A test method for tensile resilience modulus of asphalt mixture

By cutting and adjusting the specimen size, and using centering devices and tensile components, the tensile strength and resilience modulus testing process of asphalt mixtures is simplified, solving the problems of complexity and low accuracy of existing testing methods, and achieving Get fast and accurate test results.

CN117330408BActive Publication Date: 2024-10-18FOSHAN TRANSPORTATION SCI & TECH CO LTD +1
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
CN202311064814.7
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-08-22
Publication Date
2024-10-18
Estimated Expiration
2043-08-22

AI Technical Summary

Technical Problem

The existing testing methods for the tensile strength and tensile resilience modulus of asphalt mixtures are complex and cumbersome, making it difficult to obtain results quickly and accurately, and there are significant differences in the test results, which affects the accuracy of the evaluation.

Method used

By cutting the test piece into several pieces to be tested and adjusting the size, using a centering device to fix the piece to be tested on the mounting plate, connecting the tensile component and the main shaft of the material testing machine, gradually adding load and recording the peak load and rebound displacement data. Calculate the tensile strength and tensile resilience modulus values ​​to ensure that the test piece is stressed at the same position.

Benefits of technology

The test process is simplified, the accuracy and consistency of test results are improved, and the evaluation accuracy of asphalt mixture is ensured.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN117330408B_ABST
    Figure CN117330408B_ABST
Patent Text Reader

Abstract

The present invention relates to the field of civil engineering experimental technology. Specifically, the present invention discloses a method for testing the tensile resilience modulus of asphalt mixture, including: cutting a test piece into a plurality of test pieces according to test requirements, and adjusting the size of the test pieces; measuring various physical indicators of the test pieces, and fixing the test pieces on a mounting plate by a centering device; connecting an upper tensile assembly to a main shaft of a material testing machine, and connecting a locking plate of a lower tensile assembly to the mounting plate, and contacting the lower tensile assembly with an upper tensile assembly; driving the main shaft of the material testing machine to move upward at a first rate; driving the main shaft of the material testing machine to move upward at a second rate; determining the loading level according to the peak load of the test piece, driving the main shaft of the material testing machine to move upward at a first rate, and sequentially loading and unloading each level of load on the basis of the preload tension. The present invention has the advantages of simple testing and accurate test results.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of civil engineering experiments, and in particular to a method for testing the tensile resilience modulus of an asphalt mixture. Background Art

[0002] In order to accurately reflect the anti-destruction and anti-deformation capabilities of the asphalt pavement, technicians need to accurately obtain the tensile strength and rebound modulus of the asphalt mixture.

[0003] Furthermore, the "Testing Procedures for Asphalt and Asphalt Mixtures in Highway Engineering" (JTG E20-2011) also indicates that the tensile strength and tensile resilience modulus of asphalt mixtures are important indicators for the design of asphalt pavement structures, and provides a uniaxial compression strength test method for asphalt mixtures. Specifically, the procedure indicates that the test specimen is a cylindrical specimen with a diameter of 100mm and a height of 100mm, a loading rate of 2mm / min, and a test temperature of 15℃ or 20℃. The test method is divided into two parts: the first part is the uniaxial compression strength test, and the second part is the uniaxial compression resilience modulus test.

[0004] However, the existing testing methods are too complicated and cumbersome, making it difficult to simply, quickly and accurately obtain the tensile strength and tensile resilience modulus of asphalt mixtures, which greatly reduces the testing efficiency and also has the problem of low testing accuracy.

[0005] Furthermore, using existing testing methods, it is difficult to ensure that all test pieces are stretched at the same position, resulting in significant differences in the tensile strength and tensile resilience modulus obtained even under the same test conditions. This in turn causes the obtained uniaxial tensile strength and uniaxial tensile resilience modulus to be inaccurate, greatly affecting the evaluation accuracy of the asphalt mixture. Summary of the invention

[0006] The technical problem to be solved by the present invention is to provide a method for testing the tensile resilience modulus of asphalt mixture, which is simple and convenient to test and ensures accurate test results.

