Cuprous selenide-based thermoelectric materials, their preparation methods and applications
By doping AgSbF6 into the Cu2-xSe matrix to form a Sb-rich second phase, the problems of long-range migration of copper ions and excessively high carrier concentration are solved, achieving high power factor, low thermal conductivity and high stability of copper selenide-based thermoelectric materials, thus improving thermoelectric performance.
Patent Information
- Application Number
- CN202311277647.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-09-28
- Publication Date
- 2026-11-17
- Estimated Expiration
- 2043-09-28
AI Technical Summary
Existing cuprous selenide thermoelectric materials suffer from the long-range migration of copper ions, which affects the device's service performance and lifespan. Furthermore, excessively high carrier concentrations degrade thermoelectric performance.
By doping AgSbF6 into the Cu2-xSe matrix, Ag and F elements replace cation and anion vacancies, forming a Sb-rich second phase. This enhances the copper ion migration barrier, restricts long-range migration, and the second phase formed by Ag and F elements synergistically enhances phonon scattering, thereby reducing carrier concentration and thermal conductivity.
It improves the power factor and Seebeck coefficient of copper selenide-based thermoelectric materials, reduces thermal conductivity, increases the dimensionless thermoelectric figure of merit (ZT), and enhances material stability and thermoelectric performance.
Smart Images

Figure CN117320532B_ABST
Abstract
Description
Technical Field
[0001] This invention belongs to the field of energy materials technology, specifically relating to a copper selenide-based thermoelectric material, its preparation method, and its application. Background Technology
[0002] All-solid-state thermoelectric power generation technology, which is green and environmentally friendly, has attracted attention due to its ability to directly convert electrical energy into heat energy. Thermoelectric devices operate without chemical reactions or fluid media, have no moving mechanical parts, are less prone to failure, produce no noise, are highly reliable, have a long service life, and low maintenance costs. The thermoelectric conversion efficiency is determined by the dimensionless thermoelectric figure of merit ZT, expressed as ZT = σS 2 T / κ, where σ is the conductivity, S is the Seebeck coefficient, and σS 2 These are typically referred to as the power factor, where T is the absolute temperature and κ is the thermal conductivity. However, since these thermoelectric parameters are interconnected through the carrier concentration n, individually tuning any one of them is quite challenging. Previous researchers have proposed various effective performance enhancement strategies, such as bandgap convergence, nanocompositing, and configuration entropy engineering. The aim is to improve thermoelectric performance by maximizing the power factor and minimizing the thermal conductivity.
[0003] Cuprous selenide materials mainly exist in two crystal structures, referred to as the room-temperature α phase and the high-temperature β phase. The crystal structure of the room-temperature α phase is extremely complex and remains undetermined. When the temperature rises above 400K, cuprous selenide undergoes a phase transition, changing from the α phase to the β phase. This phase transition is reversible, belonging to the second-order phase transition, and the electrothermal transport properties at the phase transition point exhibit significant fluctuations. Studies have found that when the phase transition occurs, the material's density, crystal structure, and carrier concentration undergo drastic changes, leading to enhanced electroacoustic scattering. To more accurately measure the thermal conductivity at the phase transition point, researchers have incorporated the heat absorption caused by the phase transition into the thermal conductivity measurement process, which not only corrects the heat transport equation but also provides a basis for the accurate calculation of the thermoelectric figure of merit at the phase transition point. The structure of the high-temperature β phase is determined; it is a cubic structure with space group [missing information]. In the high-temperature β-phase structure of cuprous selenide, the rigid sublattice composed of Se atoms primarily determines the band edge state and carrier transport properties of the valence band, which is the essential reason for its "electronic crystal" nature. Copper ions are randomly distributed in interstitial positions, allowing for long-range migration and exhibiting liquid-like fluidity. This explains why the specific heat of cuprous selenide at high temperatures falls between that of a solid and a liquid. The migration of copper ions also scatters some transverse phonons in the material, reducing the phonon mean free path. Consequently, the intrinsic lattice thermal conductivity of cuprous selenide is only 0.5 W / m² at 1000 K. -1 K -1 In addition, the electrical conductivity and carrier mobility (20 cm⁻¹) of cuprous selenide materials are... 2 V -1 s -1It is also at a relatively high level among fast ion conductor materials. Calculations show that the electrical properties are mainly determined by the sublattice of Se, and the number of copper vacancies has almost no effect on the band shape.
