A high-impact, weather-resistant, and pressure-bearing PVC pipe and its preparation method
By using a composite toughening system of modified calcium carbonate, ACR resin, and organosilicon impact modifier, the problem of insufficient impact resistance and weather resistance of PVC-U pipes during the toughening process was solved, and PVC pipes with high impact resistance, high tensile strength, and low cost were prepared.
Patent Information
- Application Number
- CN202311496876.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-11-10
- Publication Date
- 2026-11-17
- Estimated Expiration
- 2043-11-10
AI Technical Summary
Existing PVC-U pipes have difficulty simultaneously achieving impact resistance, tensile strength, and weather resistance during toughening processes, and commonly used impact modifiers increase production costs and process complexity.
A composite toughening system is composed of modified calcium carbonate, ACR resin, organosilicon impact modifier, and acrylonitrile-modified EPDM rubber. Through compatibility treatment of modified calcium carbonate and PVC resin, combined with rutile titanium dioxide and antioxidants, a sea-island structure is formed to improve the toughness and weather resistance of the material.
It significantly improves the impact resistance and tensile strength of PVC pipes, while maintaining internal pressure resistance and weather resistance, reducing production costs and making them suitable for outdoor applications.
Smart Images

Figure BDA0004542971910000091 
Figure BDA0004542971910000101
Abstract
Description
Technical Field
[0001] This invention belongs to the field of plastic processing technology, specifically relating to a high-impact, weather-resistant, and pressure-bearing PVC pipe and its preparation method. Background Technology
[0002] Rigid polyvinyl chloride (PVC-U) pipes are plastic pipes manufactured by extrusion molding of polyvinyl chloride resin with certain additives. They have advantages such as light weight, corrosion resistance, smooth inner and outer walls, low flow resistance, good aging resistance, long service life, and simple construction and installation. They are widely used in building drainage and sewage, rainwater discharge, water supply and irrigation, and other fields.
[0003] Due to the low toughness and poor impact resistance of PVC, PVC-U pipes are prone to brittle fracture during storage, transportation, installation, and use, especially in low-temperature environments. Therefore, impact modifiers are often added to PVC formulations for blending with the resin, such as CPE, MBS, ACR, NBR (nitrile butadiene rubber), and SBR (styrene-butadiene rubber). However, to achieve good toughening effects, adding large amounts of elastomer toughening agents can lead to a decrease in tensile strength and heat deformation resistance. Furthermore, the molecular chains of rubber toughening agents such as MBS, NBR, and SBR contain unsaturated structures such as double bonds and benzene rings, making them susceptible to aging under oxygen and ultraviolet radiation, resulting in poor weather resistance and difficulty meeting the application requirements of products under long-term outdoor conditions. While modifying PVC with fiber materials can simultaneously improve the material's impact performance and tensile strength, the poor compatibility between fibers and PVC necessitates pre-treatment, leading to complex processes, stringent extrusion requirements, and excessively high production costs. Therefore, it is necessary to provide a PVC pipe and its preparation method that takes into account both impact performance and tensile strength, excellent hydraulic resistance, good weather resistance, easy extrusion molding, and low production cost.
[0004] Chinese Patent Publication No. CN108219326B discloses a high-impact PVC pipe formulation, comprising the following raw materials in parts by weight: PVC: 100-110; MBS resin: 6-8; ACR resin: 3-4; stabilizer: 5-7; calcium carbonate: 4-20; stearic acid: 0.3-0.4; polyethylene wax: 0.2-0.4; titanium dioxide: 1.5-3. This patent modifies PVC by combining MBS resin and ACR resin into a composite toughening agent, solving the technical defects of traditional PVC pipes, such as poor toughness and susceptibility to brittle fracture. However, the weather resistance of this patented PVC pipe still needs improvement. Summary of the Invention
[0005] The purpose of this invention is to provide a high-impact, weather-resistant, and pressure-bearing PVC pipe material that is easy to process, in order to solve the problems that commonly used impact modifiers are difficult to simultaneously achieve in toughening PVC-U pipes, have poor tensile strength and hydraulic resistance, and that some impact modifiers affect the weather resistance of the product.
