A method for extracting lithium from high-calcium clay-type lithium ore
Through the hydrochloric acid chemical dissociation method and sulfuric acid leaching step, the problem of low lithium extraction efficiency in high calcium clay lithium ore is solved, efficient extraction of lithium and effective utilization of gypsum waste residue are achieved, and the leaching rate of lithium and the leaching liquid are significantly improved. Lithium concentration reduces energy consumption and production costs.
Patent Information
- Application Number
- CN202311267102.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-09-28
- Publication Date
- 2024-11-01
- Estimated Expiration
- 2043-09-28
AI Technical Summary
The existing technology is difficult to efficiently extract lithium from high-cadmill lithium ore. Traditional methods such as sulfuric acid leaching and calcination-acid leaching technology have problems with low lithium utilization and a lot of gypsum waste residue, and lack effective targeting high-cadmill lithium ore. Processing method.
Calcite in high-calcium-type lithium ore is removed by hydrochloric acid chemical dissociation method. Through grinding, hydrochloric acid dissociation, calcination and sulfuric acid leaching steps, combined with non-wash filtration and low-temperature calcination, the leaching rate of lithium and the lithium concentration of the leaching solution are improved.
The efficient extraction of lithium is achieved, the lithium loss rate is less than 1%, the lithium leaching rate is increased by 6-10%, the lithium concentration of the leaching solution is increased by 40-80%, reducing the energy consumption of the lithium solution, and the dissociation solution and roasting residue are used. in the preparation of valuable calcium chloride and building materials.
Smart Images

Figure CN117327919B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of chemical metallurgy, and specifically relates to a method for extracting lithium from high-calcium clay-type lithium ore. Background Art
[0002] Lithium ore resources are a strategic resource with a wide range of applications. Due to the rapid development of new energy fields, the demand for lithium has increased sharply. Traditional lithium ore resources cannot meet the supply of lithium, and new lithium ore resources are urgently needed to be developed. Clay-type lithium ore has a relatively low lithium grade, but is widely distributed and has large reserves. If it can be developed using appropriate methods, it will be a very promising source of lithium demand.
[0003] The types of lithium resources used in industry are mainly brine-type related to salt lakes and hard rock-type related to granite pegmatites. At present, the actual supply of lithium resources in the world is mainly spodumene mines in Australia, brine in South American salt lakes and brine in Qinghai salt lakes in China. my country's self-supply of lithium resources is insufficient, and its external dependence is as high as 60%. Finding large lithium resources with economic value has become an urgent task for my country's geological exploration. A rare medium-large lithium resource prospecting area was discovered in Liuzhipingqiao, Guizhou Province. The lithium oxide reserves (average grade: 0.4%) are preliminarily estimated to exceed 40,000 tons, and the peripheral lithium mineralization information is strong, and the lithium mineralization prospect is excellent. More importantly, it was discovered for the first time that a large amount of lithium chlorite is distributed in the calcite veins of the ore-bearing strata (Permian Longyin Formation calcareous mudstone). Most of them are in the form of xenomorphic impregnation, coexisting with minerals such as fine-grained quartz and recrystallized pyrite, and distributed in groups in the calcite veins (Ye Lin, Xiang Zhenzhong, Wu Tao, et al. The discovery and significance of hydrothermal lithium chlorite in the lithium resource of Pingqiao, Liuzhi, Guizhou. Acta Mineralogica Sinica: 1-2 [2023-07-29]). Literature reports that the main minerals of sedimentary lithium mines in Liuzhi, Guizhou are lithium chlorite (21.10%), quartz (18.48%), calcite (19.10%), pyrite (5.86%), etc. However, due to the fine particle size of lithium chlorite, it is difficult to achieve lithium enrichment and recovery using traditional mineral processing methods. Only metallurgical methods can be used to enrich and recover the lithium element in this clay-type lithium ore (Hui Bo, Gong Daxing, Chen Wei. Research on the occurrence state of lithium in sedimentary lithium mines in Liuzhi, Guizhou [J]. Nonferrous Metals (Mineral Processing Part), 2021, 47(11): 1-4).