[0004] Although copper ions can scatter phonons and participate in electrical conduction, they can migrate and precipitate directionally under temperature gradient fields and high currents, which can affect the performance and lifespan of devices in practical applications. Furthermore, in the experimentally prepared cuprous selenide materials, the presence of intrinsic copper vacancies and copper ions leads to an excessively high carrier concentration, significantly degrading the thermoelectric properties of the cuprous selenide materials.
[0005] Therefore, existing cuprous selenide thermoelectric materials need to be improved. Summary of the Invention
[0006] This invention aims to at least partially solve one of the technical problems in related technologies. Therefore, one object of this invention is to provide a cuprous selenide-based thermoelectric material, its preparation method, and its application. This cuprous selenide-based thermoelectric material maintains a high power factor, low thermal conductivity, and can restrict the long-range migration of copper ions, thereby exhibiting high thermoelectric performance and strong stability.
[0007] In a first aspect, the present invention provides a cuprous selenide-based thermoelectric material. According to an embodiment of the present invention, the chemical composition of the cuprous selenide-based thermoelectric material is: Cu 2-x Se-n AgSbF6, where 0≤x≤0.25, 0<n≤2%.
[0008] The copper selenide-based thermoelectric material according to the above embodiments of the present invention has a chemical composition of Cu. 2-x Se-n AgSbF6, where 0≤x≤0.25, 0<n≤2%. This is achieved by using Cu... 2-x Adding silver hexafluoroantimonate (AgSbF6) to the matrix composition of Se allows Ag and F elements to be doped into Cu. 2-x In a Se matrix, Cu is substituted. 2-x The presence of anion and cation vacancies in the Se matrix, and the Sb element in Cu 2-xThe formation of a Sb-rich second phase in the Se matrix has several advantages. Firstly, the doping of Ag and F elements not only enhances the migration barrier of copper ions, restricting their long-range migration and thus improving the stability of cuprous selenide-based thermoelectric materials, but also effectively reduces the carrier concentration to a more optimal level, increasing carrier mobility and Seebeck coefficient, thereby improving the power factor. Secondly, Ag and F elements, acting as point defects, can synergistically enhance phonon scattering with the Sb-formed second phase, reducing the thermal conductivity and thus improving the dimensionless thermoelectric figure of merit (ZT). Furthermore, the inventors discovered that due to the limited solid solubility of different substances in the crystal lattice, excessive addition of AgSbF6 can result in Ag and F elements remaining in the Cu, unable to replace anion and cation vacancies. 2-x Other reactions occur in the Se matrix to form a second phase, which adversely affects the thermoelectric properties of cuprous selenide-based thermoelectric materials. Therefore, Cu... 2-x Se is used as the matrix, and AgSbF6 is added in an appropriate molar ratio, i.e., 0 < n ≤ 2%, to dope Ag and F elements into Cu. 2-x In a Se matrix, and to make the Sb element in Cu 2-x The formation of a Sb-rich second phase within the Se matrix not only restricts the long-range mobility of copper ions, thus improving the power factor of the cuprous selenide-based thermoelectric material, but also reduces its thermal conductivity. Consequently, this cuprous selenide-based thermoelectric material maintains a high power factor and low thermal conductivity, while simultaneously restricting the long-range mobility of copper ions, resulting in superior thermoelectric performance and strong stability.
[0009] In addition, the copper selenide-based thermoelectric material according to the above embodiments of the present invention may also have the following additional technical features:
[0010] In some embodiments of the present invention, when the chemical composition of the copper selenide-based thermoelectric material is 0.35% ≤ n ≤ 0.7%, the copper selenide-based thermoelectric material has high thermoelectric performance and strong stability.
[0011] In some embodiments of the present invention, the dimensionless thermoelectric figure of merit ZT of the copper selenide-based thermoelectric material is not less than 2.47 at 1000K.
[0012] In a second aspect, the present invention provides a method for preparing the above-mentioned cuprous selenide-based thermoelectric material. According to an embodiment of the present invention, the method includes:
[0013] (1) Based on the chemical composition Cu 2-xThe stoichiometric ratio of Se-n AgSbF6 is used to mix Cu, Se, and AgSbF6 and then ball-mill them to obtain a mixed powder.
[0014] (2) The mixed powder is subjected to discharge plasma sintering to obtain a copper selenide-based thermoelectric material.
