Silicone rubber composite materials, their preparation methods and applications
By combining layered vermiculite powder with platinum complexes, the problem of pulverization and cracking of silicone rubber composites under high-temperature flames and vibrations was solved, achieving excellent flame retardant and fireproof performance and meeting the high fireproof requirements of aerospace devices.
Patent Information
- Application Number
- CN202210740494.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-06-28
- Publication Date
- 2026-11-10
- Estimated Expiration
- 2042-06-28
AI Technical Summary
Traditional silicone rubber composite materials are prone to pulverization and surface cracking under high-temperature flames and vibrations at 1090℃±80℃, and cannot simultaneously meet the requirements of FV-0 flame retardancy and the high fire resistance of standard HB7044-2014.
Vermiculite powder with a layered structure is used in combination with platinum complexes and inorganic flame retardants. Through the expansion and cross-linking reaction of vermiculite powder, a stable protective layer is formed, which improves flame retardant and fireproof performance.
Under high-temperature flame erosion and vibration environment, a hard and solid protective layer is formed, which meets the high fire resistance requirements of FV-0 flame retardant performance and standard HB7044-2014, protecting the internal core material of pipeline products.
Smart Images

Figure BDA0003717763230000131 
Figure BDA0003717763230000141
Abstract
Description
Technical Field
[0001] This invention relates to the field of rubber materials technology, and in particular to a silicone rubber composite material, its preparation method, and its application. Background Technology
[0002] Traditional techniques often focus on the flame-retardant or fire-resistant properties of silicone rubber, resulting in a limited range of performance characteristics. However, in specific fields, such as aerospace components, when silicone rubber is used for fire-resistant sleeves in fuel lines, it is required not only to achieve an FV-0 flame-retardant rating but also to meet the fire resistance testing requirements for civil aircraft hoses and pipe assemblies (Standard HB7044-2014). It's important to note that Standard HB7044-2014 differs from the programmed temperature rise test used in general fire resistance testing. Standard HB7044-2014 requires the test sample to be burned under a high-temperature flame of 1090℃±80℃ and vibration at a certain frequency for 5-15 minutes to test its fire resistance; these test conditions are extremely stringent. Meeting both the flame-retardant and fire-resistant requirements simultaneously undoubtedly places higher demands on the overall performance of silicone rubber materials.
[0003] Although adding inorganic flame retardants and refractory fillers to silicone rubber can improve the problem of the single performance of silicone rubber, composite silicone rubber composed of traditional inorganic flame retardants and refractory fillers still has problems such as easy pulverization and premature detachment of ablation material and easy surface cracking leading to poor heat insulation under high temperature flame of 1090℃±80℃ and vibration of a certain frequency. Therefore, composite silicone rubber cannot simultaneously meet the requirements of FV-0 flame retardant performance and the high fire resistance performance of standard HB7044-2014. Summary of the Invention
[0004] Therefore, it is necessary to provide a silicone rubber composite material, its preparation method, and its application to address the above-mentioned problems. The silicone rubber composite material has excellent flame retardant and fire-resistant properties, and can simultaneously meet the requirements of FV-0 flame retardant performance and the high fire resistance performance of standard HB7044-2014. It can be used to prepare pipeline products, which can effectively protect the internal core material and have higher safety.
[0005] A silicone rubber composite material comprises the following components in parts by weight: 100 parts of silicone rubber base material, 20-45 parts of inorganic flame retardant, 30-50 parts of refractory filler, 1.0-1.5 parts of vulcanizing agent, 0.25-1.5 parts of platinum complex, 0.05-0.5 parts of nitrogen-containing compound, and 5-15 parts of heat resistant agent. The refractory filler contains layered vermiculite powder, the mass fraction of vermiculite powder in the refractory filler is greater than or equal to 65%, the mass ratio of vermiculite powder to platinum complex is 20:1-200:1, and the specific surface area of the vermiculite powder is 5 m². 2 / g-23m 2 / g.
[0006] In one embodiment, the vermiculite powder has a particle size of 300-1250 mesh.
[0007] In one embodiment, the inorganic flame retardant contains magnesium hydroxide, wherein the mass fraction of magnesium hydroxide in the inorganic flame retardant is greater than or equal to 65%.
[0008] In one embodiment, based on 100 parts by weight of silicone rubber base material, the platinum in the platinum complex is 7.5 × 10⁻⁶. -4 Parts by weight - 4.5 × 10 -3 Weight of portions.