[0004] At present, there are no reports on the method of extracting lithium from high-calcium clay-type lithium ores. Most of the literature and patents on extracting lithium from low-grade lithium-containing clay ores that have been reported use the "blank roasting-sulfuric acid leaching" and "composite roasting-leaching" processes. The above process methods are difficult to apply to the efficient extraction of lithium from high-calcium clay-type lithium ores, because high-calcium clay-type lithium resources usually contain a large amount of calcite, which reacts with sulfuric acid to form gypsum (CaSO4·2H2O) during sulfuric acid leaching. A study reported that Xu Lu et al. used Guizhou sedimentary lithium ore (Li2O 0.64%, calcite 19.84%) as the research object, and obtained lithium leachate and leaching tailings through sulfuric acid leaching, but also produced a large amount of gypsum. In addition, a clay-type lithium ore in Guizhou contains 0.58% Li2O and 18.15% calcite. The ammonium sulfate roasting-acid leaching process for lithium will produce a large amount of calcium sulfate, which will wrap the roasted sand and affect the leaching effect of lithium (Kong Lingan, Li Zhengyao, Zhong Zhenyu, etc. Ammonium sulfate roasting-acid leaching of lithium from clay-type lithium ore [J]. Nonferrous Metals Engineering, 2022, 12(12): 66-72). The amount of slag produced by direct leaching with sulfuric acid is large and the lithium utilization rate is low. Waste slag containing a large amount of gypsum is still difficult to use, so new methods for treating high-calcium clay-type lithium ore should be found.
[0005] In summary, there is no efficient utilization method for high-calcium clay-type lithium ore (Li2O content less than 1%, CaO content 10%-30%). Therefore, developing a comprehensive utilization technology specifically for high-calcium clay-type lithium ore is of great strategic significance for promoting the transformation of geological scientific and technological achievements and the development of the lithium industry chain. Summary of the invention
[0006] The purpose of the present invention is to overcome the deficiencies of the prior art and provide a method for extracting lithium from high-calcium clay-type lithium ore.
[0007] The object of the present invention is achieved through the following technical scheme: A method for extracting lithium from high-calcium clay-type lithium ore, comprising the following steps:
[0008] S1. Grinding: Grind the high calcium clay-type lithium ore to -0.074mm, accounting for 60%-90%;
[0009] Wherein, the Li2O content in the high-calcium clay-type lithium ore is less than 1%, the CaO content is 10%-30%, and the CaO mainly exists in the form of calcite;
[0010] S2, chemical dissociation: adding the ground high calcium clay-type lithium ore to hydrochloric acid for chemical dissociation, filtering the dissociation residue obtained by chemical dissociation without washing, and then drying, with a water content of less than 3%;
[0011] The concentration of the hydrochloric acid is 1-6 mol / L, the liquid-solid ratio of chemical dissociation is 2-8 L / kg, the excess coefficient of the hydrochloric acid is 1-2.5, the time is 0.5-5 h, the dissociation temperature is 20-60 ° C, and the chloride ion content of the high calcium clay-type lithium ore after unwashing and drying is 0.5-3%, and the residual acid content is 0.2-1.2%;
[0012] The non-washing filtration refers to filtering the dissociation residue without washing with water, so that part of the chlorine radical and residual acid are retained in the dissociation residue;
[0013] S3, roasting: roasting the dried dissociated slag to obtain clinker, the roasting temperature is 400-650°C, and the time is 0.5-2.0h;
[0014] S4, sulfuric acid leaching: putting the clinker into a sulfuric acid solution for leaching reaction, and filtering to obtain a lithium-rich leaching solution and an aluminum-silicon-rich leaching residue;
[0015] The concentration of the sulfuric acid solution is 0.5-3 mol / L, the liquid-solid ratio of the leaching reaction is 2-8 L / kg, the time is 0.5-5 h, and the temperature of the leaching reaction is 30-90° C.
[0016] Preferably, in step S1, the high calcium clay-type lithium ore is ground to -0.074 mm, accounting for 75%-85%.
[0017] Preferably, in step S2, the concentration of the hydrochloric acid is 2-4 mol / L, the liquid-solid ratio of chemical dissociation is 4-6 L / kg, and the time is 2-4 h.
[0018] Preferably, in step S2, the chloride ion content of the high calcium clay-type lithium ore after unwashing and drying is 1.5-2.5%, and the residual acid content is 0.5-1%.
[0019] Furthermore, in step S2, the drying temperature is lower than 110°C, and the drying method is oven drying.
[0020] Preferably, in step S3, the calcination temperature is 500-600° C., and the calcination time is 1-1.5 h.