[0015] Therefore, this method can be used to prepare copper selenide-based thermoelectric materials with good crystallinity, high reproducibility, good electrical properties, a high power factor, low thermal conductivity, and the ability to limit the long-range mobility of copper ions. These materials exhibit high thermoelectric performance and strong stability. Furthermore, this method is simple to operate, has a short cycle time, and consumes little energy, making it a promising candidate for application.
[0016] In addition, the method for preparing cuprous selenide-based thermoelectric materials according to the above embodiments of the present invention may also have the following additional technical features:
[0017] In some embodiments of the present invention, the mass ratio of grinding balls to the mixed powder during the ball milling process is (25-40):1, the rotation speed of the ball mill is 400 r / min-460 r / min, and the ball milling time is 3 h-8 h.
[0018] In some embodiments of the present invention, the ball milling is performed under a protective gas atmosphere.
[0019] In some embodiments of the present invention, the vacuum degree of the discharge plasma sintering is 0.1 Pa to 10 Pa.
[0020] In some embodiments of the present invention, the pressure applied by the upper and lower pressure heads in the furnace cavity of the discharge plasma sintering is 30MPa-65MPa.
[0021] In some embodiments of the present invention, the discharge plasma sintering temperature is 680°C-720°C. This improves the thermoelectric performance and stability of the cuprous selenide-based thermoelectric material.
[0022] In some embodiments of the present invention, the discharge plasma sintering includes a first stage and a second stage, wherein the first stage is performed according to the following steps: heating the mixed powder from room temperature to a first predetermined temperature within 5 min-10 min; the second stage is performed according to the following steps: heating from the first predetermined temperature to 680℃-720℃ within 1 min-4 min, and then holding at that temperature for 3 min-8 min. This improves the thermoelectric performance and stability of the cuprous selenide-based thermoelectric material.
[0023] In some embodiments of the present invention, the first predetermined temperature is 580°C-620°C. This improves the thermoelectric performance and stability of the cuprous selenide-based thermoelectric material.
[0024] In a third aspect, the present invention provides a thermoelectric device. According to embodiments of the invention, the thermoelectric device comprises the above-described cuprous selenide-based thermoelectric material or a cuprous selenide-based thermoelectric material prepared by the above method. Therefore, the thermoelectric device exhibits excellent thermoelectric conversion efficiency and a long service life.
[0025] Additional aspects and advantages of the invention will be set forth in part in the description which follows, and in part will be obvious from the description, or may be learned by practice of the invention. Attached Figure Description
[0026] The above and / or additional aspects and advantages of the present invention will become apparent and readily understood from the description of the embodiments taken in conjunction with the following drawings, in which:
[0027] Figure 1 These are the X-ray diffraction patterns of bulk samples of copper selenide-based thermoelectric materials from Examples 1-2 and Comparative Example 1 of this invention.
[0028] Figure 2 This is a graph showing the change in electrical conductivity as a function of temperature for bulk samples of cuprous selenide-based thermoelectric materials from Examples 1-2 and Comparative Example 1 of the present invention.
[0029] Figure 3 This is a graph showing the Seebeck coefficient as a function of temperature for bulk samples of cuprous selenide-based thermoelectric materials in Examples 1-2 and Comparative Example 1 of the present invention.
[0030] Figure 4 This is a graph showing the power factor of the bulk samples of copper selenide-based thermoelectric materials in Examples 1-2 and Comparative Example 1 as a function of temperature.
[0031] Figure 5 This is a graph showing the change of total thermal conductivity with temperature for bulk samples of cuprous selenide-based thermoelectric materials in Examples 1-2 and Comparative Example 1 of the present invention.
[0032] Figure 6 This is a graph showing the dimensionless thermoelectric figure of merit (ZT) of the bulk samples of copper selenide-based thermoelectric materials in Examples 1-2 and Comparative Example 1 as a function of temperature.
[0033] Figure 7 This is a graph showing the change of R / R0 over time for bulk samples of copper selenide-based thermoelectric materials in Embodiment 1 and Comparative Example 1 of the present invention. Detailed Implementation
[0034] Embodiments of the present invention are described in detail below, examples of which are illustrated in the accompanying drawings, wherein the same or similar reference numerals denote the same or similar elements or elements having the same or similar functions throughout. The embodiments described below with reference to the accompanying drawings are exemplary and intended to explain the present invention, and should not be construed as limiting the present invention.