[0009] In one embodiment, the silicone rubber base material includes at least one of methyl vinyl silicone rubber and methyl phenyl vinyl silicone rubber.
[0010] In one embodiment, the silicone rubber base material has a Shore hardness of 40A-60A.
[0011] A method for preparing the silicone rubber composite material as described above, the method comprising the following steps:
[0012] A silicone rubber base material is provided, which is then plasticized and mixed with an inorganic flame retardant, refractory filler, and heat resistant agent, followed by compounding and debinding to obtain a silicone rubber compound; and
[0013] The silicone rubber compound is calendered onto a roll and then mixed with a vulcanizing agent, a nitrogen-containing compound, and a platinum complex. The mixture is then subjected to thin-pass vulcanization and vulcanization to obtain a silicone rubber composite material.
[0014] In one embodiment, the plasticizing temperature is 50°C-80°C, and the plasticizing time is 5 min-8 min;
[0015] And / or, the mixing temperature is 50℃-80℃, and the mixing time is 10min-20min.
[0016] In one embodiment, the vulcanization temperature is 165°C-180°C, the vulcanization pressure is 5MPa-10MPa, and the vulcanization time is 6min-10min.
[0017] Application of a silicone rubber composite material as described above in pipeline products.
[0018] The silicone rubber composite material of the present invention has a layered structure and a specific surface area of 5 m². 2 / g-23m 2 When vermiculite powder of / g is used in combination with platinum complexes and inorganic flame retardants, on the one hand, this uniquely structured vermiculite powder will slightly expand under high-temperature flame ablation, which can not only absorb heat, but also form an expanded layer that can effectively resist external high temperatures, thereby improving the fire resistance of silicone rubber composites. On the other hand, this uniquely structured vermiculite powder can also reduce the heat release rate. When the mass ratio of vermiculite powder to platinum complex is 20:1-200:1, this uniquely structured vermiculite powder can synergistically enhance flame retardancy with the platinum complex, while changing the cracking pathway of silicone rubber, causing a chain reaction in silicone rubber, forming a cross-linked structure, promoting the char formation of silicone rubber, and helping silicone rubber composites form a stable and complete protective layer under high-temperature flame ablation, thereby improving the flame retardant performance of silicone rubber composites.
[0019] Therefore, the silicone rubber composite material possesses excellent flame retardant and fire-resistant properties, simultaneously meeting the requirements of FV-0 flame retardancy and the high fire resistance of standard HB7044-2014, and can be used to manufacture pipeline products. Especially under high-temperature flame erosion and vibration environments, a hard and robust protective layer can still be formed on the surface of the pipeline product. This protective layer is not easily powdered or cracked, and has good heat insulation properties, thus effectively protecting the core material inside the pipeline product and providing higher safety. Detailed Implementation
[0020] To facilitate understanding of the present invention, it will be described in more detail below. However, it should be understood that the present invention can be implemented in many different forms and is not limited to the embodiments or examples described herein. Rather, these embodiments or examples are provided to make the disclosure of the present invention more thorough and complete.
[0021] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as commonly understood by one of ordinary skill in the art to which this invention pertains. The terminology used herein in the description of the invention is for the purpose of describing particular embodiments or examples only and is not intended to be limiting of the invention.
[0022] The traditional fire-retardant mechanism of silicone rubber composites involves the eutectic reaction between silica produced by the high-temperature decomposition of silicone rubber and molten refractory filler or a system of refractory filler and compatibilizer to form a ceramic body. Furthermore, traditional fire-retardant performance studies primarily characterize the composite material's fire resistance by testing its ceramic conversion rate and flexural strength under programmed temperature conditions. However, under non-programmed temperature conditions, the vitrification of silicone rubber composites is limited to some extent, especially under high-temperature flame erosion and vibration environments (1090℃±80℃). In such conditions, it is difficult for silicone rubber composites to form a ceramic layer, and even if a ceramic layer is formed, its thermal stability is poor, making it prone to cracking and failing to meet the fire-retardant performance requirements of standard HB7044-2014.
[0023] Through long-term and in-depth research, the applicant discovered that when refractory fillers containing vermiculite powder are used in combination with platinum complexes and inorganic flame retardants, the structure of the vermiculite powder and the amount of vermiculite powder and platinum complex have a significant impact on whether the silicone rubber composite material can simultaneously meet the requirements of FV-0 flame retardant performance and the high fire resistance performance of standard HB7044-2014.