[0021] Preferably, in step S4, the concentration of the sulfuric acid solution is 1.5-3 mol / L, the liquid-solid ratio of the leaching reaction is 4-6 L / kg, and the time is 2-4 h.
[0022] Furthermore, in step S4, the filtering method is to use hot water for washing and filtering, and preferably the amount of hot water used is 1.5-3 times the weight of the aluminum-silicon-rich leaching residue.
[0023] In addition, the dissociation solution obtained by chemically dissociating high-calcium clay-type lithium ore with hydrochloric acid of the present invention has CaCl2 as its main component, which can be used as a raw material for preparing calcium chloride dihydrate. The aluminum-silicon-rich leaching slag obtained by the leaching reaction of the present invention has a small amount of slag and a low gypsum content (mainly Al2O3 and SiO2), and can be used as a raw material for building materials. The present invention enables efficient extraction of lithium from high-calcium clay-type lithium ore, and the gypsum content in the leaching slag is low, which is conducive to realizing the comprehensive utilization of valuable elements aluminum and silicon in the leaching slag.
[0024] The main principle of the present invention is: the calcium-containing mineral in the high-calcium clay-type lithium resource mineral composition targeted by the present invention is mainly calcite, the calcite particle size is larger than that of lithium chlorite, and calcite is easily soluble in acid, while lithium chlorite is generally difficult to dissolve in acid. The calcite in the original ore is removed by a chemical dissociation method. The lithium loss rate of this method is less than 1%, and more than 99% of the lithium in the ore is enriched in the solid phase product (the lithium enrichment ratio is 1.4-1.9), thereby reducing the ore processing amount of the roasting process and increasing the lithium content in the leachate. On the other hand, the present invention uses the dissociation slag without washing after filtration to retain part of the chloride ions and residual acid in the slag, reduces the roasting temperature during the roasting process, and shortens the roasting time, effectively improving the leaching rate of lithium in the subsequent leaching process.
[0025] The beneficial effects of the present invention are:
[0026] 1) The present invention provides an efficient smelting method for high-calcium clay-type lithium ore, which has the characteristics of low energy consumption, less reagents, less leaching slag (gypsum) and good lithium extraction effect.
[0027] 2) The present invention selects hydrochloric acid as a decalcifying agent to chemically dissociate high-calcium clay-type lithium ore, thereby removing calcium elements (calcite) in the ore, with a removal rate of more than 94.5%, preventing or greatly reducing the formation of gypsum during subsequent sulfuric acid leaching; at the same time, lithium chlorite is dissociated from the calcite wrapping, which is beneficial to the subsequent efficient leaching of lithium, and can significantly increase the lithium leaching rate (the lithium leaching rate is increased by 6-10%), and at the same time increase the lithium concentration of the leachate (the lithium concentration is increased by 40-80% compared with the original ore roasting-sulfuric acid leaching), thereby significantly reducing the energy consumption of lithium solution concentration.
[0028] 3) The present invention uses hydrochloric acid to chemically dissociate the high-calcium clay-type lithium ore, and adopts a direct filtration without washing method, which not only enriches the lithium element, but also retains a certain amount of chloride ions and residual acid in the dissociation slag; in the roasting process, it plays a role in reducing the roasting temperature and shortening the roasting time, which is beneficial to improving the subsequent lithium extraction effect and reducing the production cost.
[0029] 4) The hydrochloric acid leaching solution of the present invention contains a large amount of calcium chloride, which is comprehensively utilized to prepare calcium chloride; at the same time, due to the removal of calcium element, the amount of leaching residue is small and the chemical composition is simple, which is convenient for comprehensive utilization of leaching residue. BRIEF DESCRIPTION OF THE DRAWINGS
[0030] Figure 1 It is a process flow chart of the present invention. DETAILED DESCRIPTION
[0031] The technical solution of the present invention is further described in detail below in conjunction with the accompanying drawings, but the protection scope of the present invention is not limited to the following.
