Positive electrode plate, battery and electrical equipment
By introducing three-dimensional graphene as a compressive elasticity additive into the positive electrode sheet of a lithium-ion battery, a porous structure is constructed, which solves the problem of large volume change rate of lithium-ion batteries during charging and discharging, and improves the cycle performance and structural stability of the battery.
Patent Information
- Application Number
- CN202210703160.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-06-21
- Publication Date
- 2026-11-10
- Estimated Expiration
- 2042-06-21
AI Technical Summary
Lithium-ion batteries undergo significant volume changes during charging and discharging, leading to increased electrode polarization and electrolyte extrusion, which affects the battery's cycle performance.
Three-dimensional graphene is used as a compression elastic additive to construct a porous positive electrode sheet. The volume change of the cell is mitigated by the reversible volume change during charging and discharging, thereby reducing the volume expansion and contraction rate of the cell.
It effectively reduces the volume change rate of battery cells during charge and discharge cycles, improves the cycle performance of the battery, and enhances the structural stability and cycle life of the battery.
Smart Images

Figure CN117317224B_ABST
Abstract
Description
Technical Field
[0001] This application relates to the field of battery technology, specifically to a positive electrode, a battery, and an electrical device. Background Technology
[0002] During charging, the volume of the negative electrode in a lithium-ion battery generally increases gradually, as does the overall volume of the cell. With a fixed cell casing size, the external pressure exerted on the cell by the casing gradually increases with charging, which can lead to increased electrode polarization and electrolyte extrusion. Conversely, during discharging, the volume of the negative electrode gradually decreases, and the external pressure on the cell gradually decreases. Therefore, the cell exhibits a significant rate of volume change during charging and discharging, resulting in poor battery cycle performance. Summary of the Invention
[0003] In view of this, this application provides a positive electrode sheet, a battery, and an electrical device to reduce the volume change rate of the battery cell during cycling and improve the cycle performance of the battery.
[0004] The first aspect of this application provides a positive electrode sheet, including a positive current collector and a positive active material layer disposed on at least one side surface of the positive current collector, wherein the positive active material layer contains a compression elastic additive, wherein the compression elastic additive is three-dimensional graphene, and the three-dimensional graphene has a porous structure; wherein, after a pressure greater than 0 and less than or equal to 5 MPa is applied along the thickness direction of the positive electrode sheet, the thickness resilience and thickness compression ratio of the positive electrode sheet are each independently in the range of 2%-20%.
[0005] The positive electrode sheet mentioned above incorporates three-dimensional graphene as a compressive elasticity additive, which gives the positive electrode sheet a certain compressive elasticity. This positive electrode sheet can effectively reduce the volume change rate of the cell during charge and discharge cycles, and the effect is particularly obvious for battery systems with large negative electrode volume expansion during charging, thereby improving the cycle performance of the battery.
[0006] In some embodiments of this application, the positive electrode active material layer includes a first positive electrode coating and a second positive electrode coating stacked together, the first positive electrode coating being close to the positive electrode current collector, wherein the first positive electrode coating and / or the second positive electrode coating contains the compression additive.
[0007] In some embodiments of this application, the first positive electrode coating includes LiFe. 1-a Mn aThe PO4 active material, and the second positive electrode coating comprising a layered transition metal oxide active material and the elastic additive. Adding an elastic additive with elastic properties to the ternary material layer, which expands in volume during charging, can more significantly improve the volume change rate of the positive electrode sheet under pressure, and reduce the shrinkage of the layered transition metal oxide material layer and LiFe... 1-a Mn a The difference in volume expansion rate between the PO4 material layers prevents interlayer separation and improves the long-cycle capability of the electrode.
[0008] Secondly, this application provides a battery comprising a positive electrode as described in the first aspect of this application.
[0009] Because of the use of the aforementioned positive electrode, the battery cell exhibits smaller volume fluctuations during charging and discharging, thus improving cycle performance.
[0010] Thirdly, this application provides an electrical device having a battery as described in the second aspect of this application. Attached Figure Description
[0011] Figure 1 This is a schematic diagram of a positive electrode sheet provided in an embodiment of this application.
[0012] Figure 2 This is a schematic diagram of another structure of the positive electrode sheet provided in an embodiment of this application.
[0013] Figure 3 The images show cross-sectional scanning electron microscope (SEM) images (a) and surface electron microscope (B) images of the three-dimensional graphene used in Example 1.
[0014] Figure 4 The graph shows the cycle performance of a full cell made from the positive electrode sheet of Example 1 of this application and a full cell made from the positive electrode sheet of Comparative Example 1. Detailed Implementation
[0015] The technical solutions of the embodiments of this application will now be described in conjunction with the accompanying drawings.
[0016] See Figure 1 This application provides a positive electrode 100, including a positive current collector 10 and a positive active material layer 20 disposed on at least one side surface of the positive current collector 10. The positive active material layer 20 contains a compression elastic additive, wherein the compression elastic additive is three-dimensional graphene, and the three-dimensional graphene has a porous structure. When a pressure greater than 0 and less than or equal to 5 MPa is applied to the positive electrode 100 along the thickness direction of the positive electrode, the thickness resilience and thickness compression rate of the positive electrode 100 are each independently in the range of 2%-20%.
[0017] The pressure greater than 0 and less than or equal to 5 MPa mentioned above represents the force that the positive electrode 100 may withstand during battery charge-discharge cycles. The aforementioned thickness resilience and compression ratio data for the positive electrode 100 indicate that the positive electrode 100 has good compression resilience performance. The thickness resilience and thickness compression ratio of the positive electrode can be equal or different. In some embodiments, this pressure can be 0.1-1 MPa.