[0024] Therefore, the silicone rubber composite material provided by the present invention comprises the following components in parts by weight: 100 parts of silicone rubber base material, 20-45 parts of inorganic flame retardant, 30-50 parts of refractory filler, 1.0-1.5 parts of vulcanizing agent, 0.25-1.5 parts of platinum complex, 0.05-0.5 parts of nitrogen-containing compound, and 5-15 parts of heat resistant agent, wherein the refractory filler contains vermiculite powder with a layered structure, the mass fraction of vermiculite powder in the refractory filler is greater than or equal to 65%, the mass ratio of vermiculite powder to platinum complex is 20:1-200:1, and the specific surface area of vermiculite powder is 5 m². 2 / g-23m 2 / g.
[0025] The silicone rubber composite material of the present invention has a layered structure and a specific surface area of 5 m². 2 / g-23m 2 When vermiculite powder of / g is used in combination with platinum complexes and inorganic flame retardants, on the one hand, this uniquely structured vermiculite powder undergoes slight expansion at high temperatures, which not only absorbs heat but also forms an expanded layer that effectively resists external high temperatures, thereby improving the fire resistance of silicone rubber composites. On the other hand, this uniquely structured vermiculite powder can also reduce the heat release rate. When the mass ratio of vermiculite powder to platinum complex is 20:1-200:1, this uniquely structured vermiculite powder can synergistically enhance flame retardancy with the platinum complex, while altering the cracking pathway of silicone rubber, causing a chain reaction in silicone rubber, forming a cross-linked structure, and promoting char formation in silicone rubber. This helps silicone rubber composites form a stable and complete protective layer under high-temperature flame ablation, thereby improving the flame retardant performance of silicone rubber composites.
[0026] Furthermore, the mass ratio of the vermiculite powder to the platinum complex is preferably 35:1-95:1.
[0027] In order to coordinate the proportion and composition of refractory fillers and thus further improve the fire resistance of silicone rubber composites, the mass fraction of vermiculite powder in the refractory fillers is preferably 70%-95%.
[0028] To further improve the expansion effect of vermiculite powder at high temperatures and reduce the heat release rate, the specific surface area of the vermiculite powder can be further preferably 9m². 2 / g-19m 2 / g.
[0029] It should be noted that the vermiculite powder is made from raw vermiculite through high-temperature roasting at 900℃-1000℃, screening, and grinding. Specifically, the particle size of the vermiculite powder is 300 mesh-1250 mesh, preferably 500 mesh-1000 mesh.
[0030] In one embodiment, the refractory filler further includes at least one of wollastonite, mica powder, diatomaceous earth, silica fume, kaolin, magnesium oxide, and aluminum oxide.
[0031] To reduce the amount of inorganic flame retardants and refractory fillers added, and to minimize the impact of platinum complexes, inorganic flame retardants, and refractory fillers on the mechanical properties of silicone rubber composites, in one embodiment, based on 100 parts by weight of silicone rubber base material, the platinum in the platinum complex is 7.5 × 10⁻⁶. -4 Parts by weight - 4.5 × 10 -3 The preferred mass fraction is 1.5 × 10⁻⁶. -3 -3.0×10 -3 .
[0032] Specifically, the platinum complex comprises at least one of the following: a chloroplatinic acid-isopropanol solution, a platinum complex solution coordinated with tetrahydrofuran, a platinum complex solution coordinated with diethyl phthalate, a platinum-olefin complex, and a platinum unsaturated siloxane solution.
[0033] To further improve the stability of the protective layer structure formed by the silicone rubber composite material under high temperature flame ablation, the inorganic flame retardant contains magnesium hydroxide, and the mass fraction of magnesium hydroxide in the inorganic flame retardant is greater than or equal to 65%, preferably 75%-95%.
[0034] Specifically, the inorganic flame retardant also includes at least one of aluminum hydroxide, magnesium aluminum hydrotalcite, and zinc borate, preferably zinc borate.
[0035] In one embodiment, the silicone rubber base material includes at least one of methyl vinyl silicone rubber and methyl phenyl vinyl silicone rubber, preferably methyl vinyl silicone rubber. For ease of processing, the silicone rubber base material has a Shore hardness of 40A-60A.
[0036] The nitrogen atoms in the nitrogen-containing compound contain unshared electron pairs, which can coordinate with the p, d orbitals or hybrid orbitals of platinum, thus facilitating the flame retardancy of the platinum complex. Specifically, the nitrogen-containing compound includes at least one of piperazine-propylmethyldimethoxysilane, 3-aminopropyltriethoxysilane, and benzotriazole, preferably benzotriazole.