[0006] The objective of this invention can be achieved through the following technical solutions:
[0007] A high-impact, weather-resistant, and pressure-bearing PVC pipe is characterized by being composed of the following raw materials in parts by weight: 90-110 parts PVC resin; 2.5-4.2 parts calcium-zinc stabilizer; 0.2-0.6 parts internal lubricant; 0.4-1.1 parts external lubricant; 0.2-0.5 parts release agent; 0.8-2.0 parts processing aid; 0.1-0.25 parts antioxidant; 3-20 parts modified calcium carbonate; 3-6 parts ACR resin; 7-15 parts toughening agent; and 1.5-2.5 parts composite microparticles.
[0008] Furthermore, the modified calcium carbonate is prepared using 3000-4000 mesh heavy calcium carbonate, which is surface-treated with stearic acid, titanate coupling agent, and potassium laurate. The preparation method is as follows: 70-100 parts by weight of heavy calcium carbonate are placed in a high-speed mixer. When the temperature rises to 75-85°C, 0.5-0.8 parts by weight of stearic acid, 1.2-1.5 parts by weight of titanate coupling agent, and 4-9 parts by weight of potassium laurate are added. The temperature is further raised to 110-115°C, and after mixing for 20-30 minutes, the high-speed mixing is stopped, the material is discharged and cooled to obtain the modified calcium carbonate.
[0009] Further, the composite microparticles are prepared as follows: 100-120 parts by weight of 1 mol / L hydrochloric acid solution are added to 1-3 parts by weight of rutile titanium dioxide and stirred. Then, 0.1-0.3 parts by weight of aniline and 0.2-0.5 parts by weight of 1 mol / L potassium persulfate solution are added. The mixture is reacted in an ice-water bath for 2-4 hours, centrifuged, washed 3-4 times with hydrochloric acid, ethanol, and distilled water, dried in an oven at 80-90℃ for 2-4 hours, and ground to obtain the composite microparticles.
[0010] Furthermore, the PVC resin is a general-purpose SG-5 type resin; the internal lubricant is one or more of aliphatic dicarboxylic acid esters, long-chain fatty acid esters, fatty acid metal soaps, and polyol fatty acid amides; and the external lubricant is one or more of polyethylene wax, Fischer-Tropsch wax, and paraffin wax.
[0011] Furthermore, the release agent is composed of high-density oxidized polyethylene wax and ethylene bis-stearamide (EBS) in a weight ratio of 0.2 to 0.4:1.
[0012] Furthermore, the processing aid is an acrylonitrile / styrene copolymer (SAN) with an intrinsic viscosity of 11-13 cP, which is mainly used to promote PVC plasticization, improve processing fluidity, and increase the heat distortion temperature and surface gloss of PVC products.
[0013] Furthermore, the antioxidant is one or more of monophenol antioxidants, bisphenol antioxidants, polyphenol antioxidants, or phosphite antioxidants.
[0014] Furthermore, the ACR resin is a core-shell structured acrylate copolymer, with a core layer of lightly cross-linked acrylate copolymer and a shell layer of polar polymethyl methacrylate (PMMA). It has good compatibility with polyvinyl chloride resin, good processing fluidity, and can give the product better toughness and low-temperature impact resistance, while improving the product's weather resistance.
[0015] Furthermore, the toughening agent comprises a silicone impact modifier and acrylonitrile-modified EPDM rubber in a weight ratio of 1.5 to 2:1. The silicone impact modifier is a core-shell copolymer composed of methyl methacrylate, acrylate, and silicone. Compared with commonly used MBS impact modifiers, the silicone impact modifier uses polysiloxane instead of butadiene with poor weather resistance in the core layer, resulting in excellent weather resistance. Compared with commonly used rubber toughening agents such as NBR and SBR, the acrylonitrile-modified EPDM rubber has more prominent ozone resistance, weather resistance, and aging resistance, and has better physical and mechanical properties and processing performance.