[0018] During battery charging, as Li + As the negative electrode gradually integrates, its volume increases, generally leading to an increase in the overall cell volume. This expansion is particularly pronounced in battery systems with large negative electrode expansion (such as silicon-based materials). When the cell's package dimensions are fixed (e.g., cylindrical batteries), the increasing cell volume during charging results in significant external pressure from the battery casing. This pressure is transmitted to the positive electrode, where the compressive strength additives gradually shrink, releasing some space and mitigating the overall cell volume expansion caused by the negative electrode expansion. This reduces the extent of volume expansion during charging. Conversely, during battery discharge, as the Li... + As the positive electrode is re-intercalated from the negative electrode, the negative electrode shrinks in volume, and the external pressure on the cell gradually decreases. The aforementioned elastic additive gradually rebounds, and the increased volume from this rebound compensates for the overall cell volume shrinkage caused by the negative electrode's shrinkage, thereby reducing the cell volume shrinkage rate during discharge. Therefore, the aforementioned positive electrode sheet with elasticity can effectively reduce the cell's volume change rate during charge-discharge cycles, stabilize the distance between the positive and negative electrode surfaces, and improve the battery's cycle performance.
[0019] Specifically, controlling the thickness rebound rate and thickness compression rate of the positive electrode sheet 100 to be independently within the range of 2%-20% can improve the structural stability of the positive electrode sheet, reduce the volume change rate of the cell during charge-discharge cycles, stabilize the spacing between the positive and negative electrode surfaces, and improve the cycle stability of the battery. If the thickness rebound rate and thickness compression rate of the positive electrode sheet are lower than the above range, it means that the compression additive is insufficient to effectively bond the two material layers together, and the improvement in cycle performance is not significant. If the thickness rebound rate and thickness compression rate are higher than the above range, it means that the content of the compression additive is too high or the structural stability of the compression additive is poor, the relative content of active material is low or the structural stability of the positive electrode sheet is poor, the energy density and rate performance of the battery decreases, and the cycle stability decreases.
[0020] The method for testing the rebound performance of the above-mentioned positive electrode sheet is as follows: Apply a pressure of X1 MPa to the positive electrode sheet along its thickness direction, and measure the thickness of the positive electrode sheet under the X1 MPa pressure as H1; then remove the pressure, and after the thickness of the positive electrode sheet stabilizes, measure the thickness of the positive electrode sheet again, denoted as H2. The thickness rebound rate of the positive electrode sheet is then r = (H2 - H1) / H1. The method for testing the compression performance of the above-mentioned positive electrode sheet is as follows: Apply a pressure of X2 MPa to the positive electrode sheet with an initial thickness of H3 along its thickness direction, and measure the thickness of the positive electrode sheet under the X2 MPa pressure, denoted as H4. The thickness compression rate of the positive electrode sheet is then p = (H3 - H4) / H3. Therefore, the above-mentioned "applying a pressure greater than 0 and less than or equal to 5 MPa to the positive electrode 100 along the thickness direction of the positive electrode 100, with the thickness rebound rate and thickness compression rate of the positive electrode 100 each independently within the range of 2%-20%" can be understood as applying a pressure greater than 0 and less than or equal to 5 MPa to the positive electrode 100 along the thickness direction of the positive electrode 100, measuring the thickness of the positive electrode 100 under this pressure of greater than 0 and less than or equal to 5 MPa as H1; then removing the pressure, and waiting for the thickness of the positive electrode 100 to stabilize. Next, measure the thickness of the positive electrode sheet, denoted as H2. The thickness resilience of the positive electrode sheet is r = (H2 - H1) / H1, where r is in the range of 2%-20%. Apply a pressure greater than 0 and less than or equal to 5 MPa to the positive electrode sheet with an initial thickness of H3 along the thickness direction of the positive electrode sheet, and measure the thickness of the positive electrode sheet under the pressure greater than 0 and less than or equal to 5 MPa, denoted as H4. The thickness compression ratio of the positive electrode sheet is p = (H3 - H4) / H3, where p is in the range of 2%-20%.
[0021] In this embodiment, the porous structure of three-dimensional graphene is formed by overlapping graphene sheets. The maximum pore size of this porous structure does not exceed 300 nm. The maximum pore size refers to the diameter of the largest pore in the porous structure, and "pore size" can refer to the maximum width of each pore. Since the maximum pore size does not exceed 300 nm, it can be understood that the pore size of each pore in the porous structure does not exceed 300 nm. The smaller pore size helps to ensure that the three-dimensional graphene is not prone to structural collapse after being subjected to a certain pressure, and facilitates its resilience. In some embodiments of this application, the average pore size of the porous structure is 10-200 nm, such as 15 nm, 20 nm, 25 nm, 30 nm, 40 nm, 50 nm, 60 nm, 70 nm, etc. The average pore size of the porous structure can be measured by N2 adsorption / desorption testing.
[0022] In this embodiment of the application, the fracture strength at the joint of the overlapping graphene sheets in the three-dimensional graphene is 20-50 N / m, indicating that the three-dimensional graphene has high structural stability. Even at the joint of the graphene sheets with slightly weaker strength, the mechanical strength is still relatively high. This ensures that the three-dimensional graphene is not prone to structural collapse under certain external forces, and can be repeatedly compressed and rebounded.
[0023] The parameter "fracture strength at the joint of overlapping graphene sheets" can be obtained by performing nanoindentation tests on the joint of three-dimensional graphene using atomic force microscopy (AFM). The specific testing method is as follows: Three-dimensional graphene is fixed onto a silicon wafer with small holes on its surface. A probe is used to apply pressure to the graphene sheet in the holes, with the pressure applied near the joint of two adjacent graphene sheets. The critical pressure required to cause the joint of the two graphene sheets to fracture is recorded, thus obtaining the fracture strength at the joint between the graphene sheets.