[0037] To improve the thermal stability of silicone rubber composites and thus further enhance their fire resistance, the heat resistant agent includes at least one of iron(II,III) oxide, ferric oxide, nano-titanium dioxide, and nano-cerium oxide, and the heat resistant agent is preferably in powder form.
[0038] In one embodiment, the vulcanizing agent includes at least one of di-tert-butyl peroxide (DTBP), 2,5-dimethyl-2,5-bis(tert-butylperoxy)hexane (DBPH), and dicumyl peroxide (DCP).
[0039] This invention provides a method for preparing the silicone rubber composite material as described above, the method comprising the following steps:
[0040] S1, providing a silicone rubber base material, plasticizing the silicone rubber base material and then mixing it with an inorganic flame retardant, refractory filler and heat resistant agent, and then mixing and debinding to obtain a silicone rubber compound;
[0041] S2, the silicone rubber compound is calendered onto a roll and then mixed with a vulcanizing agent, a nitrogen-containing compound and a platinum complex, and then subjected to thin-passing and vulcanization to obtain a silicone rubber composite material.
[0042] In one embodiment, step S1 is preferably carried out in an internal mixer with a rotation speed of 40 rpm to 60 rpm, a plasticizing temperature of 50°C to 80°C, and a plasticizing time of 5 min to 8 min.
[0043] To achieve better mixing, inorganic flame retardant can be added first and mixed at 50℃-80℃ for 10-20 minutes, followed by refractory filler and mixed at 50℃-80℃ for 10-20 minutes. The heat resistant agent can be added together with the inorganic flame retardant, or together with the refractory filler, or divided into two parts: one part is added together with the inorganic flame retardant and the other part is added together with the refractory filler.
[0044] In step S2, the silicone rubber compound is preferably calendered on a two-roll calender. The speed of the front roll of the two-roll calender is set to 10-12 rpm, and the speed ratio between the front and rear rolls is set to 1:1.1-1:1.2. The distance between the front and rear rolls is 2mm-6mm. After the silicone rubber compound is coated onto the rolls, the vulcanizing agent, nitrogen-containing compound, and platinum complex are preferably added sequentially to ensure uniform mixing, and then passed through the calender 3-5 times.
[0045] In one embodiment, the vulcanization temperature is 165°C-180°C, the vulcanization pressure is 5MPa-10MPa, and the vulcanization time is 6min-10min.
[0046] The silicone rubber composite material obtained by this preparation method has excellent flame retardant and fireproof properties, and can simultaneously meet the requirements of FV-0 flame retardant performance and the high fireproof performance of standard HB7044-2014, and has broad application prospects.
[0047] The present invention also provides an application of the silicone rubber composite material described above in pipeline products.
[0048] The silicone rubber composite material described in this invention can be widely used in the manufacture of pipeline products such as wires, cables, and oil pipelines. Especially under high-temperature flame erosion and vibration environments, a hard and solid protective layer can still be formed on the surface of the pipeline product. The protective layer is not easy to powder or crack and has good heat insulation effect, thereby effectively protecting the core material inside the pipeline product and having higher safety.
[0049] The following specific embodiments will further illustrate the silicone rubber composite material, its preparation method, and its application.
[0050] Example 1
[0051] 90 parts by weight of methyl vinyl silicone rubber (Shore hardness 50A) and 10 parts by weight of methyl vinyl silicone rubber (Shore hardness 60A) were used as silicone rubber base materials and added to an internal mixer. The mixer temperature was set to 80℃ and the speed to 50 rpm, and the mixture was plasticized for 6 minutes. Then, 32 parts by weight of magnesium hydroxide, 3 parts by weight of ferric oxide, and 2 parts by weight of magnetite were added, and the mixture was mixed at 80℃ for 10 minutes. Next, 50 parts by weight of layered vermiculite powder and 3 parts by weight of nano-titanium dioxide were added, and the mixture was mixed at 80℃ for 15 minutes to obtain a silicone rubber compound. The vermiculite powder had a particle size of 1250 mesh and a specific surface area of 22.8 m². 2 / g.