[0032] Example 1
[0033] The main minerals and contents of sedimentary lithium ore in Guizhou are: lithium chlorite (21.10%), quartz (18.48%), calcite (19.10%), pyrite (5.86%) and other minerals, among which the Li2O content is 0.63% and the CaO content is 11.92%. (Hui Bo, Gong Daxing, Chen Wei. Study on the occurrence state of lithium in sedimentary lithium ore in Liuzhi area, Guizhou [J]. Nonferrous Metals (Ore Dressing Part), 2021, 47(11): 1-4)
[0034] Step 1, grinding: take 1000g of ore and grind it to a particle size of less than 0.074mm, accounting for 78%;
[0035] Step 2, chemical dissociation: add 8000 ml of 1 mol / L hydrochloric acid (HCl excess coefficient 1.88) to the sample in step 1, stir and react at room temperature for 4 hours, and dry the leached residue obtained by decalcification by direct filtration without washing, with a water content of less than 2.5%, to obtain 703.21 g of lithium enriched material (Li2O content of 0.9%), with a lithium enrichment ratio of 1.43, wherein the lithium loss rate is less than 1%, and the calcium removal rate reaches 96.42%;
[0036] Step 3, roasting: roasting the dissociated slag. Since the slag already contains chloride salt (1.89%) and residual acid (0.84%), it is only necessary to spread it evenly on the porcelain ark, put it into a muffle furnace heated to 500°C, and roast it for 1 hour. After the roasting is completed, it is naturally cooled to room temperature to obtain 659.01g of lithium concentrate clinker;
[0037] Step 4, sulfuric acid leaching: put the lithium concentrate clinker into a 3mol / L sulfuric acid solution for 5 hours, with a liquid-to-solid ratio of 2L / kg and a leaching temperature of 30°C, filter to obtain lithium-rich leaching solution and aluminum-silicon-rich leaching residue, then add 1200ml of hot water to wash the leaching residue, and reuse the obtained washing solution. The lithium leaching rate in this case is 96.93%, and the Li2O concentration of the leaching solution (lithium-rich leaching solution) is as high as 4.63g / L, and finally produces 583.78g of slag, of which 13.11g of gypsum (CaSO4·2H2O) is contained, accounting for 2.25%.
[0038] Example 2
[0039] The main minerals and contents of a clay-type lithium mine in Guizhou are: lithium chlorite (18.15%), quartz (26.04%), calcite (18.83%) and other minerals, among which the Li2O content is 0.56% and the CaO content is 23.64%. (Kong Lingan, Li Zhengyao, Zhong Zhenyu, et al. Ammonium sulfate roasting-acid leaching of lithium from clay-type lithium ore[J]. Nonferrous Metals Engineering, 2022, 12(12): 66-72.)
[0040] Step 1, grinding: Take 1000g of ore and grind it to a particle size of less than 0.074mm, accounting for 60.18%;
[0041] Step 2, chemical dissociation: add 5000 ml of 4 mol / L hydrochloric acid (HCl excess coefficient 2.37) to the sample in step 1, stir and react at 60° C. for 0.5 h, filter without washing, dry the leached residue obtained by decalcification, and obtain 586.42 g of lithium enriched product (Li2O content of 0.95%) with a lithium enrichment ratio of 1.7, wherein the lithium loss rate is less than 1%, and the calcium removal rate reaches 96.83%;
[0042] Step 3, roasting: the dissociated slag obtained in step 2 is roasted. Since the slag already contains chloride salt (2.04%) and residual acid (0.97%), it is only necessary to spread it evenly on the porcelain ark, put it into a muffle furnace heated to 400°C, and roast it for 1 hour. After the roasting is completed, the temperature is naturally cooled to room temperature to obtain 545.96g of lithium concentrate clinker;
[0043] Step 4, sulfuric acid leaching: react the lithium concentrate clinker in 1mol / L sulfuric acid solution for 0.5 hours, with a liquid-to-solid ratio of 6L / kg and a leaching temperature of 40°C, filter to obtain lithium-rich leaching solution and aluminum-silicon-rich leaching residue, then add 1500ml of hot water to wash the leaching residue, and reuse the obtained washing solution. In this case, the lithium leaching rate is 97.63%, and the Li2O concentration of the leaching solution is as high as 1.67g / L, and finally produces 469.14g of slag, of which 23.02g of gypsum is contained, accounting for 4.91%.
[0044] Example 3
[0045] The main minerals and contents of a clay-type lithium mine in Guizhou are: lithium chlorite (16.73%), quartz (21.15%), calcite (39.67%) and other minerals, among which the Li2O content is 0.51% and the CaO content is 29.71%.