[0007] In order to solve the above technical problems, the present invention provides a method for testing the tensile resilience modulus of asphalt mixture, comprising:

[0008] According to the test requirements, the test piece is cut into several pieces to be tested and the sizes of the pieces to be tested are adjusted;

[0009] Measure various physical indicators of the test piece, and fix the test piece on the mounting plate by centering the centering device;

[0010] Connecting the upper tensile assembly to the main shaft of the material testing machine, connecting the locking plate of the lower tensile assembly to the mounting plate, and bringing the lower tensile assembly into contact with the upper tensile assembly;

[0011] The main shaft of the driving material testing machine performs a pre-contact process and connects the lower tensile assembly with the upper tensile assembly using screws;

[0012] driving the main shaft of the material testing machine to move upward at a first rate to apply a tensile force to the test piece until the test piece is damaged, and recording a peak load of the test piece to obtain a tensile strength of the test piece;

[0013] Replace the test piece, and drive the main shaft of the material testing machine to move upward at a second speed to preload the tensile force on the test piece;

[0014] The loading level is determined according to the peak load of the test piece, and the main shaft of the material testing machine is driven to move upward at a first rate. Each level of load is loaded and unloaded in sequence based on the preload tension, and the tensile displacement data and rebound displacement data of the test piece under each level of load are recorded in sequence to obtain the tensile rebound modulus value of the test piece.

[0015] Preferably, the step of cutting the test piece into a plurality of pieces to be tested and adjusting the sizes of the pieces to be tested according to the test requirements comprises:

[0016] Cut the test piece into a preset number of pieces to be tested;

[0017] Performing a rotational shearing and pressing process on the piece to be tested, adjusting the diameter of the piece to be tested to a first preset diameter, and adjusting the height of the piece to be tested to a first preset height;

[0018] After the rotary shearing and pressing process is completed, the workpiece to be tested is double-sided cut and double-sided flattened, the diameter of the workpiece to be tested is adjusted to a second preset diameter, and the height of the workpiece to be tested is adjusted to a second preset height.

[0019] Preferably, the step of centering and fixing the workpiece to be tested on the mounting plate by the centering device comprises:

[0020] Place one of the mounting plates in the base of the centering device, lift the upper pull rod of the centering device, and place the other mounting plate in the upper slot of the upper pull rod;

[0021] Apply the adhesive evenly on the surface of the mounting plate and both ends of the test piece, and place the test piece on one of the mounting plates located on the base of the centering device;

[0022] Lock the lateral restraints of the centering device to center the workpiece to be tested, and lower the upper pull rod to allow the other mounting plate to bond with the workpiece to be tested;

[0023] After the adhesive is cured, lift the upper pull rod and take out the test piece, and place the test piece in the environmental chamber until the temperature of the test piece reaches the test temperature.

[0024] Preferably, the step of driving the main shaft of the material testing machine to perform a pre-contact process and simultaneously connecting the lower tensile assembly with the upper tensile assembly using screws comprises:

[0025] Drive the spindle of the material testing machine to move upward and return to its original position;

[0026] The main shaft of the material testing machine is driven to move downward at a second speed, so that the connecting head of the upper tensile assembly applies pressure to the test piece via the locking plate of the lower tensile assembly, and the lower tensile assembly is connected to the upper tensile assembly by screws;

[0027] After the connection is completed, the main shaft of the material testing machine is driven to move upward at a second rate so that the connection head of the upper tensile assembly is away from the locking disk of the lower tensile assembly.

[0028] Preferably, the steps of driving the main shaft of the material testing machine to move upward at a first rate, and sequentially loading and unloading various levels of loads on the basis of the preload tension include:

[0029] The main shaft of the material testing machine is driven to move upward at a first rate, and the load is loaded to a target load on the basis of the preload tension. Then, the main shaft of the material testing machine is driven to move downward at a first rate, and the load is unloaded from the target load to the preload tension. The tensile displacement data and the rebound displacement data of the target load are recorded according to the displacement sensor on the test piece.

[0030] After waiting for a preset time, the main shaft of the material testing machine is driven to move upward at a first rate, and loaded to the next target load on the basis of the preload tension. Then, the main shaft of the material testing machine is driven to move downward at the first rate, and unloaded from the next target load to the preload tension. The tensile displacement data and rebound displacement data of the next target load are recorded according to the displacement sensor on the test piece.

[0031] Preferably, the method further comprises the following steps:

[0032] After determining the loading level, the spindle of the material testing machine is driven to move upward at a second rate, and loaded to a preset multiple of the peak load on the basis of the preload tension. Then, the spindle of the material testing machine is driven to move downward at a second rate, and unloaded from the preset multiple of the peak load to the preload tension. The preload displacement data and preload rebound displacement data are recorded according to the displacement sensor on the test piece.

