure for not less than 120 minutes.

[0025] (2) The present invention is beneficial to regulating the emergence and growth of the second phase in the nickel-titanium alloy by adjusting the temperature and the heat and pressure holding time of the aging treatment. In addition, since both the solution treatment and the aging treatment are carried out at a pressure of not less than 80 MPa, the pores of the nickel-titanium alloy material can be effectively prevented from reopening during the heat treatment process. BRIEF DESCRIPTION OF THE DRAWINGS

[0026] Figure 1 This is a scanning electron microscope image of the microstructure of the additively manufactured nickel-titanium alloy before heat treatment in Example 1 of the present invention.

[0027] Figure 2 This is a scanning electron microscope image of the microstructure of the additively manufactured nickel-titanium alloy after heat treatment in Example 1 of the present invention.

[0028] Figure 3 This is a scanning electron microscope image of the microstructure of the additively manufactured nickel-titanium alloy after heat treatment in Example 2 of the present invention. DETAILED DESCRIPTION

[0029] In order to better illustrate the purpose, technical solutions and advantages of the present invention, the present invention will be further described below in conjunction with specific embodiments, but the protection scope and implementation methods of the present invention are not limited thereto.

[0030] Unless otherwise specified, the materials and reagents used in the following examples are commercially available.

[0031] Example 1

[0032] A heat treatment method for additively manufacturing nickel-titanium alloy, comprising the following steps:

[0033] (1) High-pressure solution treatment: The nickel-titanium alloy is placed in a hot isostatic pressing cylinder. Under the initial gas pressure of 30 MPa, the temperature and pressure are increased simultaneously, and the temperature is heated to 900°C. At this time, the cylinder pressure is 120 MPa. The temperature and pressure are maintained for 120 minutes, and then the temperature is reduced to 250°C at a rate of 100°C / min without decompression.

[0034] (2) High-pressure aging treatment: The temperature is 250°C and the air pressure is 80 MPa. The temperature and pressure are kept constant for 30 minutes. Finally, the nickel-titanium alloy is taken out after being cooled to room temperature. During the high-pressure solution and high-pressure aging treatments, the nickel-titanium alloy is always placed in the hot isostatic pressing cylinder.

[0035] according to Figure 1 and Figure 2 By comparison, it can be seen that after the nickel-titanium alloy material is treated by the method of the present invention, the density of the nickel-titanium alloy is improved and the pores are basically eliminated.

[0036] Example 2

[0037] A heat treatment method for additively manufacturing nickel-titanium alloy, comprising the following steps:

[0038] (1) High-pressure solution treatment: The nickel-titanium alloy is placed in a hot isostatic pressing cylinder, and the temperature and pressure are increased at the same time under the initial gas pressure of 30 MPa, and the cylinder pressure is heated to 1200°C. At this time, the cylinder pressure is 120 MPa, and the temperature and pressure are maintained for 120 minutes, and then the temperature is reduced to 500°C at a rate of 1000°C / min without decompression;

[0039] (2) High-pressure aging treatment: The temperature is 500°C and the air pressure is 80 MPa. The temperature and pressure are maintained for 180 minutes. Finally, the nickel-titanium alloy is taken out after being cooled to room temperature. During the high-pressure solution and high-pressure aging treatments, the nickel-titanium alloy is always placed in the hot isostatic pressing cylinder.

[0040] Example 3

[0041] A heat treatment method for additively manufacturing nickel-titanium alloy, comprising the following steps:

[0042] (1) High-pressure solution treatment: The nickel-titanium alloy is placed in a hot isostatic pressing cylinder, and the temperature and pressure are increased at the same time under the initial gas pressure of 30 MPa, and the cylinder pressure is heated to 1050°C. At this time, the cylinder pressure is 120 MPa, and the temperature and pressure are maintained for 180 minutes, and then the temperature is reduced to 350°C at a rate of 1000°C / min without decompression;

[0043] (2) High-pressure aging treatment: The temperature is 350°C and the air pressure is 80 MPa. The temperature and pressure are kept for 60 minutes. Finally, the nickel-titanium alloy is taken out after being cooled to room temperature. During the high-pressure solid solution and high-pressure aging treatments, the nickel-titanium alloy is always placed in the hot isostatic pressing cylinder.