[0024] In this embodiment, the lateral dimensions of the graphene sheets constituting the three-dimensional graphene are in the nanometer range, for example, 10-100 nm, such as 10 nm, 15 nm, 18 nm, 20 nm, 25 nm, 30 nm, 40 nm, 50 nm, 60 nm, 80 nm, 90 nm, etc. Preferably, the lateral dimensions of the graphene sheets are 10 nm-30 nm, and more preferably 10 nm-20 nm. Here, the lateral dimensions refer to the length or width of the graphene sheets, which can be obtained from electron microscope images of the three-dimensional graphene. The graphene sheets can be single-layer graphene and / or multi-layer graphene. Controlling the lateral dimensions of the graphene sheets within the above range is mainly to control the pore size formed by the overlap between the graphene sheets and the pore volume of the three-dimensional graphene within a suitable range. The pore size and pore volume of the three-dimensional graphene, together with the fracture strength at the overlap of the graphene sheets, affect the compressive resilience of the three-dimensional graphene material.
[0025] In this embodiment, the average particle size of the three-dimensional graphene is 0.5 μm-20 μm. Three-dimensional graphene with an average particle size within this range is suitable for use in positive electrode sheets. This ensures, on the one hand, that the three-dimensional graphene is uniformly dispersed and distributed in the second positive electrode coating 22, and on the other hand, that it is well-matched with the positive electrode active particles. Through filling the pores between active materials and achieving uniform dispersion, the second positive electrode coating 22 possesses uniform compressive resilience performance. Specifically, the average particle size of the three-dimensional graphene is 0.6 μm, 1 μm, 5 μm, 8 μm, 10 μm, 15 μm, 20 μm, etc.
[0026] In this embodiment of the application, the pore volume of the three-dimensional graphene is 1-10 cm³. 3The pore volume is between / g. This pore volume can be measured using nitrogen adsorption on three-dimensional graphene. Three-dimensional graphene with a pore volume within this range exhibits a large number of small pores, good compressibility, and good resilience, meaning it possesses reciprocating compression-resilience.
[0027] In this embodiment, the aforementioned three-dimensional graphene can be grown using plasma chemical vapor deposition (PECVD). An exemplary preparation method includes the following steps: a mixed gas of carbon source (e.g., C2H2) and H2 is introduced into a deposition chamber heated to a certain temperature in a plasma deposition apparatus; a plasma generator is activated to deposit and grow three-dimensional graphene material on a substrate (e.g., Cu) placed in the deposition chamber via PECVD; after the growth of the three-dimensional graphene is complete, an auxiliary gas (e.g., Ar, He) is introduced to cool the deposition chamber to room temperature under an inert atmosphere; the resulting sample is then removed from the deposition chamber, and the three-dimensional graphene material is peeled off from the substrate and broken into the desired particle size. The PECVD process generates high-energy-density and large-volume plasma, which can decompose the carbon source C2H2 into numerous carbon-containing reactive radicals, thereby achieving the growth of three-dimensional graphene. In some embodiments, the flow rate of C2H2 is 20 mL / min, the flow rate of H2 is 250 mL / min, the deposition growth temperature can be 950 °C, the flow rate of the auxiliary gas Ar is 200 mL / min, and the operating power of the plasma generator is 300 W.
[0028] In this application, the positive electrode active material layer 20 disposed on the positive electrode current collector side can be a single coating or a stacked structure of two or more coatings. When the positive electrode active material layer 20 is a single coating, it may contain one or more positive electrode active materials. When the positive electrode active material layer 20 is a stacked multilayer coating, at least one coating contains the aforementioned compression additive.
[0029] In some embodiments of this application, see Figure 2 The positive electrode active material layer 20 includes a first positive electrode coating 21 and a second positive electrode coating 22 stacked together. The first positive electrode coating 21 is close to the positive electrode current collector 10. The first positive electrode coating 21 and / or the second positive electrode coating 22 contain the aforementioned compression rebound additive. At this time, the coating of the positive electrode sheet 100 has a double-layer structure. The presence of the compression rebound additive in any one or both positive electrode coatings of the positive electrode sheet 100 ensures that the positive electrode sheet 100 has good compression rebound performance.
[0030] When the first or second positive electrode coating contains the aforementioned compression additive, the corresponding positive electrode coating may contain no conductive agent or a small amount of conductive agent. In the embodiments of this application, the first positive electrode coating 21, in addition to containing the first positive electrode active material, may also contain a binder and optionally a small amount of conductive agent or no conductive agent. Similarly, the second positive electrode coating 22, in addition to containing the second positive electrode active material, also contains a binder and optionally a small amount of conductive agent or no conductive agent. For ease of description / reference, the conductive agent and binder that may be contained in the first positive electrode coating 21 may be referred to as "first conductive agent" and "first binder," respectively, and the conductive agent and binder that may be contained in the second positive electrode coating 22 may be referred to as "second conductive agent" and "second binder," respectively.
[0031] In this embodiment, the mass of the second binder in the second positive electrode coating 22 can be 0.1%-10% of the mass of the second positive electrode active material, preferably 2%-10%. Taking the second positive electrode coating 22 containing the above-mentioned three-dimensional graphene as an example, the amount of the compression elastic additive contained in this layer is greater than the amount of the second conductive agent it contains. Specifically, the mass of the second conductive agent can be 0%-2% of the mass of the second positive electrode active material, preferably 0.1%-1.5%, more preferably 0.1%-1%. At this time, the compression elastic additive, with a greater amount than the conductive agent, can give the second positive electrode coating 22 good compression resilience properties that ordinary positive electrode coatings do not possess. Similarly, in the first positive electrode coating 21, the mass of the first binder can be 0.1%-10% of the mass of the first positive electrode active material, preferably 2%-10%. The mass of the first conductive agent contained in the first positive electrode coating 21 can be 0%-2% of the mass of the first positive electrode active material, preferably 0.1%-1.5%, more preferably 0.1%-1%.