[0052] Silicone rubber compound was added to a small two-roller tablet press. After the compound wrapped around the rollers, 1.5 parts by weight of 2,5-dimethyl-2,5-bis(tert-butylperoxy)hexane, 0.2 parts by weight of benzotriazole, and 1.0 parts by weight of a platinum unsaturated siloxane solution were added sequentially. The mixture was then thoroughly mixed on the small two-roller tablet press and placed in a stainless steel mold. The mold was then placed on a flat vulcanizing machine, with the temperature set to 180°C and the pressure to 10 MPa, and vulcanized for 6 minutes to obtain a silicone rubber composite material. The platinum content in the platinum unsaturated siloxane solution was 3.0 × 10⁻⁶ parts by weight, based on a total of 100 parts by weight of methyl vinyl silicone rubber. -3 Weight of portions.
[0053] Example 2
[0054] 70 parts by weight of methyl vinyl silicone rubber (Shore hardness 50A) and 30 parts by weight of methyl phenyl vinyl silicone rubber (Shore hardness 50A) were used as silicone rubber base materials and added to an internal mixer. The mixer temperature was set to 80℃ and the speed to 50 rpm, and the mixture was plasticized for 5 minutes. Then, 36 parts by weight of magnesium hydroxide and 5 parts by weight of ferric oxide powder were added, and the mixture was mixed at 80℃ for 10 minutes. Next, 50 parts by weight of layered vermiculite powder was added, and the mixture was mixed at 80℃ for 15 minutes to obtain a silicone rubber compound. The vermiculite powder had a particle size of 300 mesh and a specific surface area of 5.4 m². 2 / g.
[0055] The silicone rubber compound was added to a small two-roll press. After the compound wrapped around the rollers, 1.5 parts by weight of 2,5-dimethyl-2,5-bis(tert-butylperoxy)hexane, 0.1 parts by weight of benzotriazole, and 0.5 parts by weight of a chloroplatinic acid isopropanol solution were added sequentially. The mixture was then thoroughly mixed on the small two-roll press and placed in a stainless steel mold. The mold was then placed on a flat vulcanizing machine, with the temperature set at 165°C and the pressure at 10 MPa for 10 minutes to obtain a silicone rubber composite material. Based on a total of 100 parts by weight of methyl vinyl silicone rubber and methyl phenyl vinyl silicone rubber, the platinum content in the chloroplatinic acid is 1.5 × 10⁻⁶. -3 Weight of portions.
[0056] Example 3
[0057] 40 parts by weight of methyl vinyl silicone rubber (Shore hardness 40A) and 60 parts by weight of methyl vinyl silicone rubber (Shore hardness 60A) were used as silicone rubber base materials. 100 parts by weight of the silicone rubber base material were added to an internal mixer, and the mixer temperature was set to 50℃ and the speed to 50 rpm for 8 minutes. Then, 30 parts by weight of magnesium hydroxide and 5 parts by weight of zinc borate were added, and the mixture was mixed at 50℃ for 10 minutes. Next, 40 parts by weight of layered vermiculite powder, 5 parts by weight of wollastonite, and 5 parts by weight of nano-cerium dioxide were added, and the mixture was mixed at 50℃ for 15 minutes to obtain a silicone rubber compound. The vermiculite powder had a particle size of 800 mesh and a specific surface area of 11.2 m². 2 / g.
[0058] Silicone rubber compound was added to a small two-roller tablet press. After the compound wrapped around the rollers, 1.0 parts by weight of 2,5-dimethyl-2,5-bis(tert-butylperoxy)hexane, 0.05 parts by weight of benzotriazole, and 0.25 parts by weight of a platinum-olefin complex were added sequentially. The mixture was then thoroughly mixed on the small two-roller tablet press and placed in a stainless steel mold. The mold was then placed on a flat vulcanizing machine, with the temperature set at 170°C and the pressure at 10 MPa for 8 minutes to obtain a silicone rubber composite material. Based on a total of 100 parts by weight of methyl vinyl silicone rubber, the platinum in the platinum-olefin complex was 7.5 × 10⁻⁶. -4 Weight of portions.
[0059] Example 4
[0060] 90 parts by weight of methyl vinyl silicone rubber (Shore hardness 50A) and 10 parts by weight of methyl phenyl vinyl silicone rubber (Shore hardness 40A) were used as silicone rubber base materials and added to an internal mixer. The mixer temperature was set to 60℃ and the speed to 50 rpm, and the mixture was plasticized for 8 minutes. Then, 30 parts by weight of magnesium hydroxide and 5 parts by weight of magnesium aluminum hydrotalcite were added, and the mixture was mixed at 60℃ for 10 minutes. Next, 40 parts by weight of layered vermiculite powder, 10 parts by weight of mica powder, and 5 parts by weight of nano titanium dioxide were added, and the mixture was mixed at 60℃ for 20 minutes to obtain a silicone rubber compound. The vermiculite powder had a particle size of 500 mesh and a specific surface area of 9.4 m². 2 / g.