[0044] Example 4

[0045] A heat treatment method for additively manufacturing nickel-titanium alloy, comprising the following steps:

[0046] (1) High-pressure solution treatment: The nickel-titanium alloy is placed in a hot isostatic pressing cylinder. Under the initial gas pressure of 30 MPa, the temperature and pressure are increased simultaneously, and the temperature is heated to 1200°C. At this time, the cylinder pressure is 150 MPa. The temperature and pressure are maintained for 240 minutes, and then the temperature is reduced to 500°C at a rate of 1000°C / min without decompression.

[0047] (2) High-pressure aging treatment: The temperature is 500°C and the gas pressure is 120 MPa. The temperature and pressure are maintained for 120 min, and the nickel-titanium alloy is taken out after finally cooling to room temperature. During the high-pressure solid solution and high-pressure aging treatments, the nickel-titanium alloy is always placed in the hot isostatic pressing cylinder.

[0048] Example 5

[0049] A heat treatment method for additively manufacturing nickel-titanium alloy, comprising the following steps:

[0050] (1) High-pressure solution treatment: The nickel-titanium alloy is placed in a hot isostatic pressing cylinder. Under the initial gas pressure of 30 MPa, the temperature and pressure are increased simultaneously, and the temperature is heated to 1100°C. At this time, the cylinder pressure is 130 MPa. The temperature and pressure are maintained for 210 minutes, and then the temperature is reduced to 400°C at a rate of 1000°C / min without decompression.

[0051] (2) High-pressure aging treatment: The temperature is 400°C and the air pressure is 100 MPa. The temperature is kept at this temperature for 80 minutes, and the nickel-titanium alloy is taken out after finally cooling to room temperature. During the high-pressure solution and high-pressure aging treatments, the nickel-titanium alloy is always placed in the hot isostatic pressing cylinder.

[0052] Example 6

[0053] The difference from Example 1 is that in step (1), the cooling rate at the end of the solution treatment is 800°C / min, and the other steps are the same as Example 1.

[0054] Example 7

[0055] The difference from Example 1 is that in step (1), the cooling rate at the end of the solution treatment is 900°C / min, and the other steps are the same as Example 1.

[0056] Comparative Example 1

[0057] The difference from Example 1 is that in step (1), the temperature after heating and pressurizing of the solution treatment is 800°C, and the other steps are the same as Example 1.

[0058] Comparative Example 2

[0059] The difference from Example 1 is that in step (1), the temperature after heating and pressurizing of the solution treatment is 1500°C, and the other steps are the same as Example 1.

[0060] Comparative Example 3

[0061] The difference from Example 1 is that in step (1), the gas pressure of the cylinder during the solution treatment is 60 MPa, and the other steps are the same as Example 1.

[0062] Comparative Example 4

[0063] The difference from Example 1 is that in step (1), the heat preservation and pressure holding time of the solution treatment is 100 minutes, and the other steps are the same as Example 1.

[0064] Comparative Example 5

[0065] The difference from Example 1 is that in step (1), the cooling rate at the end of the solution treatment is 80°C / min, and the other steps are the same as Example 1.

[0066] Comparative Example 6

[0067] The difference from Example 1 is that in step (1), the cooling rate at the end of the solution treatment is 1200°C / min, and the other steps are the same as Example 1.

[0068] Comparative Example 7

[0069] The difference from Example 1 is that in step (2), the temperature during the heat preservation and pressure preservation during the aging treatment is 200° C., and the other steps are the same as Example 1.

[0070] Comparative Example 8

[0071] The difference from Example 1 is that in step (2), the temperature during the heat preservation and pressure preservation during the aging treatment is 600° C., and the other steps are the same as Example 1.

[0072] Comparative Example 9

[0073] The difference from Example 1 is that in step (2), the gas pressure of the cylinder during the aging treatment is 50 MPa, and the other steps are the same as Example 1.