[0033] Preferably, the method further comprises the following steps:

[0034] After measuring the various physical indicators of the test piece, the mounting pins are pasted to the surface of the test piece at intervals along the circumference of the test piece by a pneumatic pasting device;

[0035] The upper support member and the lower support member are respectively connected to the mounting nails, and are respectively fixed to the two ends of the guide rod of the displacement sensor through the upper support member and the lower support member, so as to fix the displacement sensor on the test piece.

[0036] Preferably, the step of recording the peak load of the test piece to obtain the tensile strength of the test piece comprises:

[0037] According to the function R = 4P / πd 2 , determine the tensile strength R of the test piece, where P is the peak load and d is the diameter of the test piece;

[0038] The step of obtaining the tensile modulus of elasticity of the test piece comprises:

[0039] According to the function E=h / k, the tensile elastic modulus of the test piece under each level of load is determined, where h is the height of the test piece and k is the slope of the linear curve of each level of load and rebound displacement data;

[0040] The average value of the tensile elastic modulus of the test piece under the third-level load, the fourth-level load, and the fifth-level load is taken as the tensile elastic modulus value.

[0041] Preferably, the method further comprises the following steps:

[0042] Calculate the standard deviation of the tensile modulus of elasticity of the test pieces, and determine whether the difference between the tensile modulus of elasticity of each test piece and the average tensile modulus of elasticity of the test pieces is greater than the standard deviation multiplied by the slope k;

[0043] If the answer is yes, the tensile modulus of elasticity of the test piece is discarded;

[0044] If the judgment is no, the tensile modulus value of the tested piece is retained;

[0045] According to the tensile elastic modulus values ​​of the other test pieces, the tensile elastic modulus value for pavement design is obtained.

[0046] Preferably, the step of obtaining the tensile modulus of resilience value for pavement design according to the tensile modulus of resilience values ​​of the remaining test pieces comprises:

[0047] According to the function Determine the tensile modulus of resilience value Em for pavement design, where E* is the average tensile modulus of resilience of the remaining test pieces, S is the standard deviation of the tensile modulus of resilience of the remaining test pieces, n is the valid number of test pieces, and t is the guarantee rate coefficient.

[0048] The implementation of the present invention has the following beneficial effects:

[0049] According to the test requirements, the present invention cuts the test piece into several test pieces and adjusts the sizes of the test pieces to test the tensile strength and tensile elastic modulus values ​​respectively;

[0050] Next, the density, porosity and other physical indicators of the test piece are measured, and the test piece is fixed on the mounting plate by the centering device so that the mounting plate can remain parallel and bonded to the test piece in a vertically aligned manner to avoid eccentric force during the stretching process; at the same time, by vertically aligning the mounting plate and the test piece, it can be ensured that each test piece is stretched at the same position, ensuring accurate test results.

[0051] Subsequently, the upper tensile assembly is connected to the main shaft of the material testing machine, and the locking plate of the lower tensile assembly is connected to the mounting plate, and the lower tensile assembly is brought into contact with the upper tensile assembly. The detachable tensile assembly enables the staff to connect the lower tensile assembly with the upper tensile assembly after completing the centering of the workpiece to be tested, so as to facilitate the installation and centering of the workpiece to be tested.

[0052] Subsequently, the spindle of the driving material testing machine is subjected to a pre-contact process to eliminate the initial installation stress, and the lower tensile assembly is connected to the upper tensile assembly using screws;

[0053] After completion, the tensile strength test of the test piece can be carried out, and the main shaft of the material testing machine is driven to move upward at a first rate to apply tensile force to the test piece until the test piece is broken, and the peak load of the test piece is recorded to obtain the tensile strength of the test piece;

[0054] After obtaining the peak load of the test piece, the uniaxial tensile resilience modulus test of the test piece can be performed. First, the test piece damaged in the previous tensile strength test is replaced, and the main shaft of the material testing machine is driven to move upward at the second rate to preload the tensile force on the test piece;

[0055] Subsequently, the loading level is determined according to the peak load of the test piece, and the main shaft of the material testing machine is driven to move upward at a first rate. The loads of each level are loaded and unloaded in sequence on the basis of the preload tension, and the tensile displacement data and rebound displacement data of the test piece under each level of load are recorded in sequence to obtain the tensile rebound modulus value of the test piece. The test is simple and the test results are accurate.