[0046] Step 1, grinding: take 1000g of ore and grind it to a particle size of less than 0.074mm, accounting for 90.04%;
[0047] Step 2, chemical dissociation: add 2000 ml of 6 mol / L hydrochloric acid (HCl excess coefficient 1.13) to the sample in step 1, stir and react at 55° C. for 2 h, filter without washing, dry the leached residue obtained by decalcification, and obtain 552.18 g of lithium enriched product (Li2O content of 0.92%) with a lithium enrichment ratio of 1.8, wherein the lithium loss rate is less than 1%, and the calcium removal rate reaches 95.82%;
[0048] Step 3, roasting: the dissociated slag obtained in step 2 is roasted. Since the slag already contains chloride salt (0.68%) and residual acid (0.26%), it is only necessary to spread it evenly on the porcelain ark, put it into a muffle furnace heated to 550° C., and roast it for 0.5 hours. After the roasting is completed, the temperature is naturally cooled to room temperature to obtain 513.52 g of lithium concentrate clinker;
[0049] Step 4, sulfuric acid leaching: put the lithium concentrate clinker into a 0.5mol / L sulfuric acid solution, react for 3 hours under the conditions of a liquid-to-solid ratio of 8L / kg and a leaching temperature of 40°C, filter to obtain lithium-rich leaching solution and aluminum-silicon-rich leaching residue, then add 900ml of hot water to wash the leaching residue, and reuse the obtained washing solution. In this case, the lithium leaching rate is 97.18%, and the Li2O concentration of the leaching solution is as high as 1.21g / L, and finally 441.68g of slag is produced, of which 38.1g of gypsum is contained, accounting for 8.63%.
[0050] Example 4
[0051] A clay-type lithium mine, whose main minerals and contents are: lithium chlorite (14.21%), quartz (22.05%), calcite (42.01%) and other minerals, among which the Li2O content is 0.51% and the CaO content is 28.31%.
[0052] Step 1, grinding: take 1000g of ore and grind it to a particle size of less than 0.10mm, accounting for 68%;
[0053] Step 2, chemical dissociation: add 4000ml of 2.63mol / L hydrochloric acid (HCl excess coefficient 1.05) to the sample in step 1, stir and react at 35°C for 5h, filter without washing, dry the leached residue obtained by decalcification, the water content is less than 2.9%, and 581.86g of lithium enriched material (Li2O content is 0.83%) is obtained, and the lithium enrichment ratio is 1.84. The lithium loss rate is less than 1%, and the calcium removal rate reaches 94.99%;
[0054] Step 3, roasting: the dissociated slag obtained in step 2 is roasted, the slag contains chloride salt (0.51%) and residual acid (0.2%), and the slag is evenly spread on a porcelain ark, roasted at 600° C. for 2 hours, and naturally cooled to room temperature after roasting to obtain 539.97 g of lithium concentrate clinker;
[0055] Step 4, sulfuric acid leaching: put the lithium concentrate clinker into a 2mol / L sulfuric acid solution, leaching for 1 hour at a liquid-to-solid ratio of 3.5L / kg and a leaching temperature of 80°C, filter to obtain lithium-rich leaching solution and aluminum-silicon-rich leaching residue, then add 1000ml of hot water to wash the leaching residue, and reuse the obtained washing solution. In this case, the lithium leaching rate is 96.53%, the Li2O concentration of the leaching solution is as high as 2.3g / L, and 454.38g of slag is finally produced, of which 43.28g of gypsum is contained, accounting for 9.52%.
[0056] Example 5
[0057] A clay-type lithium ore, the main lithium mineral is lithium chlorite (14.83%), a small amount of lithium mica; calcite accounts for 26.72% of the ore. The clay-type lithium ore has a Li2O content of 0.58% and a CaO content of 16.74%.