[0032] In some embodiments of this application, the first positive electrode coating 21 contains LiFe. 1-a Mn a The PO4 active material, wherein 0 ≤ a ≤ 1; the second positive electrode coating 22 comprises a lithium layered transition metal oxide active material and the aforementioned compression spring additive. In some embodiments of this application, 0 ≤ a ≤ 0.8, and / or the lithium layered transition metal oxide active material is a ternary material, that is, the aforementioned first positive electrode active material includes LiFe 1-a Mn a PO4 active material, the above-mentioned second positive electrode active material includes ternary active material.
[0033] Among them, LiFe 1-a Mn aPO4 materials shrink in volume during charging (e.g., the volume shrinkage rate of LiFePO4 during charging is about 7%), while lithium-containing layered transition metal oxides increase in volume during normal charging. For example, the volume of ternary materials increases by about 6% during normal charging. The volume changes of the two are asynchronous and show opposite trends, which can easily lead to the separation of the bilayer during long-term cycling.
[0034] During battery charging, the cell volume generally increases. As charging progresses, this increasing cell volume leads to greater external pressure from the battery casing. When a certain amount of the aforementioned elastic additive is added to the layered transition metal oxide layer (i.e., the second positive electrode coating 22) on the surface of the positive electrode, under this greater external pressure, the elastic additive gradually shrinks in volume, releasing some space for the expanding layered transition metal oxide. This reduces the volume expansion rate of the second positive electrode coating 22 containing the layered transition metal oxide during charging, thus minimizing its interaction with the LiFe-containing coating. 1-a Mn a The difference in volume change rate between the first positive electrode coatings 21 of the PO4 material reduces the overall volume change of the cell during charging. However, during battery discharge, the LiFe... 1-a Mn a The volume of the first positive electrode coating 21 of the PO4 material increases, while the volume of the second positive electrode coating 22 containing layered transition metal oxides decreases during discharge. The negative electrode volume also shrinks during discharge, and the external pressure on the cell gradually decreases. The spring-loaded additive gradually rebounds, which helps reduce the volume shrinkage rate of the second positive electrode coating 22 containing layered transition metal oxides during discharge. This reduces the difference in volume change between the two positive electrode coatings during discharge. Therefore, the presence of the spring-loaded additive can improve the volume change rate of each layer of the positive electrode 100 under different pressures, thereby preventing interlayer separation due to the difference in volume expansion rates of the two positive electrode coatings during long-term cycling.
[0035] In addition, for the positive electrode sheet 100 with a double-layer structured coating, the layered transition metal oxide with high energy density (such as a ternary material) is arranged on the surface layer of the positive electrode sheet 100 away from the positive current collector, which has low impedance for lithium ion conduction, thereby reducing its polarization resistance in the high potential range, lowering the electrochemical polarization during discharge, and further facilitating its uniform charge and discharge and improving cycle performance. Second, arranging the layered transition metal oxide (such as a ternary material) on the surface layer of the positive electrode sheet 100 can also make the surroundings of the layered transition metal oxide particles mostly be layered transition metal oxide particles in the same SOC (State of Charge) state, which is beneficial to homogenizing the surrounding environment of the layered transition metal oxide, realizing uniform discharge of the layered transition metal oxide particles, and helping to ensure the structural stability of the layered transition metal oxide and the exertion of material capacity, so as to stably exert the cycle performance. Third, since the particle size of the layered transition metal oxide (such as a ternary material) is generally larger than that of LiFe 1- a Mn a PO4 material, the porosity in the layered transition metal oxide layer will be significantly greater than that of the LiFe 1-a Mn a PO4 material layer, so that the pore structure on the surface layer of the positive electrode sheet 100 is relatively loose, which is more conducive to being infiltrated by the electrolyte, making the deintercalation / intercalation of Li+ in the layered transition metal oxide smoother, facilitating the exhibition of its high-capacity characteristics. At the same time, the layered transition metal oxide layer with relatively high porosity on the surface layer has less impact on the discharge of the LiFe 1-a Mn a PO4 material in the inner layer, which is beneficial to the exertion of the rate performance of the inner layer material, thereby ensuring that the overall positive electrode sheet exerts high capacity.
[0036] In the embodiments of the present application, the general structural formula of the ternary material is LiNi x Co y M z O2, where M is at least one metal element from Group IIIB to Group VA, 0.33≤x≤0.98, 0<y<1, 0<z<1, and x+y+z=1. For example, M is at least one of Mn, Al, Zr, Ti, Y, Sr, W and the like, and M being Mn or Al is relatively common. When the value of x is relatively high, the ternary material has a high specific capacity and good rate performance, and the ternary material at this time can be referred to as a "high-nickel ternary material". Preferably, the value range of x is 0.70≤x≤0.98, more preferably 0.80≤x≤0.90, and even more preferably 0.83≤x≤0.88. Optionally, y satisfies 0.01≤y≤0.33, and z satisfies 0.01≤z≤0.33.
[0037] In the present application, when a=0, the general formula is LiFe 1-a Mna The material of PO4 is specifically lithium iron phosphate; when a > 0, the material is specifically lithium manganese iron phosphate, where a ≤ 0.8, which helps to ensure the stability of the structure of lithium manganese iron phosphate.
[0038] Generally, LiFe 1-a Mn a The particle size of PO4 material is smaller than that of layered transition metal oxide active materials. Optionally, the particle size D50 of the layered transition metal oxide active material is 3-15 μm, for example, 3-10 μm. Optionally, the LiFe... 1-a Mn a The particle size D50 of the PO4 material is 0.8-1.8 μm, for example, 0.8-1.5 μm. Further, the LiFe... 1-a Mn a PO4 materials also have a carbon coating layer on their surface to improve their conductivity; LiFe 1-a Mn a PO4 may contain doped elements to improve its rate performance.