[0035] In a first aspect, the present invention provides a cuprous selenide-based thermoelectric material. According to an embodiment of the present invention, the cuprous selenide-based thermoelectric material is Cu. 2-x The chemical composition of the Se-AgSbF6 complex is: Cu 2-x Se-nAgSbF6, where 0≤x≤0.25, 0<n≤2%, and x represents Cu 2-x The content of AgSbF6 is based on the amount of Se.
[0036] The inventors discovered that by using Cu 2-x Adding AgSbF6 to the matrix composition of Se allows Ag and F elements to be doped into Cu. 2-x In a Se matrix, Cu is substituted. 2-x The presence of anion and cation vacancies in the Se matrix, and the Sb element in Cu 2-x The formation of a Sb-rich second phase in the Se matrix has several advantages. Firstly, the doping of Ag and F elements not only enhances the migration barrier of copper ions, restricting their long-range migration and thus improving the stability of cuprous selenide-based thermoelectric materials, but also effectively reduces the carrier concentration to a more optimal level, increasing carrier mobility and Seebeck coefficient, thereby improving the power factor. Secondly, Ag and F elements, acting as point defects, can synergistically enhance phonon scattering with the Sb-formed second phase, reducing the thermal conductivity and thus improving the dimensionless thermoelectric figure of merit (ZT). Furthermore, the inventors discovered that due to the limited solid solubility of different substances in the crystal lattice, excessive addition of AgSbF6 can result in Ag and F elements remaining in the Cu, unable to replace anion and cation vacancies. 2-x Other reactions occur in the Se matrix to form a second phase, which adversely affects the thermoelectric properties of cuprous selenide-based thermoelectric materials. Therefore, Cu... 2-x Using Se as the matrix, AgSbF6 is added at an appropriate molar ratio (0.35% ≤ n ≤ 0.7%) to dope Ag and F elements into Cu. 2-x In a Se matrix, and to make the Sb element in Cu 2-xThe formation of a Sb-rich second phase within the Se matrix not only restricts the long-range mobility of copper ions, thus improving the power factor of the cuprous selenide-based thermoelectric material, but also reduces its thermal conductivity. Consequently, this cuprous selenide-based thermoelectric material maintains a high power factor and low thermal conductivity, while simultaneously restricting the long-range mobility of copper ions, resulting in superior thermoelectric performance and strong stability.
[0037] Preferably, in the chemical composition of the above-mentioned cuprous selenide-based thermoelectric material, 0.35% ≤ n ≤ 0.7%. Specifically, when 0.35% ≤ n ≤ 0.7%, the obtained cuprous selenide-based thermoelectric material has a dimensionless thermoelectric figure of merit (ZT) of not less than 2.47 at 1000K, exhibiting high thermoelectric performance and strong stability.
[0038] In a second aspect, the present invention provides a method for preparing the above-mentioned cuprous selenide-based thermoelectric material. According to an embodiment of the present invention, the method includes:
[0039] S100: Preparation of mixed powder
[0040] In this step, based on the chemical composition Cu 2-x The stoichiometric ratio of Se-n AgSbF6 is determined by weighing Cu, Se, and AgSbF6, mixing them, and then ball-milling them under a protective gas atmosphere to obtain a mixed powder. The purity of Cu is not less than 99.9%, Se is not less than 99.99%, and AgSbF6 is 99% by mass. The protective gas can be an inert gas, such as high-purity argon with a purity of not less than 99.999%. Further, the mass ratio of grinding balls to the mixed powder during the ball milling process can be (25-40):1, the ball milling speed can be 400-460 r / min, and the ball milling time can be 3-8 h. This method uses ball milling to process the raw materials to obtain a mixed powder. It is simple to operate, has a short cycle time, low energy consumption, and ensures sufficient reaction between the materials during subsequent discharge plasma sintering.
[0041] S200: The mixed powder is subjected to discharge plasma sintering.