[0058] Step 1, grinding: Take 1000g of ore and grind it until the particle size is less than 0.10mm, accounting for 85%;
[0059] Step 2, chemical dissociation: add the sample in step 1 to 2500 ml of 3.5 mol / L hydrochloric acid (HCl excess coefficient 1.46), stir and react at 45° C. for 3 h, filter without washing, dry the leached residue obtained by decalcification, and the water content is less than 3%, to obtain 681.8 g of lithium enriched material (Li2O content is 0.85%), the lithium enrichment ratio is 1.47, wherein the lithium loss rate is less than 1%, and the calcium removal rate reaches 96.08%;
[0060] Step 3, roasting: the dissociated slag obtained in step 2 is roasted. The slag contains chloride salt (0.78%) and residual acid (0.31%), so it only needs to be evenly spread on the porcelain ark and roasted at 650° C. for 2 hours. After the roasting is completed, the temperature is naturally cooled to room temperature to obtain 634.07g of lithium concentrate clinker;
[0061] Step 4, sulfuric acid leaching: put the lithium concentrate clinker into a 1.5mol / L sulfuric acid solution, leached for 2.5 hours at a liquid-solid ratio of 4L / kg and a leaching temperature of 55°C, filter to obtain lithium-rich leaching solution and aluminum-silicon-rich leaching residue, then add 850ml of hot water to wash the leaching residue, and reuse the obtained washing solution. In this case, the lithium leaching rate is 96.87%, the Li2O concentration of the leaching solution is as high as 2.22g / L, and finally 545.44g of slag is produced, of which 20.15g of gypsum is contained, accounting for 3.4%.
[0062] Comparative Example 1 (the difference from Example 3 is that no chemical dissociation step is performed)
[0063] Using the same clay-type lithium ore in Guizhou as in Example 3, the process steps are as follows:
[0064] Step 1, grinding: take 1000g of ore and grind it to a particle size of less than 0.074mm, accounting for 90.04%;
[0065] Step 2, roasting: the ground ore is evenly spread on the porcelain ark, placed in a muffle furnace heated to 550°C, roasted for 0.5 hours, and naturally cooled to room temperature after roasting to obtain lithium concentrate clinker;
[0066] Step 3, sulfuric acid leaching: put the lithium concentrate clinker into a 1.5mol / L sulfuric acid solution, react for 3 hours under the conditions of a liquid-to-solid ratio of 8L / kg and a leaching temperature of 90°C (Note, this comparative example adds more sulfuric acid than Example 3 for full dissociation, because this comparative example does not have a hydrochloric acid dissociation step), filter to obtain lithium-rich leachate and aluminum-silicon leach residue, then add 900ml of hot water to wash the leach residue, and the obtained washing solution is reused. The lithium leaching rate under this condition is 87.49%. However, the Li2O concentration of the leachate under this condition is only 0.53g / L, and 1637.5g of slag is finally produced, of which 912.5g of gypsum is contained, accounting for 55.73%.
[0067] Comparative Example 2 (the difference from Example 5 is that no chemical dissociation step is performed)
[0068] Using the same clay-type lithium ore from Guizhou as in Example 5, the process steps are as follows:
[0069] Step 1, grinding: Take 1000g of ore and grind it until the particle size is less than 0.10mm, accounting for 85%;
[0070] Step 2, roasting: the ground ore is evenly spread on the porcelain ark, placed in a muffle furnace heated to 650°C, roasted for 2 hours, and naturally cooled to room temperature after roasting to obtain lithium concentrate clinker;
[0071] Step 3, sulfuric acid leaching: put the lithium concentrate clinker into a 1.5mol / L sulfuric acid solution, leached for 2.5 hours under the conditions of a liquid-to-solid ratio of 6L / kg and a leaching temperature of 90°C (Note, this comparative example adds more sulfuric acid than Example 5 for full dissociation, because this comparative example does not have a hydrochloric acid dissociation step), filter to obtain lithium-rich leachate and aluminum-silicon leach residue, then add 850ml of hot water to wash the leach residue, and the obtained washing solution is reused. The lithium leaching rate under this condition is 89.09%. However, the Li2O concentration of the leachate under this condition is only 0.82g / L, and 1248.05g of slag is finally produced, which contains 514.1g of gypsum, accounting for 41.19%.
[0072] Comparative Example 3 (the difference from Example 2 is that washing was performed)
[0073] Using the same clay-type lithium ore in Guizhou as in Example 2, the process steps are as follows:
[0074] Step 1, grinding: Take 1000g of ore and grind it to a particle size of less than 0.074mm, accounting for 60.18%;
[0075] Step 2, chemical dissociation: add 5000 ml of 4 mol / L hydrochloric acid (HCl excess coefficient 2.37) to the sample in step 1, stir and react at 60° C. for 0.5 h, filter and wash, dry the leached residue obtained by decalcification, the water content is less than 2.3%, the chloride content in the dissociated residue is less than 0.1%, and the residual acid content is less than 0.01%;
[0076] Step 3, roasting: roasting the dissociated slag obtained in step 2, spreading it evenly on a porcelain ark, placing it in a muffle furnace heated to 400° C., and roasting it blank for 1 hour. After the roasting is completed, the temperature is naturally lowered to room temperature to obtain lithium concentrate clinker;
[0077] Step 4, sulfuric acid leaching: react the lithium concentrate clinker in 1 mol / L sulfuric acid solution for 0.5 hours, with a liquid-to-solid ratio of 6L / kg and a leaching temperature of 40°C, filter to obtain lithium-rich leaching solution and aluminum-silicon leaching residue, then add 1500ml of hot water to wash the leaching residue, and reuse the obtained washing solution. The lithium leaching rate under this condition is 89.74%, and the Li2O concentration of the leaching solution is only 1.46g / L, and finally 488.62g of slag is produced, of which 24.04g of gypsum is contained, accounting for 4.92%.