[0039] This application does not impose any special restrictions on the binders and conductive agents in the first positive electrode coating 21 and the second positive electrode coating 22; conventional materials existing in the art can be used. The first and second binders can be independently selected from one or more of polyvinylidene fluoride (PVDF), polytetrafluoroethylene (PTFE), polyvinyl alcohol (PVA), styrene-butadiene rubber (SBR), polyacrylonitrile (PAN), polyimide (PI), polyacrylic acid (PAA), polyacrylate, polyolefins (such as polyethylene, polypropylene, polystyrene, etc.), sodium carboxymethyl cellulose (CMC), sodium alginate, etc., but are not limited thereto. The first and second conductive agents can be independently selected from one or more of carbon black (such as acetylene black, Ketjen black, Super P, 350G carbon black, etc.), furnace black, mesophase carbon microspheres, carbon fibers, carbon nanotubes, graphene, etc., but are not limited thereto.
[0040] In this embodiment, the thickness of the first positive electrode coating 21 can be in the range of 10 μm-150 μm, preferably 20-100 μm. The thickness of the second positive electrode coating 22 can be in the range of 5 μm-50 μm, preferably 5-30 μm. In some embodiments, LiFe... 1-a Mn a The thickness of the first positive electrode coating 21 of PO4 is greater than that of the second positive electrode coating 22 containing the ternary active material. In this case, the aforementioned positive electrode 100 can not only achieve a higher thickness than pure LiFe with the same areal density, but also... 1-a Mn a PO4 cathodes offer higher capacity while ensuring LiFe... 1-a Mna PO4 and layered transition metal oxide materials in positive electrode 100 exhibit performance comparable to pure LiFe. 1-a Mn a The respective properties of PO4 and pure layered transition metal oxide materials as electrodes.
[0041] In this application, the positive current collector 10 can be any material suitable for serving as the current collector of the positive electrode 100, including but not limited to elemental metal foil, alloy foil, metal-plated polymer film, or the aforementioned materials with carbon coating on the surface. Specifically, the elemental metal foil can be aluminum foil, the alloy foil can be aluminum alloy foil, and the metal plated on the surface of the polymer film can be an elemental aluminum layer or an aluminum alloy layer.
[0042] In some embodiments of this application, Figure 2 The double-coated positive electrode shown can be prepared by the following method: A LiFe-containing coating is sequentially coated onto the surface of the positive current collector 10. 1-a Mn a The first positive electrode slurry containing PO4 active material and the second positive electrode slurry containing ternary active material and compression additive are dried and pressed, and then the first positive electrode coating 21 and the second positive electrode coating 22 are sequentially stacked on the positive electrode current collector 10 to obtain the positive electrode sheet.
[0043] Among them, the first positive electrode slurry, after drying, forms a LiFe-containing material. 1-a Mn a The first positive electrode coating 21 of PO4 active material and the second positive electrode slurry, after drying, form a second positive electrode coating 22 containing ternary active material and compression additives. The first positive electrode slurry may further include a first conductive agent and a first binder, and the second positive electrode slurry may further include a second conductive agent and a second binder. The types and contents of each conductive agent and binder are as described above in this application. Furthermore, the solvents contained in the first and second positive electrode slurries can be independently selected from one or more of N-methylpyrrolidone (NMP), dimethylformamide (DMF), diethylformamide (DEF), water, and alcohol solvents (such as ethanol), with NMP being the most common. The solvent content is not particularly limited, as long as it meets the requirements for the flowability and uniformity of the slurry coating.
[0044] In this embodiment, the first positive electrode slurry and the second slurry can be sequentially coated using a coating machine with dual coating dies; alternatively, they can be coated separately using coating machines with single coating dies. The second positive electrode slurry can be applied after the first positive electrode slurry has dried to form the first positive electrode coating. Furthermore, the positive electrode current collector can be coated on one side or both sides. In other words, a stacked structure of the first and second positive electrode coatings can be formed on one side surface of the positive electrode current collector, or a stacked structure of the first and second positive electrode coatings can be formed on both opposite sides of the positive electrode current collector.
[0045] This application does not limit the areal density of the aforementioned positive electrode sheet, and it can be designed according to the specific electrochemical system. In some embodiments, the first positive electrode slurry is prepared such that the areal density of the first positive electrode coating on one side reaches 100-200 g / m². 2 The coating process involves applying a second positive electrode slurry to achieve a single-sided surface density of 10-100 g / m². 2 Coating is then performed. In this embodiment of the application, during the preparation of the positive electrode sheet, the pressure used for pressing can be 50-200 MPa, for example, 150 MPa.
[0046] In some embodiments of this application, a buffer layer containing the aforementioned compression elastic additive and binder may be provided between the first positive electrode coating 21 and the second positive electrode coating 22. Figure 2 (Not shown). This buffer layer also has compression and rebound properties, which can act as a spring-like connection between the two positive electrode coatings, weakening the volume change difference between the two positive electrode coatings during battery cycling, avoiding interlayer separation, and better improving the long-cycle capability of the positive electrode sheet.
[0047] This application also provides a battery, which includes the positive electrode sheet described above in this application embodiment.
[0048] In this embodiment of the application, the battery further includes a negative electrode, a separator, and an electrolyte disposed between the positive and negative electrode. The separator separates the positive and negative electrode, maintaining their insulation and electrolyte retention properties. The separator, together with the positive and negative electrode, constitutes the battery cell, which is housed within the battery casing.
[0049] In some embodiments of this application, the battery can be assembled by the following method: a positive electrode, a separator, and a negative electrode are sequentially stacked to form a cell; the cell is housed in a battery casing, and an electrolyte is injected; then the battery casing is sealed to obtain the battery. In other embodiments of this application, the battery can be assembled by the following method: a positive electrode, a semi-solid electrolyte or a solid electrolyte, and a negative electrode are sequentially stacked to form a cell; the cell is housed in a battery casing, and then the battery casing is sealed to obtain the battery. When a semi-solid electrolyte or a solid electrolyte is used, the positive and negative electrodes may contain semi-solid electrolyte materials or solid electrolyte materials.