[0056] It should be noted that the present invention uses a centering device so that the mounting plate can remain parallel and bonded to the workpiece to be tested in a vertically aligned manner, thereby avoiding eccentric force during the stretching process; at the same time, by vertically aligning the mounting plate with the workpiece to be tested, it can be ensured that each workpiece to be tested is stretched at the same position, thereby ensuring accurate test results.

[0057] Furthermore, the present invention makes the stretching assembly detachable, so that the staff can connect the lower stretching assembly and the upper stretching assembly after completing the alignment of the test piece, so as to facilitate the installation and alignment of the test piece and eliminate the initial installation stress, thereby further ensuring the accuracy of the test results. BRIEF DESCRIPTION OF THE DRAWINGS

[0058] Figure 1 It is a schematic flow chart of a preferred embodiment of a method for testing the tensile resilience modulus of asphalt mixture of the present invention;

[0059] Figure 2 It is a schematic diagram of the process of adjusting the size of the piece to be tested according to the present invention;

[0060] Figure 3 It is a schematic diagram of the process of centering and fixing the workpiece to be tested on the mounting plate by the centering device of the present invention;

[0061] Figure 4 It is a schematic diagram of the process of installing the displacement sensor on the object to be tested according to the present invention;

[0062] Figure 5 It is a schematic flow diagram of the pre-contacting process of the present invention;

[0063] Figure 6 It is a schematic diagram of the process of obtaining tensile displacement data and rebound displacement data in the present invention. DETAILED DESCRIPTION

[0064] In order to make the purpose, technical solution and advantages of the present invention clearer, the present invention will be further described in detail below with reference to the accompanying drawings. It is hereby stated that the directional terms such as up, down, left, right, front, back, inside, outside, etc. that appear or will appear in the text of the present invention are only based on the accompanying drawings of the present invention, and are not specific limitations of the present invention.

[0065] Combination Figures 1 to 6 One embodiment of the present invention provides a method for testing the tensile resilience modulus of asphalt mixture, comprising:

[0066] S1. According to the test requirements, the test piece is cut into several test pieces, and the sizes of the test pieces are adjusted to test the tensile strength and tensile elastic modulus values ​​respectively;

[0067] S2. Determine the density, porosity and other physical indicators of the test piece, and fix the test piece on the mounting plate through the centering device, so that the mounting plate can remain parallel and bonded to the test piece in a vertically centered manner to avoid eccentric force during the stretching process; at the same time, by vertically aligning the mounting plate and the test piece, it can be ensured that each test piece is stretched at the same position, ensuring accurate test results.

[0068] S3, connecting the upper tensile assembly to the main shaft of the material testing machine, and connecting the locking plate of the lower tensile assembly to the mounting plate, and making the lower tensile assembly contact with the upper tensile assembly. By making the tensile assembly detachable, the staff can connect the lower tensile assembly with the upper tensile assembly after completing the centering of the workpiece to be tested, so as to facilitate the installation and centering of the workpiece to be tested;

[0069] S4, driving the spindle of the material testing machine to perform a pre-contact process to eliminate the initial installation stress, and connecting the lower tensile assembly with the upper tensile assembly using screws;

[0070] S5, driving the main shaft of the material testing machine to move upward at a first rate to apply a tensile force to the test piece until the test piece is damaged, and recording the peak load of the test piece to obtain the tensile strength of the test piece;

[0071] S6, replacing the test piece that was damaged in the previous tensile strength test, and driving the main shaft of the material testing machine to move upward at a second rate to preload the tensile force on the test piece;

[0072] S7. Determine the loading level according to the peak load of the test piece, drive the main shaft of the material testing machine to move upward at a first rate, load and unload each level of load in sequence based on the preload tension, and record the tensile displacement data and rebound displacement data of the test piece under each level of load in sequence to obtain the tensile rebound modulus value of the test piece. The test is simple and the test result is accurate.

[0073] It should be noted that the present invention uses a centering device to keep the mounting plate parallel and vertically aligned with the test piece to avoid eccentric force during the stretching process; at the same time, by vertically aligning the mounting plate with the test piece, it can ensure that each test piece is stretched at the same position, ensuring accurate test results. The first rate is 2mm / min and the second rate is 0.5mm / min.