[0061] The silicone rubber compound was added to a small two-roller tablet press. After the compound wrapped around the rollers, 1.0 parts by weight of 2,5-dimethyl-2,5-bis(tert-butylperoxy)hexane, 0.2 parts by weight of 3-aminopropyltriethoxysilane, and 1.0 parts by weight of a platinum unsaturated siloxane solution were added sequentially. The mixture was then thoroughly mixed on the small two-roller tablet press and placed in a stainless steel mold. The mold was then placed on a flat vulcanizing machine, with the temperature set at 170°C and the pressure at 10 MPa for 8 minutes to obtain a silicone rubber composite material. The composite material was based on a total of 100 parts by weight of methyl vinyl silicone rubber and methyl phenyl vinyl silicone rubber, and the platinum content in the platinum unsaturated siloxane solution was 3.0 × 10⁻⁶. -3 Weight of portions.
[0062] Example 5
[0063] Take 50 parts by weight of methyl vinyl silicone rubber (Shore hardness 40A) and 50 parts by weight of methyl vinyl silicone rubber (Shore hardness 60A) as silicone rubber base materials, add them to a Banbury mixer, set the mixer temperature to 70℃ and the speed to 40 rpm, and plasticize for 5 minutes. Then, add 36 parts by weight of magnesium hydroxide and 5 parts by weight of ferric oxide powder, and mix at 70℃ for 10 minutes. Next, add 45 parts by weight of layered vermiculite powder and 5 parts by weight of diatomaceous earth, and mix at 70℃ for 15 minutes to obtain a silicone rubber compound, wherein the vermiculite powder has a particle size of 1250 mesh and a specific surface area of 22.8 m². 2 / g.
[0064] The silicone rubber compound was added to a small two-roller tablet press. After the compound wrapped around the rollers, 1.5 parts by weight of 2,5-dimethyl-2,5-bis(tert-butylperoxy)hexane, 0.3 parts by weight of piperazine-propylmethyldimethoxysilane, and 1.0 part by weight of a platinum unsaturated siloxane solution were added sequentially. The mixture was then thoroughly mixed on the small two-roller tablet press and placed in a stainless steel mold. The mold was then placed on a flat vulcanizing machine, with the temperature set at 165°C and the pressure at 10 MPa, and vulcanized for 10 minutes to obtain a silicone rubber composite material. The platinum content in the platinum unsaturated siloxane solution was 3.0 × 10⁻⁶ parts by weight, based on a total of 100 parts by weight of methyl vinyl silicone rubber. -3 Weight of portions.
[0065] Example 6
[0066] Take 80 parts by weight of methyl vinyl silicone rubber (Shore hardness 50A) and 20 parts by weight of methyl vinyl silicone rubber (Shore hardness 60A) as silicone rubber base materials, add them to a Banbury mixer, set the mixer temperature to 80℃ and the speed to 50 rpm, and plasticize for 5 minutes. Then, add 36 parts by weight of magnesium hydroxide and 5 parts by weight of ferric oxide powder, and mix at 80℃ for 10 minutes. Then add 50 parts by weight of layered vermiculite powder, and mix at 80℃ for 15 minutes to obtain a silicone rubber compound, wherein the vermiculite powder has a particle size of 600 mesh and a specific surface area of 9.8 m². 2 / g.
[0067] Silicone rubber compound was added to a small two-roller tablet press. After the compound wrapped around the rollers, 1.5 parts by weight of 2,5-dimethyl-2,5-bis(tert-butylperoxy)hexane, 0.1 parts by weight of benzotriazole, and 0.25 parts by weight of a platinum unsaturated siloxane solution were added sequentially. The mixture was then thoroughly mixed on the small two-roller tablet press and placed in a stainless steel mold. The mold was then placed on a flat vulcanizing machine, with the temperature set at 165°C and the pressure at 10 MPa, and vulcanized for 10 minutes to obtain a silicone rubber composite material. The platinum content in the platinum unsaturated siloxane solution was 7.5 × 10⁻⁶ parts by weight, based on a total of 100 parts by weight of methyl vinyl silicone rubber. -4 Weight of portions.