[0050] The separator can be a polymer separator, non-woven fabric, or other commonly used battery separators, including but not limited to single-layer PP (polypropylene) film, single-layer PE (polyethylene) film, double-layer PP / PE, double-layer PP / PP, and triple-layer PP / PE / PP separators. The electrolyte includes electrolyte salts and organic solvents. The specific types and compositions of the electrolyte salts and organic solvents are standard choices in the battery industry and can be selected based on actual needs. The solid or semi-solid electrolyte can be a sulfide electrolyte, oxide electrolyte, polymer electrolyte, etc. The battery casing can be aluminum-plastic film, copper-plastic film, steel-plastic film, or other packaging films, and can also be an aluminum casing, steel casing, etc., depending on the type of battery.
[0051] This application also provides an electrical device equipped with the battery described in this application. The electrical device can be a means of transportation, such as a car or boat, or a 3C product. Due to the use of the battery, the electrical device has a long battery life and high safety.
[0052] The technical solution of this application will be further described below with reference to several specific embodiments.
[0053] Example 1
[0054] A method for preparing a positive electrode sheet, comprising:
[0055] (1) Lithium iron phosphate, binder PVDF and conductive agent Super P are mixed in solvent NMP at a mass ratio of 100:3:2 and stirred evenly to obtain the first positive electrode slurry;
[0056] The ternary active material NCM811 (with the general structural formula LiNi) was used. 0.8 Co 0.1 Mn 0.1 O2) was mixed with PVDF, Super P and three-dimensional graphene in a mass ratio of 100:2:1:5 in the solvent NMP and stirred evenly to obtain the second positive electrode slurry;
[0057] (2) Using aluminum foil as the positive electrode current collector, a first positive electrode slurry and a second positive electrode slurry are sequentially coated on one side surface of the aluminum foil. After drying, a double coating is formed with a first positive electrode coating and a second positive electrode coating stacked together. The first positive electrode coating 21 is close to the aluminum foil and is formed by drying the first slurry, with an areal density of 165 g / m³. 2 The second positive electrode coating 22 is formed by drying the second slurry, and has an areal density of 18.85 g / m³. 2 ;
[0058] Then, in the same manner, a first positive electrode coating and a second positive electrode coating are sequentially formed on the other side of the aluminum foil to obtain a double-sided positive electrode sheet; the double-sided positive electrode sheet is rolled under a pressure of 150 MPa to obtain a positive electrode sheet for use; wherein, in the positive electrode sheet, the thickness of the first positive electrode coating 21 on one side is 72 μm, and the thickness of the second positive electrode coating 22 on one side is 6 μm.
[0059] In Example 1, the mass ratio of lithium iron phosphate to NCM811 was 165 × 100 / 105 : 18.85 × 100 / 108 = 9. Furthermore, the three-dimensional graphene used in Example 1 (see...) Figure 3 It comprises overlapping graphene sheets, and the three-dimensional graphene has a porous structure. The average particle size of the three-dimensional graphene is 0.8 μm, and the pore volume is 2.5 cm³. 3 / g, the average pore size of the porous structure in the three-dimensional graphene is 12nm, and the interplanar spacing of the (002) crystal planes of the three-dimensional graphene is 0.34nm; the fracture strength of the joint of the graphene sheets that overlapped with each other in the three-dimensional graphene was measured to be 40N / m by nanoindentation test by AFM.
[0060] The preparation method of the three-dimensional graphene used in Example 1 is as follows: Cu is used as a substrate and placed in the deposition chamber of a PECVD deposition equipment for vacuum heating to reach a growth temperature of 950°C. A mixed gas of carbon source C2H2 and H2 (wherein the flow rate of C2H2 is 20 mL / min and the flow rate of H2 is 250 mL / min) is introduced into the deposition chamber, and the plasma generator of the deposition equipment is turned on to deposit and grow three-dimensional graphene material on the substrate by PECVD. After the growth of three-dimensional graphene is completed, the plasma generator and heating source are turned off, and the introduction of C2H2 and H2 is stopped. At the same time, the auxiliary gas Ar is introduced at a flow rate of 200 mL / min to cool the deposition chamber to room temperature in an inert atmosphere. Then, the sample is taken out from the deposition chamber, and the graphene material is peeled off from the substrate and crushed to the required particle size to obtain the three-dimensional graphene material required in Example 1.
[0061] Example 2
[0062] The difference between Example 2 and Example 1 is that in the second positive electrode slurry, the mass ratio of NCM811 to PVDF, Super P, and three-dimensional graphene is 100:2:2:15; and the first positive electrode slurry has an areal density of 150 g / m³ for the first positive electrode coating to be formed. 2 The coating process is carried out, with the second positive electrode slurry having an areal density of 50 g / m². 2 Apply the coating.
[0063] The positive electrode sheet prepared in Example 2 is denoted as P2. The thickness of the first positive electrode coating 21 on one side is 65 μm, and the thickness of the second positive electrode coating 22 on one side is 15 μm.
[0064] Example 3
[0065] The difference between Example 3 and Example 1 is that in the second positive electrode slurry, the mixing mass ratio of NCM811 to PVDF, Super P and three-dimensional graphene is 100:2:1:3.
[0066] Example 4
[0067] The difference between Example 4 and Example 1 is that in the second positive electrode slurry, the mixing mass ratio of NCM811 to PVDF, Super P and three-dimensional graphene is 100:2:1:20.
[0068] Example 5
[0069] The difference between Example 5 and Example 1 is that the three-dimensional graphene used in Example 5 has an average particle size of 3 μm and a pore volume of 3 cm³. 3 / g, the average pore size of the porous structure in this three-dimensional graphene is 40nm; the fracture strength of the joint of the graphene sheets that are overlapped together in the three-dimensional graphene was measured to be 30N / m by nanoindentation test by AFM.