[0074] Furthermore, the present invention makes the stretching assembly detachable, so that the staff can connect the lower stretching assembly and the upper stretching assembly after completing the alignment of the test piece, so as to facilitate the installation and alignment of the test piece and eliminate the initial installation stress, thereby further ensuring the accuracy of the test results.

[0075] Further, combined with Figure 2 The step of cutting the test piece into a plurality of test pieces and adjusting the size of the test pieces according to the test requirements includes:

[0076] S11, cutting the test piece into a preset number of test pieces to ensure the number of test pieces for the tensile strength test and the tensile elastic modulus test;

[0077] S12, performing a rotational shearing and pressing process on the workpiece to be tested, adjusting the diameter of the workpiece to be tested to a first preset diameter, and adjusting the height of the workpiece to be tested to a first preset height;

[0078] S13, after the rotary shearing and pressing process is completed, the workpiece to be tested is double-sided cut and double-sided flattened, the diameter of the workpiece to be tested is adjusted to a second preset diameter, and the height of the workpiece to be tested is adjusted to a second preset height.

[0079] As one of the embodiments, the test piece can be cut into 3-5 test pieces; when the test pieces are subjected to rotational shearing and pressing treatment, the diameter of the test pieces is adjusted to 140-150 mm, and the height of the test pieces is adjusted to 140-150 mm; after the rotational shearing and pressing treatment, the test pieces are double-sided cut and double-sided flattened, and the diameter of the test pieces is adjusted to 100 mm ± 2 mm, and the height of the test pieces is adjusted to 100 ± 1 mm.

[0080] It should be noted that the flatness and levelness of the two end surfaces of the test piece have a great influence on the test results of the tensile rebound modulus, so it is necessary to ensure that the height difference of the test piece after grinding does not exceed 2mm.

[0081] Preferably, combined Figure 3 The steps of centering and fixing the workpiece to be tested on the mounting plate by the centering device include:

[0082] S21, placing one of the mounting plates in the base of the centering device, lifting the upper pull rod of the centering device, and placing the other mounting plate in the upper slot of the upper pull rod;

[0083] S22, evenly apply the adhesive on the surface of the mounting plate and both ends of the test piece, and place the test piece on one of the mounting plates located on the base of the centering device;

[0084] S23, locking the lateral restraint of the centering device to center the workpiece to be tested, and lowering the upper pull rod to allow the other mounting plate to bond with the workpiece to be tested;

[0085] S24. After the adhesive is cured, lift the upper pull rod and take out the test piece, and place the test piece in the environmental chamber until the temperature of the test piece reaches the test temperature.

[0086] It should be noted that the lateral restraint of the centering device is locked to center the test piece and prevent the test piece from deviating during the curing process, and the upper pull rod is lowered to bond the other mounting plate to the test piece, so that under the gravity of the upper pull rod and the lateral restraint, the test piece and each mounting plate are tightly fitted to form a whole. The adhesive can be a polyurethane two-component adhesive, and 100g of the polyurethane two-component adhesive is weighed on a scale, fully mixed, and evenly applied to the surface of the mounting plate and both ends of the test piece.

[0087] Preferably, combined with Figure 5 The step of driving the spindle of the material testing machine to perform a pre-contact process and connecting the lower tensile component with the upper tensile component using screws includes:

[0088] S41, driving the main axis of the material testing machine to move upward and return to its original position;

[0089] S42, driving the main shaft of the material testing machine to move downward at a second rate, so that the connecting head of the upper tensile assembly applies pressure to the test piece via the locking plate of the lower tensile assembly, and connecting the lower tensile assembly and the upper tensile assembly with screws;

[0090] S43, after the connection is completed, the main shaft of the material testing machine is driven to move upward at a second rate so that the connecting head of the upper tensile assembly is away from the locking disk of the lower tensile assembly.

[0091] It should be noted that the material testing machine can use UTM-30, which drives the spindle of the material testing machine to move upward and return to its original position to ensure that the spindle has no contact with the installed workpiece to be tested. Furthermore, when the spindle of the material testing machine is driven to move downward at the second rate, the pressure applied to the workpiece to be tested is 50N, which can be observed through the force sensor of the material testing machine. Furthermore, when using screws to connect the lower tensile assembly and the upper tensile assembly, they should be tightened synchronously to avoid tightening one of the bolts and then tightening the next one, which will cause uneven force on the workpiece to be tested. In addition, when the spindle of the material testing machine is driven to move upward at the second rate, the force sensor of the material testing machine is cleared to ensure accurate test results.