[0078] Comparative Example 4 (the difference from Comparative Example 3 is that the roasting temperature and time are increased)
[0079] Using the same clay-type lithium ore in Guizhou as in Example 2, the process steps are as follows:
[0080] Step 1, grinding: Take 1000g of ore and grind it to a particle size of less than 0.074mm, accounting for 60.18%;
[0081] Step 2, chemical dissociation: add 5000 ml of 4 mol / L hydrochloric acid (HCl excess coefficient 2.37) to the sample in step 1, stir and react at 60° C. for 0.5 h, filter and wash, dry the leached residue obtained by decalcification, the water content is less than 2.3%, the chloride content in the dissociated residue is less than 0.1%, and the residual acid content is less than 0.01%;
[0082] Step 3, roasting: the dissociated slag obtained in step 2 is roasted, evenly spread on a porcelain ark, placed in a muffle furnace heated to 700°C, and blank roasted for 3 hours. After the roasting is completed, the temperature is naturally cooled to room temperature to obtain lithium concentrate clinker;
[0083] Step 4, sulfuric acid leaching: react the lithium concentrate clinker in 1 mol / L sulfuric acid solution for 0.5 hours, with a liquid-to-solid ratio of 6L / kg and a leaching temperature of 40°C, filter to obtain lithium-rich leaching solution and aluminum-silicon leaching residue, then add 1500ml of hot water to wash the leaching residue, and reuse the obtained washing solution. The lithium leaching rate under this condition is 96.34%, and the Li2O concentration of the leaching solution is only 1.65g / L, and finally 469.23g of slag is produced, of which 23.03g of gypsum is contained, accounting for 4.91%.
[0084] For the convenience of comparison, the applicant organizes the main data involved in the above embodiments and comparative examples into the following table:
[0085] Table 1: Main chemical composition of high calcium clay lithium ore / %
[0086] index <![CDATA[Li2O]]> <![CDATA[K2O]]> MgO CaO TFe <![CDATA[SiO2]]> <![CDATA[Al2O3]]> Example 1 0.63 0.69 0.25 11.92 4.13 39.01 20.14 Example 2 0.56 1.63 0.38 23.64 4.24 40.07 20.85 Example 3 0.51 0.98 0.28 29.71 4.31 39.58 20.21 Example 4 0.45 0.87 0.31 28.13 4.19 40.12 20.32 Example 5 0.58 0.75 0.29 16.74 4.19 39.28 20.18
[0087] Table 2: Main data parameters of Examples 1-5
[0088]
[0089] As can be seen from the above table, after chemical dissociation, dissociation slag ranging from about 25% to 70% is obtained. Therefore, the chemical dissociation step can reduce the amount of roasting materials in the subsequent steps by 75% to 30%. Therefore, the amount of material for subsequent processing is less, and the required energy consumption and dosage of reagents are less; and chemical dissociation can remove more than 94.5% of calcium elements, greatly reducing the production of subsequent sulfuric acid leaching gypsum, so the amount of waste slag in the by-product is less.
[0090] Table 3: Main data parameters of Comparative Examples 1-4, Examples 2, 3, and 5
[0091]
[0092] As can be seen from the above table, the difference between Comparative Example 1 and Comparative Example 2, respectively, compared with Example 3 and Example 5, is that the chemical dissociation step is not performed. The experimental data show that not only the leaching rate and leaching concentration of lithium are significantly reduced, but also a large amount of gypsum is produced; the difference between Comparative Example 3 and Example 2 is that filtering and washing are performed, and the leaching rate of lithium is greatly reduced, indicating that without washing and filtering, retaining chloride salt and residual acid can improve the leaching rate of lithium, and the concentration of the leachate is also improved to a certain extent. Compared with Example 2, the difference between Comparative Example 4 and Example 2 is that filtering and washing are performed in the comparative example, and the roasting temperature and time are increased, and the effect is similar. It can be seen that without washing and filtering, the effect of reducing the roasting temperature and time can be reduced.