[0042] In this step, the mixed powder prepared by S100 is placed in a graphite mold and subjected to discharge plasma sintering under pressure in a vacuum to obtain a cuprous selenide-based thermoelectric material. During the discharge plasma sintering process, Ag and F elements are doped into Cu. 2-x In a Se matrix, Cu is substituted. 2-xThe anion and cation vacancies in the Se matrix can enhance the migration barrier of copper ions, restricting their long-range migration and thus improving the stability of cuprous selenide-based thermoelectric materials. Furthermore, it can effectively reduce the carrier concentration in these materials, increasing carrier mobility and the Seebeck coefficient, thereby improving the power factor. (Note: The last sentence about Sb in Cu is unrelated and appears to be a separate, incomplete thought.) 2-x In the Se matrix, a Sb-rich second phase is formed. Ag and F elements, as point defects, can synergistically enhance phonon scattering with the Sb-formed second phase, thereby reducing the thermal conductivity of the cuprous selenide-based thermoelectric material and thus increasing its dimensionless thermoelectric figure of merit (ZT).
[0043] Furthermore, the vacuum degree of the above-mentioned discharge plasma sintering can be 0.1 Pa-10 Pa, the pressure applied by the upper and lower pressure heads in the furnace cavity can be 30 MPa-65 MPa, and the sintering temperature can be 680℃-720℃. According to a specific embodiment of the present invention, the discharge plasma sintering includes a first stage and a second stage, wherein the first stage is carried out according to the following steps: within 5 min-10 min, the above-mentioned mixed powder is heated from room temperature to 580℃-620℃ to make the mass transfer during the molding process of the mixed powder more sufficient; the second stage is carried out according to the following steps: within 1 min-4 min, the temperature is raised from 580℃-620℃ to 680℃-720℃, and then held at 680℃-720℃ for 3 min-8 min, which can obtain good crystallinity and avoid the volatilization of Se element, making the ratio of Cu element to Se element closer to the target value; finally, it is cooled from the holding temperature of the second stage to room temperature to obtain the copper selenide-based thermoelectric material. The cooling rate during the cooling process is preferably 10 K / min, which can avoid the adverse effects on the cuprous selenide-based thermoelectric material caused by the excessive phase transition of cuprous selenide, thereby improving the thermoelectric performance and stability of the cuprous selenide-based thermoelectric material.
[0044] Therefore, this method can prepare copper selenide-based thermoelectric materials with good crystallinity, high reproducibility, good electrical properties, high power factor, low thermal conductivity, and the ability to limit the long-range mobility of copper ions, exhibiting high thermoelectric performance and strong stability. Furthermore, this method is simple to operate, has a short cycle time, and low energy consumption, and has broad application prospects.
[0045] In a third aspect, the present invention provides a thermoelectric device. According to embodiments of the present invention, the thermoelectric device comprises the above-described cuprous selenide-based thermoelectric material or a cuprous selenide-based thermoelectric material prepared by the above-described method. Therefore, the thermoelectric device exhibits excellent thermoelectric conversion efficiency and a long service life. Those skilled in the art will understand that the features and advantages described above for the cuprous selenide-based thermoelectric material and its preparation method also apply to this thermoelectric device, and will not be repeated here.
[0046] The present invention will now be described with reference to specific embodiments. It should be noted that these embodiments are merely descriptive and do not limit the invention in any way. Where specific techniques or conditions are not specified in the embodiments, they shall be performed in accordance with the techniques or conditions described in the literature in the art or according to the product instructions. Reagents or instruments whose manufacturers are not specified are all conventional products that can be obtained commercially.
[0047] Comparative Example 1
[0048] (1) According to its chemical composition Cu 1.99 Se (i.e. Cu) 2-x In the stoichiometric ratio of Se-n AgSbF6 (x = 0.01, n = 0), 10 grams of a raw material mixture was weighed out, specifically 6.1561 grams of Cu elemental powder (purity 99.9%, size 625 mesh) and 3.8439 grams of Se elemental powder (purity 99.99%). The weighed mixture was placed in a stainless steel ball mill jar, with the mass ratio of stainless steel grinding balls to raw materials being 40:1. High-purity argon gas was filled into the ball mill jar as a protective gas, and the mixture was ball-milled for 6 hours at a speed of 460 r / min in a planetary ball mill (QM-3SP2, Nanjing University Instrument Factory).
[0049] (2) The powder obtained after ball milling was placed in a graphite mold, compacted, and then placed in a spark plasma sintering furnace (SPS). Under a vacuum of 5 Pa and a longitudinal pressure of 65 MPa, the temperature was raised to 600 °C in 9 min during the heating phase, and then raised from 600 °C to 700 °C in 3 min. After holding at 700 °C for 5 min, the temperature was cooled to room temperature at a rate of 10 K / min to obtain a product with the chemical composition Cu. 1.99 Selenide cuprous-based thermoelectric material bulk.