[0092] On the other hand, combined Figure 6 In order to accurately obtain tensile displacement data and rebound displacement data, the spindle of the driving material testing machine moves upward at a first rate, and the steps of sequentially loading and unloading various levels of loads on the basis of the preload tension include:

[0093] S71, driving the main shaft of the material testing machine to move upward at a first rate, loading the load to a target load on the basis of the preload tension, then driving the main shaft of the material testing machine to move downward at the first rate, unloading the load from the target load to the preload tension, and recording the tensile displacement data and the rebound displacement data of the target load according to the displacement sensor on the test piece;

[0094] S72, after waiting for a preset time, drive the main shaft of the material testing machine to move upward at a first rate, load to the next target load on the basis of the preload tension, then drive the main shaft of the material testing machine to move downward at the first rate, unload from the next target load to the preload tension, and record the tensile displacement data and rebound displacement data of the next target load according to the displacement sensor on the test piece.

[0095] It should be noted that the load levels include level 1 load 0.1P, level 2 load 0.2P, level 3 load 0.3P, level 4 load 0.4P, level 5 load 0.5P, and level 6 load 0.6P, where P is the peak load;

[0096] As one of the embodiments, the main shaft of the material testing machine is driven to move upward at a first rate, and a primary load of 0.1P is loaded on the basis of a preload tension of 100N, and the main shaft of the material testing machine is driven to move downward at a first rate, and the primary load of 0.1P is unloaded to a preload tension of 100N;

[0097] Wait for 30 seconds to allow the test piece to rebound and deform, and then carry out the loading and unloading process of the second, third, ... sixth level loads in sequence. After each unloading to 100N, wait for the sample to rebound and deform for 30 seconds before starting the next level of load loading.

[0098] Furthermore, during the loading and unloading process, a displacement sensor attached to the test piece can be used to record the deformation of the sample in the height direction. The difference between the displacement when loaded to the peak value of each load level and the displacement after rebounding 30s after unloading to 100N is taken as the rebound deformation under this load level.

[0099] Furthermore, in order to quickly determine whether the test result is valid and further ensure the test accuracy, the present invention also includes the following steps:

[0100] S73, determining whether the tensile displacement data of the sixth level load is greater than the rebound displacement data;

[0101] If the judgment is yes, the test result is valid;

[0102] If the judgment is no, the test result is invalid.

[0103] Preferably, to realize the preloading function, the present invention further comprises the following steps:

[0104] After the loading level is determined, the spindle of the material testing machine is driven to move upward at the second rate, and the load is loaded to a preset multiple of the peak load on the basis of the preload tension, and then the spindle of the material testing machine is driven to move downward at the second rate, and the load is unloaded from the preset multiple of the peak load to the preload tension, and the preload displacement data and preload rebound displacement data are recorded according to the displacement sensor on the test piece. Among them, the preset multiple can be 0.2 times.

[0105] In addition, combined Figure 4 In order to realize the function of accurately detecting the tensile displacement data and rebound displacement data of the test piece by the displacement sensor, the present invention also includes the following steps:

[0106] S25, after measuring various physical indicators of the test piece, the mounting pins are pasted to the surface of the test piece at intervals along the circumference of the test piece by a pneumatic pasting device;

[0107] S26, connecting the upper support member and the lower support member to the mounting nails respectively, and fixing them to the two ends of the guide rod of the displacement sensor through the upper support member and the lower support member respectively, and fixing the displacement sensor on the test piece.

[0108] It should be noted that the upper support member and the lower support member are respectively fixed to the two ends of the guide rod of the displacement sensor, so that the upper support member and the lower support member are vertically aligned, and during the loading process, the vertical deviation of the upper support member and the lower support member is limited to ensure the accuracy of the vertical deformation value collection.

[0109] In addition, in order to obtain the tensile strength of the test piece, the step of recording the peak load of the test piece to obtain the tensile strength of the test piece includes:

[0110] According to the function R = 4P / πd 2 , determine the tensile strength R of the test piece, where P is the peak load and d is the diameter of the test piece;

[0111] The step of obtaining the tensile modulus of elasticity of the test piece comprises:

[0112] According to the function E=h / k, the tensile elastic modulus of the test piece under each level of load is determined, where h is the height of the test piece and k is the slope of the linear curve of each level of load and rebound displacement data;

[0113] It should be noted that the average value of the tensile elastic modulus of the test piece under the third-level load, the fourth-level load, and the fifth-level load is taken as the tensile elastic modulus value to ensure the accuracy of the test results.