[0070] Example 6
[0071] The difference between Example 6 and Example 1 is that: lithium manganese iron phosphate (structural formula LiFe) is used. 0.25 Mn 0.75 PO4) replaces lithium iron phosphate in Example 1.
[0072] Example 7
[0073] The difference between Example 7 and Example 1 is that the second positive electrode coating 22 does not contain three-dimensional graphene, while the first positive electrode coating 21 contains the three-dimensional graphene. Specifically, lithium iron phosphate, PVDF, Super P, and three-dimensional graphene are mixed in a mass ratio of 100:3:2:5 to prepare the first positive electrode slurry; NCM811 is mixed with PVDF and Super P in a mass ratio of 100:2:1 to prepare the second positive electrode slurry. Furthermore, the first positive electrode slurry has a single-sided areal density of 30 g / m² for the first positive electrode coating to be formed. 2 The coating process is carried out, with the second positive electrode slurry having an areal density of 125 g / m³. 2 Apply the coating.
[0074] Example 8
[0075] The ternary active material NCM811, binder PVDF, conductive agent Super P, and three-dimensional graphene were mixed in NMP solvent at a mass ratio of 100:2.9:1.9:8 and stirred evenly to prepare the positive electrode slurry with a single-sided areal density of 200 g / m³. 2 Coating is applied to both opposite surfaces of the aluminum foil.
[0076] To highlight the beneficial effects of this application, the following comparative examples 1-3 are also provided.
[0077] Comparative Example 1
[0078] Lithium iron phosphate material and ternary active material NCM811 were mixed at a mass ratio of 90:10 to obtain a mixed positive electrode active material. This mixed material was then mixed with PVDF and Super P at a mass ratio of 100:3:3 in NMP solvent and stirred until homogeneous to obtain a positive electrode slurry. This positive electrode slurry was coated onto opposite sides of an aluminum foil, and after drying and rolling, a positive electrode sheet D1 was obtained. The thickness of the positive electrode coating on one side of the positive electrode sheet D1 was 65 μm, and the areal density on one side was 185 g / m³. 2 .
[0079] Comparative Example 2
[0080] The difference between Comparative Example 2 and Example 1 is that neither the first positive electrode coating 21 nor the second positive electrode coating 22 contains three-dimensional graphene. The formulation of the first positive electrode slurry is the same as in Example 1, while in the second positive electrode slurry, the mass ratio of NCM811 to PVDF and Super P is 100:2:1. Furthermore, the first positive electrode slurry is prepared to achieve a single-sided areal density of 165 g / m² for the first positive electrode coating to be formed. 2 The coating process is carried out, with the second positive electrode slurry having a single-sided areal density of 18.5 g / m². 2 Apply the coating.
[0081] Comparative Example 3
[0082] The difference between Comparative Example 3 and Example 8 is that the positive electrode active coating does not contain three-dimensional graphene.
[0083] Comparative Example 4
[0084] The difference between Comparative Example 4 and Example 1 is that the second positive electrode slurry was prepared by mixing ternary active material NCM811 with PVDF, Super P and three-dimensional graphene in a ratio of 100:2:1:2.
[0085] Among them, the thickness springback rate and thickness compression rate of the positive electrode sheet obtained in Comparative Example 4 are both less than 2% (see Table 2 below for details).
[0086] To strongly support the beneficial effects of the technical solution of this application, the positive electrode sheets in the above examples are all prepared into corresponding full cells according to the following method: (1) Natural graphite, silicon suboxide, conductive agent, and binder are mixed in water at a mass ratio of 95:5:1:3.5 to obtain a negative electrode slurry; the negative electrode slurry is coated on both sides of an 8μm thick copper foil, and after baking to remove the solvent, a negative electrode active material layer is formed on the copper foil, and then rolled, slit, and die-cut to obtain a double-sided negative electrode sheet; (2) The positive electrode sheets, PE separator, and the above negative electrode sheets of each embodiment or comparative example are stacked in sequence to form a cell, which is then filled with liquid and sealed in an aluminum-plastic film. After high-temperature aging, formation, aging, capacity testing, and vacuum sealing, a full cell is obtained.
[0087] The prepared battery is then placed in a fixture, with a gap between the fixture and the battery equal to 2% of the battery thickness. The fixture position remains fixed, and the batteries undergo initial charge-discharge capacity testing and cycle performance testing. It should be noted that since different batteries are required for the initial charge-discharge specific capacity test and capacity retention test, at least two full cells should be prepared for each embodiment or comparative example.
[0088] The test method for the first charge and discharge capacity is as follows: at 25°C, each full battery is charged at a constant current of 0.1C to 4.25V, and then charged at a constant voltage of 4.25V to the cutoff current of 0.05C; then discharged at 0.1C to 2.5V to obtain the first charge specific capacity and the first discharge specific capacity.
[0089] Cyclic performance test: At 25℃, each full cell was first charged at 1C with a constant current to 4.25V, then charged at 4.25V with a constant voltage to the cutoff current of 0.1C, and then discharged at 1C to 2.5V. This cycle was repeated 300 times. The initial discharge capacity and the discharge capacity after 300 cycles were recorded. The capacity retention rate after 300 cycles = (discharge capacity after 300 cycles / initial discharge capacity) * 100%.
[0090] The relevant results are summarized in Table 1 below, and the battery cycle performance curves for some examples are plotted in Table 2. Figure 4 .
[0091] Table 1
[0092]
[0093] As can be seen from Table 1, the battery made using the positive electrode sheet with compression-rebound characteristics according to the embodiments of this application has excellent cycle performance when the cell is cyclic in a space with a fixed volume.