[0016] The present invention also provides a method for preparing the above-mentioned high-impact, weather-resistant, and pressure-bearing PVC pipe, characterized by the following steps:
[0017] (1) Preparation of the modified calcium carbonate: 70-100 parts by weight of heavy calcium carbonate of 3000-4000 mesh are placed in a high-speed mixer. When the temperature rises to 75-85°C, 0.5-0.8 parts by weight of stearic acid, 1.2-1.5 parts by weight of titanate coupling agent, and 4-9 parts by weight of potassium laurate are added. The temperature is further raised to 110-115°C. After mixing for 20-30 minutes, the high-speed mixing is stopped, the material is discharged and cooled to obtain the modified calcium carbonate.
[0018] (2) Preparation of the composite microparticles: Add 100-120 parts by weight of 1 mol / L hydrochloric acid solution to 1-3 parts by weight of rutile titanium dioxide and stir to mix. Add 0.1-0.3 parts by weight of aniline and 0.2-0.5 parts by weight of 1 mol / L potassium persulfate solution as an oxidant. React in an ice-water bath for 2-4 hours. Centrifuge, wash 3-4 times with hydrochloric acid, ethanol and distilled water, dry in an oven at 80-90℃ for 2-4 hours, and grind to obtain composite microparticles.
[0019] (3) Weigh out each raw material according to the weight proportions in the above formula;
[0020] (4) Add PVC resin, calcium-zinc stabilizer, internal lubricant, processing aid, antioxidant, ACR resin, toughening agent, and composite microparticles to a high-speed mixer and start mixing. When the temperature of the mixture reaches 80-85℃, add external lubricant, release agent, and modified calcium carbonate. Continue mixing until the temperature reaches 130-140℃. Send the mixture to a cooling mixer and stir. Cool to 42-50℃ and discharge.
[0021] (5) The cold mixture is passed through a vibrating screen to separate the powder and other residues, and then transported to a storage tank to stand and mature for 6-12 hours to obtain the prepared PVC mixture.
[0022] (6) The above-mentioned PVC compound is conveyed to a twin-screw extruder for plasticizing and extrusion. The extruder has a processing temperature of 170-210°C and a main screw speed of 25-38 rpm. The billet exit die is cooled and shaped to obtain the PVC pipe.
[0023] The beneficial effects of this invention are:
[0024] (1) The PVC pipe of this invention uses a composite toughening system composed of modified calcium carbonate, ACR resin, organosilicon impact modifier, and acrylonitrile-modified EPDM rubber. This system balances the impact performance and tensile strength of the material, significantly improving the impact resistance of the pipe while maintaining its tensile strength and internal pressure resistance. It also exhibits excellent weather resistance and corrosion resistance, making it suitable for various applications such as outdoor rainwater drainage, irrigation, water supply, underground sewage drainage, and industrial wastewater discharge. The materials used in this invention are environmentally friendly, easy to extrude, simple to prepare, and have low production costs, while also exhibiting good processing performance.
[0025] (2) This invention rationally combines modified calcium carbonate, ACR resin, silicone impact modifier, and acrylonitrile-modified EPDM rubber, adding them to PVC resin processing to achieve a synergistic effect. Specifically, ACR resin and silicone impact modifier form a so-called "sea-island" structure with the continuous PVC phase in the form of a dispersed phase, resulting in ideal toughening effect. Compared to commonly used MBS impact modifiers, silicone impact modifiers exhibit excellent weather resistance, almost no impact on material modulus, and minimal loss in pipe tensile strength and pressure resistance. The modified EPDM rubber possesses excellent weather resistance and processing performance, further enhancing the toughness and impact resistance of the pipe.
[0026] (3) The modified calcium carbonate used in the PVC pipes of this invention is prepared by surface treatment of 3000-4000 mesh heavy calcium carbonate with stearic acid and titanate coupling agent, which greatly improves the dispersion ability of calcium carbonate and its compatibility with polyvinyl chloride resin, enhances the matrix's ability to disperse and absorb impact energy, and enables calcium carbonate to achieve the effect of strengthening and toughening. Compared with the nano-grade light calcium carbonate commonly used for filler modification, the modified calcium carbonate has the advantages of low price, low oil absorption value, and better fluidity, which can reduce melt viscosity and additive dosage, give PVC formulation better processing performance, and significantly reduce product material costs.