[0114] Further, combine again Figure 6 To further ensure the accuracy of the test results, the present invention further includes the following steps:

[0115] S74, calculating the standard deviation of the tensile modulus of elasticity of the test pieces, and determining whether the difference between the tensile modulus of elasticity of each test piece and the average tensile modulus of elasticity of the test pieces is greater than the standard deviation multiplied by the slope k;

[0116] If the answer is yes, the tensile modulus of elasticity of the test piece is discarded;

[0117] If the judgment is no, the tensile modulus value of the tested piece is retained;

[0118] S75. Obtain a tensile elastic modulus value for road surface design based on the tensile elastic modulus values ​​of the remaining test pieces.

[0119] Furthermore, the step of obtaining the tensile modulus of resilience value for pavement design according to the tensile modulus of resilience values ​​of the remaining test pieces includes:

[0120] According to the function Determine the tensile modulus of resilience value Em for pavement design, where E* is the average tensile modulus of resilience of the remaining test pieces, S is the standard deviation of the tensile modulus of resilience of the remaining test pieces, n is the valid number of test pieces, and t is the guarantee rate coefficient.

[0121] It should be noted that t varies with the guarantee rate, and The values ​​are listed in the following table:

[0122]

[0123]

[0124] It should be noted that the guarantee rate for expressways and first-class highways is 95%, and the guarantee rate for other grades of highways is 90%.

[0125] The above is a preferred embodiment of the present invention. It should be pointed out that a person skilled in the art can make several improvements and modifications without departing from the principle of the present invention. These improvements and modifications are also considered to be within the scope of protection of the present invention.

Claims

1. A method for testing the tensile modulus of elasticity of asphalt mixture, characterized in that: include: According to the test requirements, the test piece is cut into several pieces to be tested and the sizes of the pieces to be tested are adjusted; Measure various physical indicators of the test piece, and fix the test piece on the mounting plate by centering the centering device; The mounting nails are pasted to the surface of the test piece along the circumferential interval of the test piece by a pneumatic pasting device; the upper support and the lower support are respectively connected to the mounting nails, and the upper support and the lower support are respectively fixed to the two ends of the guide rod of the displacement sensor through the upper support and the lower support, and the displacement sensor is fixed to the test piece; Connecting the upper tensile assembly to the main shaft of the material testing machine, connecting the locking plate of the lower tensile assembly to the mounting plate, and bringing the lower tensile assembly into contact with the upper tensile assembly; The main shaft of the material testing machine is driven to perform a pre-contact process, and the lower tensile assembly and the upper tensile assembly are connected by screws; the specific steps include: driving the main shaft of the material testing machine to move upward and return to position; driving the main shaft of the material testing machine to move downward at a second rate, so that the connecting head of the upper tensile assembly applies pressure to the test piece through the locking disk of the lower tensile assembly, and connecting the lower tensile assembly and the upper tensile assembly by screws; after the connection is completed, the main shaft of the material testing machine is driven to move upward at a second rate, so that the connecting head of the upper tensile assembly is away from the locking disk of the lower tensile assembly; driving the main shaft of the material testing machine to move upward at a first rate to apply a tensile force to the test piece until the test piece is damaged, and recording a peak load of the test piece to obtain a tensile strength of the test piece; Replace the test piece, and drive the main shaft of the material testing machine to move upward at a second speed to preload the tensile force on the test piece; Determine the loading level according to the peak load of the test piece, drive the main shaft of the material testing machine to move upward at a first rate, load and unload each level of load in sequence on the basis of the preload tension, and record the tensile displacement data and rebound displacement data of the test piece under each level of load in sequence to obtain the tensile rebound modulus value of the test piece, wherein each level of load includes a first level load of 0.1P, a second level load of 0.2P, a third level load of 0.3P, a fourth level load of 0.4P, a fifth level load of 0.5P, and a sixth level load of 0.6P, wherein P is the peak load; The step of obtaining the tensile elastic modulus value of the test piece includes: determining the tensile elastic modulus of the test piece under each level of load according to the function E=h / k, wherein h is the height of the test piece, and k is the slope of the linear curve of each level of load and rebound displacement data; taking the average value of the tensile elastic modulus of the test piece under the third level load, the fourth level load, and the fifth level load as the tensile elastic modulus value.