[0094] The full cells that underwent the first charge-discharge capacity test were disassembled, and the positive electrode of each full cell was taken to test the electrode rebound performance and compression performance. The results are summarized in Table 2 below.
[0095] The rebound performance of each positive electrode is tested as follows: A pressure of X1 MPa is applied to each electrode, and the thickness of the electrode under the X1 MPa pressure is measured as H1; then the pressure is removed, and after the thickness of the electrode stabilizes, the thickness of the electrode is measured again and recorded as H2. The thickness rebound rate of the electrode is then r = (H2 - H1) / H1. The rebound performance of the positive electrode is tested as follows: A pressure of X2 MPa is applied to an electrode with an initial thickness of H3, and the thickness of the electrode under the X2 MPa pressure is measured and recorded as H4. The thickness compression rate of the electrode is then p = (H3 - H4) / H3. In this embodiment, X1 = 0.5 MPa, X2 = 0.3 MPa.
[0096] Table 2
[0097] Electrode thickness resilience Electrode thickness compression ratio Example 1 2.3% 2.2% Example 2 9.2% 9.1% Example 3 2.0% 2.0% Example 4 4.2% 4.1% Example 5 2.4% 2.3% Example 6 2.3% 2.2% Example 7 3.5% 3.4% Example 8 19.4% 19.3% Comparative Example 1 0.1% 0% Comparative Example 2 0.1% 0.1% Comparative Example 3 0.1% 0% Comparative Example 4 0.9% 0.8%
[0098] As shown in Table 2, adding an appropriate amount of three-dimensional graphene to the positive active material layer of each positive electrode sheet in the embodiments of this application endows the positive electrode sheet with certain compression-rebound characteristics, which is beneficial to improving the cycle performance of the battery when cycling in a fixed volume space. In addition, the positive electrode sheet with a positive coating formed by directly coating ternary materials and lithium iron phosphate (Comparative Example 1) has no compression and rebound performance. However, after the ternary material layer and the lithium phosphate material layer are set in layers, and an appropriate amount of three-dimensional graphene is added to the ternary material layer (Examples 1-5), the compression and rebound performance of the positive electrode sheet is more significant, which is beneficial to further improve the cycle performance of the battery. In addition, for the positive electrode sheet with a single layer of positive active material layer, the addition of three-dimensional graphene to the positive active coating (Example 8) also results in a significantly better compression-rebound performance than the positive electrode sheet without three-dimensional graphene (Comparative Example 3). In addition, although three-dimensional graphene was added to the ternary material layer of Comparative Example 4, the amount added was small, so the thickness rebound rate and thickness compression rate of the positive electrode sheet of Comparative Example 4 were both less than 2%, that is, the compression-rebound performance of the positive electrode sheet was not outstanding. As a result, the cycle performance of the battery of Comparative Example 4 in a fixed volume space was still significantly lower than that of Example 1 (see Table 1 above).
[0099] The embodiments described above are merely illustrative of several implementation methods of this application, and while the descriptions are specific and detailed, they should not be construed as limiting the scope of this patent application. It should be noted that those skilled in the art can make various modifications and improvements without departing from the concept of this application, and these all fall within the protection scope of this application. Therefore, the protection scope of this patent application should be determined by the appended claims.
Claims
1. A positive electrode plate, characterized in that, The device includes a positive current collector and a positive active material layer disposed on at least one surface of the positive current collector. The positive active material layer contains a compressive elastic additive, wherein the compressive elastic additive is three-dimensional graphene. The three-dimensional graphene comprises overlapping graphene sheets with a porous structure. The tensile strength at the overlap of the overlapping graphene sheets is 20-50 N / m. The average particle size of the three-dimensional graphene is 0.5 µm-20 µm, and the pore volume of the three-dimensional graphene is 1-10 cm³. 3 Between / g; the mass of the compression additive is 3%-50% of the mass of the positive active material in the positive active material layer; wherein, after a pressure greater than 0 and less than or equal to 5 MPa is applied along the thickness direction of the positive electrode sheet, the thickness rebound rate and thickness compression rate of the positive electrode sheet are each independently in the range of 2%-20%.
2. The positive electrode sheet as described in claim 1, characterized in that, The average pore size of the porous structure of the three-dimensional graphene is 10-200 nm.
3. The positive electrode sheet as described in claim 1, characterized in that, The lateral dimensions of the graphene sheet are 10nm-100nm.
4. The positive electrode sheet as described in claim 3, characterized in that, The graphene sheet has a lateral dimension of 10nm-30nm.
5. The positive electrode sheet as described in any one of claims 1-4, characterized in that, The positive electrode active material layer includes a first positive electrode coating and a second positive electrode coating stacked together, the first positive electrode coating being close to the positive electrode current collector, wherein the first positive electrode coating and / or the second positive electrode coating contain the compression additive.
6. The positive electrode sheet as described in claim 5, characterized in that, The first positive electrode coating includes LiFe 1-a Mn a PO4 active material, 0≤a≤1; the second positive electrode coating comprises a layered transition metal oxide active material and the compression spring additive.
7. The positive electrode sheet as described in claim 6, characterized in that, 0≤a≤0.8, the layered transition metal oxide active material is a ternary material.
8. The positive electrode sheet as described in claim 6, characterized in that, The thickness of the first positive electrode coating is in the range of 10-150µm, and the thickness of the second positive electrode coating is in the range of 5-50µm.
9. The positive electrode sheet as described in claim 5, characterized in that, A buffer layer containing the compression additive and binder is also provided between the first positive electrode coating and the second positive electrode coating.
10. A battery, characterized in that, The battery includes a positive electrode as described in any one of claims 1-9.
11. An electrical appliance, characterized in that, The electrical device includes the battery as described in claim 10.
Citation Information
Patent Citations
Cathode of lithium ion battery
CN109980181A
Graphene foam-protected metal fluoride and metal chloride cathode active materials for lithium batteries
CN110366792A