[0068] Example 7
[0069] 70 parts by weight of methyl vinyl silicone rubber (Shore hardness 50A) and 30 parts by weight of methyl vinyl silicone rubber (Shore hardness 60A) were used as silicone rubber base materials. 100 parts by weight of the silicone rubber base material were added to an internal mixer, and the mixer temperature was set to 50℃ and the speed to 50 rpm for 8 minutes. Then, 30 parts by weight of magnesium hydroxide and 5 parts by weight of zinc borate were added, and the mixture was mixed at 50℃ for 10 minutes. Next, 30 parts by weight of layered vermiculite powder, 5 parts by weight of wollastonite, and 5 parts by weight of mica powder were added, and the mixture was mixed at 50℃ for 15 minutes to obtain a silicone rubber compound. The vermiculite powder had a particle size of 800 mesh and a specific surface area of 11.2 m². 2 / g.
[0070] Silicone rubber compound was added to a small two-roller press. After the compound wrapped around the rollers, 1.0 parts by weight of 2,5-dimethyl-2,5-bis(tert-butylperoxy)hexane, 0.05 parts by weight of benzotriazole, and 1.5 parts by weight of isopropanol solution of chloroplatinic acid were added sequentially. The mixture was then thoroughly mixed on the small two-roller press and placed in a stainless steel mold. The mold was then placed on a flat vulcanizing machine, with the temperature set at 170°C and the pressure at 10 MPa for 8 minutes to obtain a silicone rubber composite material. Based on a total of 100 parts by weight of methyl vinyl silicone rubber, the platinum content in the isopropanol solution of chloroplatinic acid was 4.5 × 10⁻⁶. -3 Weight of portions.
[0071] Comparative Example 1
[0072] The only difference between Comparative Example 1 and Example 1 is that the silicone rubber composite material was prepared without the addition of platinum-based unsaturated siloxane solution and benzotriazole.
[0073] Comparative Example 2
[0074] The only difference between Comparative Example 2 and Example 1 is that 50 parts by mass of wollastonite were used instead of 50 parts by mass of layered vermiculite powder.
[0075] Comparative Example 3
[0076] The only difference between Comparative Example 3 and Example 1 is that 50 parts by weight of mica powder were used instead of 50 parts by weight of vermiculite powder with a layered structure.
[0077] Comparative Example 4
[0078] The only difference between Comparative Example 4 and Example 1 is that 25 parts by mass of layered vermiculite powder and 25 parts by mass of wollastonite were used instead of 50 parts by mass of layered vermiculite powder. The particle size of the vermiculite powder in both examples was 1250 mesh, and the specific surface area was 22.8 m². 2 / g.
[0079] Comparative Example 5
[0080] The only difference between Comparative Example 5 and Example 1 is that 18 parts by mass of layered vermiculite powder and 32 parts by mass of wollastonite were used instead of 50 parts by mass of layered vermiculite powder. The particle size of the vermiculite powder in both examples was 1250 mesh, and the specific surface area was 22.8 m². 2 / g.
[0081] Comparative Example 6
[0082] The only difference between Comparative Example 6 and Example 1 is that Comparative Example 6 uses a specific surface area of 2.3 m². 2 / g of layered vermiculite powder replaced a specific surface area of 22.8m². 2 / g of layered vermiculite powder, wherein the particle size of the vermiculite powder is 1250 mesh.
[0083] The silicone rubber composite materials prepared in Examples 1-7 and Comparative Examples 1-6 were subjected to flame retardant and fire resistance performance tests. Flame retardant performance was characterized using a horizontal-vertical burner, and the results were determined according to GB / T10707-2008 Rubber Combustion Performance. Fire resistance performance was tested according to the Fire Resistance Test Requirements for Civil Aircraft Hoses and Pipe Components (Standard HB7044-2014). The test results are shown in Table 1 below.
[0084] Table 1
[0085]
[0086]
[0087] Compared with Comparative Example 1, it can be seen that the combined use of platinum complex and nitrogen-containing compound can improve the flame retardant effect of silicone rubber composite material. Furthermore, the platinum complex can enable the silicone rubber composite material to form a dense block structure in the fire resistance test, which is not easy to pulverize.