2. The asphalt mixture tensile resilience modulus test method according to claim 1, characterized in that: The step of cutting the test piece into a plurality of test pieces according to the test requirements and adjusting the sizes of the test pieces comprises: Cut the test piece into a preset number of pieces to be tested; Performing a rotational shearing and pressing process on the piece to be tested, adjusting the diameter of the piece to be tested to a first preset diameter, and adjusting the height of the piece to be tested to a first preset height; After the rotary shearing and pressing process is completed, the workpiece to be tested is double-sided cut and double-sided flattened, the diameter of the workpiece to be tested is adjusted to a second preset diameter, and the height of the workpiece to be tested is adjusted to a second preset height.

3. The asphalt mixture tensile resilience modulus test method according to claim 1, characterized in that: The step of centering and fixing the workpiece to be tested on the mounting plate by the centering device comprises: Place one of the mounting plates in the base of the centering device, lift the upper pull rod of the centering device, and place the other mounting plate in the upper slot of the upper pull rod; Apply the adhesive evenly on the surface of the mounting plate and both ends of the test piece, and place the test piece on one of the mounting plates located on the base of the centering device; Lock the lateral restraints of the centering device to center the workpiece to be tested, and lower the upper pull rod to allow the other mounting plate to bond with the workpiece to be tested; After the adhesive is cured, lift the upper pull rod and take out the test piece, and place the test piece in the environmental chamber until the temperature of the test piece reaches the test temperature.

4. The asphalt mixture tensile resilience modulus test method according to claim 1, characterized in that: The steps of driving the main shaft of the material testing machine to move upward at a first rate, and sequentially loading and unloading various levels of loads based on the preload tension include: The main shaft of the material testing machine is driven to move upward at a first rate, and the load is loaded to a target load on the basis of the preload tension. Then, the main shaft of the material testing machine is driven to move downward at a first rate, and the load is unloaded from the target load to the preload tension. The tensile displacement data and the rebound displacement data of the target load are recorded according to the displacement sensor on the test piece. After waiting for a preset time, the main shaft of the material testing machine is driven to move upward at a first rate, and loaded to the next target load on the basis of the preload tension. Then, the main shaft of the material testing machine is driven to move downward at the first rate, and unloaded from the next target load to the preload tension. The tensile displacement data and rebound displacement data of the next target load are recorded according to the displacement sensor on the test piece.

5. The asphalt mixture tensile resilience modulus test method according to claim 4, characterized in that: The following steps are also included: After determining the loading level, the spindle of the material testing machine is driven to move upward at a second rate, and loaded to a preset multiple of the peak load on the basis of the preload tension. Then, the spindle of the material testing machine is driven to move downward at a second rate, and unloaded from the preset multiple of the peak load to the preload tension. The preload displacement data and preload rebound displacement data are recorded according to the displacement sensor on the test piece.

6. The asphalt mixture tensile resilience modulus test method according to claim 1, characterized in that: The step of recording the peak load of the test piece to obtain the tensile strength of the test piece includes: According to the function R = 4P / πd 2 , determine the tensile strength R of the test piece, where P is the peak load and d is the diameter of the test piece.

7. The asphalt mixture tensile resilience modulus test method according to claim 6, characterized in that: The following steps are also included: Calculate the standard deviation of the tensile modulus of elasticity of the test pieces, and determine whether the difference between the tensile modulus of elasticity of each test piece and the average tensile modulus of elasticity of the test pieces is greater than the standard deviation multiplied by the slope k; If the answer is yes, the tensile modulus of elasticity of the test piece is discarded; If the judgment is no, the tensile modulus value of the tested piece is retained; According to the tensile elastic modulus values ​​of the other test pieces, the tensile elastic modulus value for pavement design is obtained.

8. The asphalt mixture tensile resilience modulus test method according to claim 7, characterized in that: The step of obtaining the tensile modulus of elasticity value for pavement design according to the tensile modulus of elasticity values ​​of the remaining test pieces comprises: According to the function Determine the tensile modulus of resilience value Em for pavement design, where E* is the average tensile modulus of resilience of the remaining test pieces, S is the standard deviation of the tensile modulus of resilience of the remaining test pieces, n is the valid number of test pieces, and t is the guarantee rate coefficient.

Citation Information

Patent Citations

  • Asphalt mixture tension dynamic modulus measurement method

    CN107748106A