[0027] (4) The present invention adds rutile titanium dioxide and antioxidant to the product. At the same time, each toughening component has good weather resistance, which can effectively improve the heat resistance, light resistance and aging resistance of the pipe and extend its service life.
[0028] (5) The present invention uses high-density oxidized polyethylene wax and ethylene bis-stearamide as release agents. Both have good internal and external lubrication and release ability, which can improve the fluidity and release properties of melt-blocked plastics during processing, and improve the negative impact of the use of modified heavy calcium carbonate on the appearance gloss of the product, thereby improving the surface gloss and brightness of the pipe.
[0029] (6) The processing aids and lubricants used in this invention, in addition to improving the overall dispersibility and processing performance of the material system, are also used to improve the negative impact of using rubber toughening agents on the processing fluidity of the material system, making it easier to extrude and mold. Detailed Implementation
[0030] The technical solutions of the present invention will be clearly and completely described below with reference to the embodiments of the present invention. Obviously, the described embodiments are only some embodiments of the present invention, and not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those of ordinary skill in the art without creative effort are within the scope of protection of the present invention.
[0031] Example 1
[0032] A high-impact, weather-resistant, and pressure-bearing PVC pipe comprises the following raw materials in parts by weight: 100 parts PVC resin, 3.2 parts calcium-zinc stabilizer, 0.4 parts aliphatic dicarboxylic acid ester (internal lubricant), 0.7 parts polyethylene wax (external lubricant), 0.2 parts release agent, 1.5 parts acrylonitrile / styrene copolymer (processing aid), 0.2 parts polyphenol antioxidant, 8 parts modified calcium carbonate, 4 parts ACR resin, 10 parts toughening agent, and 2 parts composite microparticles.
[0033] Furthermore, the modified calcium carbonate is prepared using 3500-mesh heavy calcium carbonate, which is surface-treated with stearic acid, titanate coupling agent, and potassium laurate. The preparation method is as follows: 100 parts by weight of heavy calcium carbonate are placed in a high-speed mixer. When the temperature rises to 80°C, 0.6 parts by weight of stearic acid, 1.2 parts by weight of titanate coupling agent, and 4 parts by weight of potassium laurate are added. The temperature is further increased to 115°C, and after mixing for 20 minutes, the high-speed mixing is stopped, the material is discharged and cooled to obtain the modified calcium carbonate.
[0034] Further, the composite microparticles are prepared as follows: 100 parts by weight of 1 mol / L hydrochloric acid solution are added to 1 part by weight of rutile titanium dioxide and stirred. Then, 0.1 parts by weight of aniline and 0.2 parts by weight of 1 mol / L potassium persulfate solution are added. The mixture is reacted in an ice-water bath for 2 hours, centrifuged, washed three times with hydrochloric acid, ethanol and distilled water, dried in an oven at 80°C for 4 hours, and ground to obtain the composite microparticles.
[0035] Furthermore, the release agent is composed of high-density oxidized polyethylene wax and ethylene bis-stearamide (EBS) in a weight ratio of 0.3:1.
[0036] Furthermore, the toughening agent comprises an organosilicon impact modifier and an acrylonitrile-modified EPDM rubber in a weight ratio of 2:1.
[0037] The method for preparing the above-mentioned high-impact, weather-resistant, and pressure-bearing PVC pipes is as follows:
[0038] (1) Weigh the PVC resin, calcium-zinc stabilizer, internal lubricant aliphatic dicarboxylic acid ester, external lubricant polyethylene wax, release agent, processing aid acrylonitrile / styrene copolymer, polyphenol antioxidant, calcium-zinc calcium carbonate, ACR resin, toughening agent combination, and composite microparticles according to the weight parts in the above formula.
[0039] (2) Add PVC resin, calcium-zinc stabilizer, internal lubricant aliphatic dicarboxylic acid ester, processing aid acrylonitrile / styrene copolymer, polyphenol antioxidant, ACR resin, toughening agent combination, and composite microparticles to a high-speed mixer and start mixing; when the temperature of the mixture reaches 80°C, add external lubricant polyethylene wax, release agent, and modified calcium carbonate, and continue mixing until 135°C. Then, send the mixture into a cooling mixer for stirring and cool it to 45°C before discharging.