[0088] Compared with Example 1, Comparative Examples 2 and 3 show that vermiculite powder can effectively solve the surface cracking problem of silicone rubber composite material in fire resistance test compared with wollastonite and mica powder. Furthermore, when combined with platinum complex and flame retardant, it can form a dense and hard shell on the surface of silicone rubber composite material in fire resistance test, which can effectively protect the internal core material.
[0089] Comparative Example 4, compared to Example 1, shows that when the mass fraction of vermiculite powder in the refractory filler is less than 65%, the prepared flame-retardant and fire-resistant silicone rubber sample cracks on the surface during the fire test. Comparative Example 5, compared to Example 1, shows that when the mass ratio of vermiculite powder to the platinum complex is less than 20:1, the prepared flame-retardant and fire-resistant silicone rubber sample cracks on the surface during the fire test.
[0090] Comparative Example 6 and Example 1 show that when the specific surface area of the vermiculite powder used is less than 5m², 2 When the concentration was / g, the prepared flame-retardant and fire-resistant silicone rubber sample cracked on the surface during the fire resistance test.
[0091] The technical features of the above embodiments can be combined in any way. For the sake of brevity, not all possible combinations of the technical features in the above embodiments are described. However, as long as there is no contradiction in the combination of these technical features, they should be considered to be within the scope of this specification.
[0092] The embodiments described above are merely illustrative of several implementations of the present invention, and while the descriptions are relatively specific and detailed, they should not be construed as limiting the scope of the invention patent. It should be noted that those skilled in the art can make various modifications and improvements without departing from the concept of the present invention, and these all fall within the protection scope of the present invention. Therefore, the protection scope of this invention patent should be determined by the appended claims.
Claims
1. A silicone rubber composite material, characterized in that, The silicone rubber composite material comprises the following components in parts by weight: 100 parts of silicone rubber base material, 20-45 parts of inorganic flame retardant, 30-50 parts of refractory filler, 1.0-1.5 parts of vulcanizing agent, 0.25-1.5 parts of platinum complex, 0.05-0.5 parts of nitrogen-containing compound, and 5-15 parts of heat resistant agent. The refractory filler contains layered vermiculite powder, with a mass fraction of vermiculite powder greater than or equal to 65% in the refractory filler. The mass ratio of vermiculite powder to the platinum complex is 20:1-200:1, and the specific surface area of the vermiculite powder is 5 m². 2 / g-23m 2 / g, wherein the nitrogen-containing compound includes at least one of piperazinepropylmethyldimethoxysilane, 3-aminopropyltriethoxysilane, and benzotriazole.
2. The silicone rubber composite material according to claim 1, characterized in that, The vermiculite powder has a particle size of 300-1250 mesh.
3. The silicone rubber composite material according to claim 1, characterized in that, The inorganic flame retardant contains magnesium hydroxide, and the mass fraction of magnesium hydroxide in the inorganic flame retardant is greater than or equal to 65%.
4. The silicone rubber composite material according to claim 1, characterized in that, Based on 100 parts by weight of silicone rubber base material, the platinum in the platinum complex is 7.5 × 10⁻⁶. -4 Parts by weight - 4.5 × 10 -3 Weight (parts).
5. The silicone rubber composite material according to claim 1, characterized in that, The silicone rubber base material includes at least one of methyl vinyl silicone rubber and methyl phenyl vinyl silicone rubber.
6. The silicone rubber composite material according to claim 1 or 5, characterized in that, The Shore hardness of the silicone rubber base material is 40A-60A.
7. A method for preparing a silicone rubber composite material as described in any one of claims 1-6, characterized in that, Includes the following steps: A silicone rubber base material is provided, which is then plasticized and mixed with an inorganic flame retardant, refractory filler, and heat resistant agent, followed by compounding and debinding to obtain a silicone rubber compound; and The silicone rubber compound is calendered onto a roll and then mixed with a vulcanizing agent, a nitrogen-containing compound, and a platinum complex. The mixture is then subjected to thin-pass vulcanization and vulcanization to obtain a silicone rubber composite material.
8. The method for preparing the silicone rubber composite material according to claim 7, characterized in that, The plasticizing temperature is 50℃-80℃, and the plasticizing time is 5min-8min; And / or, the mixing temperature is 50℃-80℃, and the mixing time is 10min-20min.
9. The method for preparing the silicone rubber composite material according to claim 7, characterized in that, The vulcanization temperature is 165℃-180℃, the vulcanization pressure is 5MPa-10MPa, and the vulcanization time is 6min-10min.
10. The use of a silicone rubber composite material as described in any one of claims 1-6 in pipeline products.