[0050] After sanding the surface of the bulk copper selenide thermoelectric material prepared in Comparative Example 1, phase identification was performed, and thermoelectric performance and stability tests were conducted. The stability test method was as follows: the initial resistance R0 of the sample was measured using a ZEM-3 Seebeck coefficient / resistance measurement system. In an air environment, a continuous directional pulse current and temperature were applied to the sample (pulse period of 1800s, duration of each current and temperature application of 900s, and current density of 20A / cm²).2 The sample resistance R was measured using a ZEM-3 Seebeck coefficient / resistance measurement system when the temperature was 453K and the current was 0, and R / R0 was calculated.
[0051] The X-ray diffraction pattern of the copper selenide-based thermoelectric material prepared in Comparative Example 1 is shown in Figure 1. Figure 1 , Figure 1 This indicates that the prepared material is pure-phase cuprous selenide.
[0052] The conductivity of the copper selenide-based thermoelectric material prepared in Comparative Example 1 as a function of temperature is shown in the figure. Figure 2 See Seebeck coefficient Figure 3 Power factor see Figure 4 Total thermal conductivity see Figure 5 The dimensionless thermoelectric figure of merit ZT value is shown in [reference needed]. Figure 6 .Depend on Figures 2 to 6 It can be seen that the chemical composition is Cu 1.99 The electrical conductivity of the copper selenide-based thermoelectric material of Se decreases with increasing temperature, the Seebeck coefficient increases with increasing temperature, the power factor increases with increasing temperature, the thermal conductivity decreases with increasing temperature, and the dimensionless thermoelectric figure of merit ZT increases with increasing temperature, reaching 2.37 at 1000 K.
[0053] The ratio of the resistance R of the cuprous selenide-based thermoelectric material prepared in Comparative Example 1 to its initial resistance R0 over time is shown in the figure. Figure 7 , Figure 7 This indicates that the chemical composition changed to Cu over time. 1.99 The R / R0 of the Se selenide cuprous thermoelectric material gradually decreases, indicating that the pure phase sample has poor stability.
[0054] Example 1
[0055] (1) According to its chemical composition Cu 1.99 Se-0.35% AgSbF6 (i.e., Cu) 2-x Weigh 10 grams of a raw material mixture according to the stoichiometric ratio of x = 0.01 and n = 0.35% in Se-n AgSbF6. Specifically, the mixture consists of 6.1202 grams of Cu elemental powder (99.9% purity, 625 mesh), 3.8214 grams of Se elemental powder (99.99% purity), and 0.0584 grams of AgSbF6 powder (99% purity). Place the weighed mixture into a stainless steel ball mill jar, with a stainless steel grinding ball to raw material mass ratio of 40:1. Fill the ball mill jar with high-purity argon as a protective gas and ball mill at 460 r / min for 6 hours in a planetary ball mill (QM-3SP2, Nanjing University Instrument Factory).
[0056] (2) The powder obtained after ball milling was placed in a graphite mold, compacted, and then placed in a spark plasma sintering furnace (SPS). Under a vacuum of 5 Pa and a longitudinal pressure of 65 MPa, the temperature was raised to 600 °C in 9 min during the heating phase, and then raised from 600 °C to 700 °C in 3 min. After holding at 700 °C for 5 min, the temperature was cooled to room temperature at a rate of 10 K / min to obtain a product with the chemical composition Cu. 1.99 Bulk of Se-0.35% AgSbF6 copper selenide-based thermoelectric material.
[0057] After the surface of the bulk copper selenide thermoelectric material prepared in Example 1 was polished with sandpaper, phase identification was performed, and thermoelectric performance and stability tests were conducted. The test methods were the same as those in Comparative Example 1.