[0040] (3) The cold mixture is passed through a vibrating screen to separate the powder and other residues, and then transported to a storage tank to stand and mature for 12 hours to obtain the prepared PVC mixture.
[0041] (4) Set the barrel temperature of the twin-screw extruder to 170-180°C, the die temperature to 175-190°C, the die head temperature to 205°C, and the screw speed to 30 rpm. The mixed materials are transported to the extruder for plasticizing and extrusion. After cooling and shaping, the PVC pipe is obtained.
[0042] Example 2
[0043] A high-impact, weather-resistant, and pressure-bearing PVC pipe comprises the following raw materials in parts by weight: 90 parts PVC resin, 2.5 parts calcium-zinc stabilizer, 0.2 parts internal lubricant long-chain fatty acid ester, 0.4 parts external lubricant paraffin wax, 0.2 parts release agent, 0.8 parts processing aid acrylonitrile / styrene copolymer, 0.1 parts phosphite antioxidant, 3 parts modified calcium carbonate, 3 parts ACR resin, 7 parts toughening agent, and 1.5 parts composite microparticles.
[0044] Furthermore, the modified calcium carbonate is prepared using 3500-mesh heavy calcium carbonate, which is surface-treated with stearic acid, titanate coupling agent, and potassium laurate. The preparation method is as follows: 70 parts by weight of heavy calcium carbonate are placed in a high-speed mixer. When the temperature rises to 80°C, 0.5 parts by weight of stearic acid, 1.3 parts by weight of titanate coupling agent, and 5 parts by weight of potassium laurate are added. The temperature is further increased to 115°C, and after mixing for 20 minutes, the high-speed mixing is stopped, and the material is discharged and cooled to obtain the modified calcium carbonate.
[0045] Further, the composite microparticles are prepared as follows: 110 parts by weight of 1 mol / L hydrochloric acid solution are added to 2 parts by weight of rutile titanium dioxide and stirred. Then, 0.2 parts by weight of aniline and 0.4 parts by weight of 1 mol / L potassium persulfate solution are added. The mixture is reacted in an ice-water bath for 2 hours, centrifuged, washed three times with hydrochloric acid, ethanol and distilled water, dried in an oven at 80°C for 4 hours, and ground to obtain composite microparticles.
[0046] Furthermore, the release agent is composed of high-density oxidized polyethylene wax and ethylene bis-stearamide (EBS) in a weight ratio of 0.2:1.
[0047] Furthermore, the toughening agent comprises an organosilicon impact modifier and an acrylonitrile-modified EPDM rubber in a weight ratio of 1.5:1.
[0048] The method for preparing the above-mentioned high-impact, weather-resistant, and pressure-bearing PVC pipes is as follows:
[0049] (1) Weigh the PVC resin, calcium-zinc stabilizer, internal lubricant long-chain fatty acid ester, external lubricant paraffin, release agent, processing aid acrylonitrile / styrene copolymer, phosphite antioxidant, calcium-zinc calcium carbonate, ACR resin, toughening agent combination, and composite microparticles according to the weight parts in the above formula.
[0050] (2) Add PVC resin, calcium-zinc stabilizer, internal lubricant long-chain fatty acid ester, processing aid acrylonitrile / styrene copolymer, phosphite antioxidant, ACR resin, toughening agent combination, and composite microparticles to a high-speed mixer and start mixing; when the temperature of the mixture reaches 80°C, add external lubricant paraffin wax, release agent, and modified calcium carbonate, and continue mixing until 135°C. Then, send the mixture into a cooling mixer for stirring and cool it to 45°C before discharging.
[0051] (3) The cold mixture is passed through a vibrating screen to separate the powder and other residues, and then transported to a storage tank to stand and mature for 12 hours to obtain the prepared PVC mixture.
[0052] (4) Set the barrel temperature of the twin-screw extruder to 170-180°C, the die temperature to 175-190°C, the die head temperature to 205°C, and the screw speed to 30 rpm. The mixed materials are transported to the extruder for plasticizing and extrusion. After cooling and shaping, the PVC pipe is obtained.