[0074] Comparative Example 10

[0075] The difference from Example 1 is that in step (2), the heat preservation and pressure holding time of the aging treatment is 200 minutes, and the other steps are the same as Example 1.

[0076] Comparative Example 11

[0077] The difference from Example 1 is that in step (2), the heat preservation and pressure holding time of the aging treatment is 10 minutes, and the other steps are the same as Example 1.

[0078] Comparative Example 12

[0079] The difference from Example 1 is that in step (1), after keeping the temperature and pressure for 120 minutes, the mixture is naturally cooled to room temperature and the nickel-titanium alloy is taken out.

[0080] experiment

[0081] The nickel-titanium alloys after heat treatment in the above-mentioned embodiment and comparative example were subjected to performance testing using the following method:

[0082] Density: Determination method of density of dense sintered metal materials and cemented carbide GB / T 3850-2015;

[0083] Tensile strength: Tensile test of metal materials GB / T 228.1-2010;

[0084] Elongation: Tensile test of metal materials GB / T 228.1-2010.

[0085] Table 1

[0086]

[0087]

[0088] It can be seen from Table 1 that when the heating temperature, gas pressure and insulation time during solution treatment and the temperature, gas pressure and insulation time during aging treatment are not within the scope protected by this application, the performance of the nickel-titanium alloy will be affected to a certain extent. Therefore, the present invention adjusts the heating temperature, gas pressure and insulation time during solution treatment within the scope protected by this application, and at the same time controls the temperature, gas pressure and insulation time during aging treatment, which can not only effectively improve the comprehensive mechanical properties of the nickel-titanium alloy material, but also combine the original multi-step heat treatment, thereby improving the production efficiency of nickel-titanium alloy parts.

[0089] In summary, the present invention effectively eliminates the residual internal pores and microcracks of the nickel-titanium alloy material during the additive manufacturing process by applying a uniform isostatic pressure of not less than 120MPa to the nickel-titanium alloy at 900-1200°C and keeping the temperature and pressure for not less than 120 minutes. At the same time, the high-pressure solution treatment can fully dissolve the impurities produced in the additive manufacturing process into the matrix, thereby obtaining a uniform single-phase matrix structure; and by adjusting the cooling rate at the end of the solution treatment, the precipitation of the second phase inside the nickel-titanium alloy is regulated. In addition, the present invention further regulates the emergence and growth of the second phase in the nickel-titanium alloy by adjusting the temperature of the aging treatment and the insulation and pressure holding time. In addition, since both the solution treatment and the aging treatment are carried out at a pressure of not less than 80MPa, the nickel-titanium alloy material can effectively avoid the reopening of pores during the heat treatment process.

[0090] Finally, it should be noted that the above embodiments are only used to illustrate the technical solution of the present invention rather than to limit the scope of protection of the present invention. Although the present invention has been described in detail with reference to the preferred embodiments, those skilled in the art should understand that the technical solution of the present invention can be modified or replaced by equivalents without departing from the essence and scope of the technical solution of the present invention.

Claims

1. A heat treatment method for additively manufactured nickel-titanium alloy, It is characterized in that The following steps are involved: (1) placing the nickel-titanium alloy in a sealed container and heating and pressurizing it to a temperature of 1050-1200° C. and a pressure of 120-130 MPa in the sealed container; then maintaining the temperature and pressure for 180-240 minutes, and finally cooling the alloy to 250-350° C. at a cooling rate of 100-900° C. / min; (2) The nickel-titanium alloy in the sealed container is kept at a temperature and pressure of 80 MPa for 30 minutes, then cooled to room temperature and the nickel-titanium alloy is taken out.

2. The heat treatment method for additively manufacturing nickel-titanium alloy according to claim 1, It is characterized in that The closed container is a hot isostatic pressing cylinder.

3. An additively manufactured nickel-titanium alloy, It is characterized in that The nickel-titanium alloy is obtained by being treated by the heat treatment method for additively manufacturing nickel-titanium alloy according to any one of claims 1-2.

4. An application of the additively manufactured nickel-titanium alloy as claimed in claim 3 in the fields of aerospace and biomedicine.