[0093] The above is only a preferred embodiment of the present invention. It should be understood that the present invention is not limited to the form disclosed herein, and should not be regarded as excluding other embodiments, but can be used in various other combinations, modifications and environments, and can be modified within the scope of the concept described herein through the above teachings or the technology or knowledge of the relevant field. The changes and modifications made by those skilled in the art shall not deviate from the spirit and scope of the present invention, and shall be within the scope of protection of the claims attached to the present invention.
Claims
1. A method for extracting lithium from high-calcium clay-type lithium ore, characterized in that: The following steps are involved: S1. Grinding: Grind the high calcium clay-type lithium ore to -0.074mm, accounting for 60%-90%; Wherein, the Li2O content in the high calcium clay-type lithium ore is less than 1%, and the CaO content is 10%-30%; S2, chemical dissociation: adding the ground high calcium clay-type lithium ore to hydrochloric acid for chemical dissociation, filtering the dissociation residue obtained by chemical dissociation without washing, and then drying, with a water content of less than 3%; The concentration of the hydrochloric acid is 1-6 mol / L, the liquid-solid ratio of chemical dissociation is 2-8 L / kg, the excess coefficient of the hydrochloric acid is 1-2.5, the time is 0.5-5 h, the dissociation temperature is 20-60 ° C, and the chloride ion content of the high calcium clay-type lithium ore after unwashing and drying is 0.5-3%, and the residual acid content is 0.2-1.2%; The non-washing filtration refers to filtering the dissociation residue without washing with water, so that part of the chlorine radical and residual acid are retained in the dissociation residue; S3, roasting: roasting the dried dissociated slag to obtain clinker, the roasting temperature is 400-650°C, and the time is 0.5-2.0h; S4, sulfuric acid leaching: putting the clinker into a sulfuric acid solution for leaching reaction, and filtering to obtain a lithium-rich leaching solution and an aluminum-silicon-rich leaching residue; The concentration of the sulfuric acid solution is 0.5-3 mol / L, the liquid-solid ratio of the leaching reaction is 2-8 L / kg, the time is 0.5-5 h, and the temperature is 30-90° C.
2. A method for extracting lithium from high-calcium clay-type lithium ore according to claim 1, characterized in that: In step S1, the high calcium clay-type lithium ore is ground to -0.074 mm, accounting for 75%-85%.
3. A method for extracting lithium from high-calcium clay-type lithium ore according to claim 1, characterized in that: In step S2, the concentration of the hydrochloric acid is 2-4 mol / L, the liquid-solid ratio of chemical dissociation is 4-6 L / kg, and the time is 2-4 h.
4. A method for extracting lithium from high-calcium clay-type lithium ore according to claim 1, characterized in that: In step S2, the chloride ion content of the high calcium clay-type lithium ore after unwashing and drying is 1.5-2.5%, and the residual acid content is 0.5-1%.
5. A method for extracting lithium from high-calcium clay-type lithium ore according to claim 1, characterized in that: In step S2, the drying temperature is lower than 110°C.
6. A method for extracting lithium from high-calcium clay-type lithium ore according to claim 1, characterized in that: In step S3, the calcination temperature is 500-600° C., and the calcination time is 1-1.5 hours.
7. A method for extracting lithium from high-calcium clay-type lithium ore according to claim 1, characterized in that: In step S4, the concentration of the sulfuric acid solution is 1.5-3 mol / L, the liquid-solid ratio of the leaching reaction is 4-6 L / kg, and the time is 2-4 h.
8. The method for extracting lithium from high-calcium clay-type lithium ore according to claim 1, characterized in that: In step S4, the filtering method is to use hot water for washing and filtering, and the amount of hot water used is 1.5-3 times the weight of the aluminum-silicon-rich leaching residue.
Citation Information
Cited By
Grinding and leaching integrated gradient lithium extraction method for clay type lithium ore
CN120006112A
Synergistic roasting-selective lithium extraction method for clay type lithium ore and waste lithium iron phosphate
CN121362886A