[0053] Comparative Example 1
[0054] Heavy calcium carbonate was added directly without modification with stearic acid, titanate coupling agent, and potassium laurate. The remaining steps were the same as in Example 1.
[0055] Comparative Example 2
[0056] No heavy calcium carbonate was added; the remaining steps were the same as in Example 1.
[0057] Comparative Example 3
[0058] The rutile titanium dioxide was not modified with hydrochloric acid solution, aniline, or potassium persulfate solution (an oxidizing agent). Instead, the rutile titanium dioxide was added directly, and the remaining steps were the same as in Example 1.
[0059] Comparative Example 4
[0060] No rutile titanium dioxide was added; the remaining steps were the same as in Example 1.
[0061] Comparative Example 5
[0062] No toughening agent was added, and the remaining steps were the same as in Example 1.
[0063] The PVC pipes prepared in Examples 1-2 and Comparative Examples 1-5 were tested for performance in accordance with GB / T 10002.1-2006 "Rigid Polyvinyl Chloride (PVC-U) Pipes for Water Supply", GB / T 13664-2006 "Rigid Polyvinyl Chloride (PVC-U) Pipes for Low-Pressure Irrigation", and QB / T 2480-2022 "Rigid Polyvinyl Chloride (PVC-U) Rainwater Pipes and Fittings for Building". The test results are shown in Table 1.
[0064] Table 1:
[0065]
[0066]
[0067] As shown in Table 1, the PVC pipes prepared in Examples 1-2 exhibited significantly higher performance in terms of impact resistance, hydraulic properties, tensile strength, and weather resistance compared to the PVC pipes in Comparative Examples 1-5. Comparing Example 1 with Comparative Example 1, the PVC pipe prepared by directly adding heavy calcium carbonate showed worse performance than the PVC pipe prepared by adding modified calcium carbonate. Comparing Comparative Example 1 with Comparative Example 2, the PVC pipe prepared without adding heavy calcium carbonate showed worse performance than the PVC pipe prepared with heavy calcium carbonate. Comparing Example 1 with Comparative Example 3, the PVC pipe prepared by directly adding rutile titanium dioxide showed worse performance than the PVC pipe prepared with modified rutile titanium dioxide. Comparing Example 3 with Example 4, the PVC pipe prepared without adding rutile titanium dioxide showed worse performance than the PVC pipe prepared with rutile titanium dioxide. Comparing Example 1 with Comparative Example 5, the PVC pipe prepared without adding toughening agent showed worse performance than the PVC pipe prepared with toughening agent.
[0068] It should be noted that, in this document, relational terms such as "first" and "second" are used only to distinguish one entity or operation from another, and do not necessarily require or imply any such actual relationship or order between these entities or operations. Furthermore, the terms "comprising," "including," or any other variations thereof are intended to cover non-exclusive inclusion, such that a process, method, article, or apparatus that comprises a list of elements includes not only those elements but also other elements not expressly listed, or elements inherent to such process, method, article, or apparatus.
[0069] Although embodiments of the invention have been shown and described, it will be understood by those skilled in the art that various changes, modifications, substitutions and alterations can be made to these embodiments without departing from the principles and spirit of the invention, the scope of which is defined by the appended claims and their equivalents.
Claims
1. A high-impact, weather-resistant, and pressure-bearing PVC pipe, characterized in that, It is composed of the following raw materials in parts by weight: 90-110 parts PVC resin; 2.5-4.2 parts calcium-zinc stabilizer; 0.2-0.6 parts internal lubricant; 0.4-1.1 parts external lubricant; 0.2-0.5 parts release agent; 0.8-2.0 parts processing aid; 0.1-0.25 parts antioxidant; 3-20 parts modified calcium carbonate; 3-6 parts ACR resin; 7-15 parts toughening agent; 1.5-2.5 parts composite microparticles; The toughening agent comprises an organosilicon impact modifier in a weight ratio of 1.5 to 2:1 and acrylonitrile-modified EPDM rubber. The organosilicon impact modifier is a core-shell copolymer composed of methyl methacrylate, acrylate and organosilicon. The composite microparticles are prepared by the following method: 100-120 parts by weight of 1 mol / L hydrochloric acid solution are added to 1-3 parts by weight of rutile titanium dioxide and stirred. Then, 0.1-0.3 parts by weight of aniline and 0.2-0.5 parts by weight of 1 mol / L potassium persulfate solution are added. The mixture is reacted in an ice-water bath for 2-4 hours, centrifuged, washed 3-4 times with hydrochloric acid, ethanol, and distilled water, dried in an oven at 80-90℃ for 2-4 hours, and then ground to obtain the final product. The processing aid is an acrylonitrile / styrene copolymer with an intrinsic viscosity of 11-13 cP.