[0058] The X-ray diffraction pattern of the copper selenide-based thermoelectric material prepared in Example 1 is shown in [reference needed]. Figure 1 The conductivity of the cuprous selenide-based thermoelectric material prepared in Example 1 as a function of temperature is shown in the figure. Figure 2 See Seebeck coefficient Figure 3 Power factor see Figure 4 Total thermal conductivity see Figure 5 The dimensionless thermoelectric figure of merit ZT value is shown in [reference needed]. Figure 6 .Depend on Figures 2 to 6 It can be seen that the chemical composition is Cu 1.99 The electrical conductivity of the Se-0.35%AgSbF6 cuprous selenide-based thermoelectric material decreases with increasing temperature, and is generally slightly lower than that of the cuprous selenide-based thermoelectric material prepared in Comparative Example 1. The Seebeck coefficient increases with increasing temperature, and is generally higher than that of the cuprous selenide-based thermoelectric material prepared in Comparative Example 1. The power factor increases with increasing temperature, and is significantly higher than that of the cuprous selenide-based thermoelectric material prepared in Comparative Example 1. This is because Ag and F doping can effectively control carrier concentration and mobility. Due to the decrease in electrical conductivity combined with the scattering effect of Ag and F point defects and the second relative phonons formed by Sb, the thermal conductivity decreases with increasing temperature, and is generally lower than that of the cuprous selenide-based thermoelectric material prepared in Comparative Example 1. The dimensionless thermoelectric figure of merit (ZT) increases with increasing temperature, and the power factor reaches 14.0 W·m at 1050 K. -1 ·K -2 The total thermal conductivity is 0.49 W·m. -1 ·K -1 The dimensionless thermoelectric figure of merit ZT value can reach 3.0.
[0059] The ratio of the resistance R of the copper selenide-based thermoelectric material prepared in Example 1 to its initial resistance R0 over time is shown in the figure. Figure 7 , Figure 7 This indicates that after 25,000 seconds, the chemical composition is Cu. 1.99The R / R0 of the Se-0.35% AgSbF6 copper selenide-based thermoelectric material did not show significant degradation, indicating that the Cu ion stability of the copper selenide-based thermoelectric material prepared in Example 1 was good, i.e., good chemical stability.
[0060] Example 2
[0061] (1) According to its chemical composition Cu 1.99 Se-0.7% AgSbF6 (i.e., Cu) 2-x In the stoichiometric ratio of Se-n AgSbF6 (x = 0.01, n = 0.7%), 10 grams of a raw material mixture was weighed out, specifically: 6.0843 grams of Cu elemental powder (purity 99.9%, size 625 mesh), 3.7991 grams of Se elemental powder (purity 99.99%), and 0.1166 grams of AgSbF6 powder (purity 99%). The weighed mixture was placed in a stainless steel ball mill jar, with the mass ratio of stainless steel grinding balls to raw materials being 40:1. High-purity argon gas was filled into the ball mill jar as a protective gas, and the mixture was ball-milled for 6 hours at a speed of 460 r / min in a planetary ball mill (QM-3SP2, Nanjing University Instrument Factory).
[0062] (2) The powder obtained after ball milling was placed in a graphite mold, compacted, and then placed in a spark plasma sintering furnace (SPS). Under a vacuum of 5 Pa and a longitudinal pressure of 65 MPa, the temperature was raised to 600 °C in 9 min during the heating phase, and then raised from 600 °C to 700 °C in 3 min. After holding at 700 °C for 5 min, the temperature was cooled to room temperature at a rate of 10 K / min to obtain a product with the chemical composition Cu. 1.99 Bulk of Se-0.7% AgSbF6 copper selenide-based thermoelectric material.
[0063] After the surface of the bulk copper selenide thermoelectric material prepared in Example 2 was polished with sandpaper, phase identification was performed, and thermoelectric performance and stability tests were conducted. The test methods were the same as those in Comparative Example 1.
[0064] The X-ray diffraction pattern of the copper selenide-based thermoelectric material prepared in Example 2 is shown in [reference needed]. Figure 1 The conductivity of the cuprous selenide-based thermoelectric material prepared in Example 2 as a function of temperature is shown in the figure. Figure 2 See Seebeck coefficient Figure 3 Power factor see Figure 4 Total thermal conductivity see Figure 5 The dimensionless thermoelectric figure of merit ZT value is shown in [reference needed]. Figure 6 .Depend on Figures 2 to 6 It can be seen that the chemical composition is Cu 1.99The electrical conductivity of the Se-0.7%AgSbF6 cuprous selenide-based thermoelectric material decreased with increasing temperature, and was generally slightly lower than that of the cuprous selenide-based thermoelectric material prepared in Comparative Example 1. The Seebeck coefficient increased with increasing temperature, and was generally higher than that of the cuprous selenide-based thermoelectric material prepared in Comparative Example 1. The power factor increased with increasing temperature, and was significantly higher than that of the cuprous selenide-based thermoelectric material prepared in Comparative Example 1. This is because Ag and F doping can effectively control carrier concentration and mobility. Due to the decrease in electrical conductivity combined with the scattering effect of Ag and F point defects and the second relative phonons formed by Sb, the thermal conductivity decreased with increasing temperature, and was generally lower than that of the cuprous selenide-based thermoelectric material prepared in Comparative Example 1. The dimensionless thermoelectric figure of merit (ZT) increased with increasing temperature, reaching 2.47 at 1000 K. The stability test results of the cuprous selenide-based thermoelectric material prepared in Example 2 were similar to those in Example 1, both exhibiting strong chemical stability.