2. A method for preparing the high-impact, weather-resistant, and pressure-bearing PVC pipe as described in claim 1, characterized in that, Follow these steps: (1) Preparation of the modified calcium carbonate: 70-100 parts by weight of heavy calcium carbonate of 3000-4000 mesh are placed in a high-speed mixer. When the temperature rises to 75-85℃, 0.5-0.8 parts by weight of stearic acid, 1.2-1.5 parts by weight of titanate coupling agent, and 4-9 parts by weight of potassium laurate are added. The temperature is further raised to 110-115℃. After mixing for 20-30 minutes, the high-speed mixing is stopped, the material is discharged and cooled to obtain the modified calcium carbonate. (2) Prepare the composite microparticles; (3) Weigh out each raw material according to the weight proportions in the formula; (4) Add PVC resin, calcium-zinc stabilizer, internal lubricant, processing aid, antioxidant, ACR resin, toughening agent, and composite microparticles to a high-speed mixer and start mixing. When the temperature of the mixture reaches 80-85℃, add external lubricant, release agent, and modified calcium carbonate. Continue mixing until the temperature reaches 130-140℃. Send the mixture to a cooling mixer and stir. Cool to 42-50℃ and discharge. (5) The cold mixture is passed through a vibrating screen to separate the powder residue, and then transported to a storage tank for standing and maturation for 6-12 hours to obtain the prepared PVC mixture. (6) The above-mentioned PVC compound is conveyed to a twin-screw extruder for plasticizing and extrusion. The extruder has a processing temperature of 170-210°C and a main screw speed of 25-38 rpm. After the billet exit die is cooled and shaped, the high-impact, weather-resistant, and pressure-bearing PVC pipe is obtained.
3. The high-impact, weather-resistant, and pressure-bearing PVC pipe according to claim 1, characterized in that, The PVC resin is a general-purpose SG-5 type resin; the internal lubricant is one or more of aliphatic dicarboxylic acid esters, long-chain fatty acid esters, fatty acid metal soaps, and polyol fatty acid amides; the external lubricant is one or more of polyethylene wax, Fischer-Tropsch wax, and paraffin wax.
4. The high-impact, weather-resistant, and pressure-bearing PVC pipe according to claim 1, characterized in that, The release agent is composed of high-density oxidized polyethylene wax and ethylene bis-stearamide in a weight ratio of 0.2 to 0.4:
1.
5. The high-impact, weather-resistant, and pressure-bearing PVC pipe according to claim 1, characterized in that, The antioxidant is one or more of monophenol antioxidants, bisphenol antioxidants, polyphenol antioxidants, or phosphite antioxidants.
6. The high-impact, weather-resistant, and pressure-bearing PVC pipe according to claim 1, characterized in that, The ACR resin is a core-shell structured acrylate copolymer, with a core layer being a lightly cross-linked acrylate copolymer and a shell layer being a polar polymethyl methacrylate.
Citation Information
Patent Citations
A high-impact PVC pipe formulation and its preparation method
CN108219326B
Impact-resistant modified polyvinyl chloride tube material and preparation process thereof
CN101775180A
Modified titanium dioxide preparation method
CN107227510A
Antioxidant PVC communication pipe and preparation method thereof
CN111548578A
Superfine calcium carbonate filler for PVC (polyvinyl chloride) cable as well as preparation method and application of superfine calcium carbonate filler
CN116396533A