[0065] As can be seen from Examples 1-2, by Cu 2-x Adding AgSbF6 to the matrix composition of Se can maintain the power factor of the obtained copper selenide-based thermoelectric material at a high level, with low thermal conductivity, and exhibits high thermoelectric performance and strong stability.
[0066] In the description of this specification, the references to terms such as "one embodiment," "some embodiments," "example," "specific example," or "some examples," etc., indicate that a specific feature, structure, material, or characteristic described in connection with that embodiment or example is included in at least one embodiment or example of the present invention. In this specification, the illustrative expressions of the above terms do not necessarily refer to the same embodiment or example. Furthermore, the specific features, structures, materials, or characteristics described may be combined in any suitable manner in one or more embodiments or examples. Moreover, without contradiction, those skilled in the art can combine and integrate the different embodiments or examples described in this specification, as well as the features of different embodiments or examples.
[0067] Although embodiments of the present invention have been shown and described above, it is understood that the above embodiments are exemplary and should not be construed as limiting the present invention. Those skilled in the art can make changes, modifications, substitutions and variations to the above embodiments within the scope of the present invention.
Claims
1. A cuprous selenide-based thermoelectric material, characterized in that, The chemical composition of the copper selenide-based thermoelectric material is as follows: With 2-x It - n AgSbF6, Where, 0≤ x ≤0.25, 0 < n ≤2%; The copper selenide-based thermoelectric material is prepared by a method comprising the following steps: (1) Based on the chemical composition Cu 2-x Se - n To obtain a mixed powder, Cu, Se, and AgSbF6 are mixed in a stoichiometric ratio and then ball-milled. (2) The mixed powder is subjected to discharge plasma sintering to obtain a copper selenide-based thermoelectric material.
2. The cuprous selenide-based thermoelectric material according to claim 1, characterized in that, 0.35%≤ n ≤0.7%。 3. The cuprous selenide-based thermoelectric material according to claim 2, characterized in that, At 1000K, the dimensionless thermoelectric figure of merit of the copper selenide-based thermoelectric material is not less than 2.
47.
4. A method for preparing the cuprous selenide-based thermoelectric material according to any one of claims 1-3, characterized in that, include: (1) Based on the chemical composition Cu 2-x Se - n To obtain a mixed powder, Cu, Se, and AgSbF6 are mixed in a stoichiometric ratio and then ball-milled. (2) The mixed powder is subjected to discharge plasma sintering to obtain a copper selenide-based thermoelectric material.
5. The method according to claim 4, characterized in that, The mass ratio of grinding balls to mixed powder during the ball milling process is (25-40):1, the rotation speed of the ball mill is 400r / min-460r / min, and the ball milling time is 3h-8h.
6. The method according to claim 4, characterized in that, The ball milling was carried out under a protective gas atmosphere.
7. The method according to claim 4, characterized in that, The vacuum degree of the discharge plasma sintering is 0.1 Pa to 10 Pa.
8. The method according to claim 4, characterized in that, The pressure applied by the upper and lower pressure heads in the furnace cavity of the discharge plasma sintering is 30MPa-65MPa.
9. The method according to claim 4, characterized in that, The temperature of the discharge plasma sintering is 680℃-720℃.
10. The method according to claim 9, characterized in that, The discharge plasma sintering includes a first stage and a second stage. The first stage is carried out according to the following steps: Within 5-10 minutes, the mixed powder is heated from room temperature to a first predetermined temperature; The second stage is carried out according to the following steps: Within 1-4 minutes, the temperature is raised from the first predetermined temperature to 680℃-720℃, and then held for 3-8 minutes.
11. The method according to claim 10, characterized in that, The first predetermined temperature is 580℃-620℃.