A method for preparing a proton exchange membrane with a wrinkled surface and a water electrolysis membrane electrode.
By forming a uniform wrinkled structure on the surface of the proton exchange membrane through solution impregnation, the problem of preparing large-area membrane electrodes in the prior art has been solved, and the preparation of water electrolysis membrane electrodes with larger contact area and lower energy consumption has been achieved, which is suitable for mass production.
Patent Information
- Application Number
- CN202311241959.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-09-25
- Publication Date
- 2026-11-10
- Estimated Expiration
- 2043-09-25
AI Technical Summary
Existing technologies make it difficult to prepare proton exchange membranes with wrinkled surfaces on a large scale without relying on specific equipment and molds, which limits the contact area between the membrane and the catalyst layer, resulting in high electrochemical polarization and high energy consumption for hydrogen production.
A uniformly distributed wrinkled structure was formed on the surface of a proton exchange membrane by solution impregnation. An oxidant was added to a ruthenium precursor solution and the pH was adjusted. The membrane was then treated in a sulfuric acid solution in a water bath to prepare a proton exchange membrane with a wrinkled surface. This membrane was then combined with traditional processes to prepare a water electrolysis membrane electrode.
It increases the specific surface area of the proton exchange membrane, enhances the three-phase reaction interface, and reduces the energy consumption of electrolytic hydrogen production, making it suitable for batch processing and large-scale production.
Smart Images

Figure CN117385411B_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of solid polymer water electrolysis hydrogen production technology, and in particular to a method for preparing a proton exchange membrane with a wrinkled surface and a water electrolysis membrane electrode. Background Technology
[0002] Solid-state polymer water electrolysis is a highly efficient and long-life hydrogen production technology. Currently, reducing the single-cell voltage of the electrolyzer is an effective way to reduce hydrogen production costs and promote the large-scale application of this technology. The membrane electrode assembly (MEA), a core component of the water electrolyzer, is crucial to the overall energy consumption of hydrogen production in the stack. Electrochemical polarization is a major component of MEA energy consumption; therefore, reducing MEA electrochemical polarization can effectively lower hydrogen production energy consumption and is a current main research direction.
[0003] In researching ways to improve membrane electrode efficiency, expanding the three-phase reaction interface between the proton exchange membrane and the catalyst layer is an effective technique for reducing electrochemical polarization. Currently, commercially available proton exchange membranes have a completely flat surface. When fabricated as a membrane electrode, the contact surface between the catalyst layer and the membrane is only a two-dimensional plane, thus limiting the contact area between the membrane and the catalyst layer. To expand the contact area between the catalyst layer and the membrane, nanoimprinting and plasma etching techniques have been developed to increase the specific surface area of proton exchange membranes. However, these techniques heavily rely on specific equipment and imprinting molds, and are difficult to use for the fabrication of large-area membrane electrodes, thus limiting their application in large-scale fabrication.
[0004] Wrinkled morphology can increase the specific surface area of proton exchange membranes, but the only current preparation method uses thermosetting elastic molds (PDMS) as imprint templates, followed by hot pressing with the proton exchange membrane. As mentioned earlier, this method has the disadvantages of relying on specific molds, having many steps, and being difficult to use for the preparation of large-area membrane electrodes. Summary of the Invention
[0005] The purpose of this invention is to provide a method for preparing a proton exchange membrane and a water electrolysis membrane electrode with a wrinkled surface. This invention achieves surface wrinkling of the proton exchange membrane and enhances the performance of the water electrolysis membrane electrode. The method for preparing a proton exchange membrane with a wrinkled surface proposed in this invention can promote the transformation of the proton exchange membrane surface from a two-dimensional flat morphology to a three-dimensional wrinkled morphology without the use of molds or specific equipment. Membranes with this type of morphology exhibit a larger specific surface area.
[0006] This invention is achieved through the following technical solutions:
[0007] This invention protects a method for preparing a proton exchange membrane with a wrinkled surface, comprising the following steps:
[0008] (1) Add an oxidant to the ruthenium precursor solution, with a molar ratio of oxidant to ruthenium precursor of 1:1-8:1, and adjust the pH of the solution to 8-12;
[0009] (2) At room temperature, place the proton exchange membrane in the above solution and let it stand for 0.5-72 hours. After rinsing, place it in a sulfuric acid solution at 70℃-90℃ for 0.5-1.5 hours and then dry it to obtain a proton exchange membrane with a wrinkled surface. The drying temperature is 70℃-90℃.
[0010] The method for preparing a surface-wrinkled proton exchange membrane proposed in this invention is an easy-to-implement solution impregnation method, which can achieve wrinkling treatment of large-area membrane materials, and is therefore suitable for mass production of membrane materials.
[0011] Preferably, the concentration of the ruthenium precursor solution in step (1) is 0.01-0.5 M. The ruthenium precursor solution is prepared by dissolving ruthenium precursor powder in deionized water to obtain a ruthenium precursor solution with a concentration of 0.01-0.5 M. More preferably, the ruthenium precursor is RuCl3.
[0012] Preferably, the oxidant in step (1) is NaClO or H2O2, and the molar ratio of the oxidant to the ruthenium precursor is 2:1-8:1. H2O2 is preferably a 30% (w / w) aqueous solution of H2O2.
[0013] Preferably, the specific steps of adjusting the solution pH to 8-12 in step (1) are as follows: adjusting the solution pH to 8-12 by adding an alkaline solution or a phosphate buffer solution. More preferably, the alkaline solution is a sodium hydroxide solution, and the phosphate buffer solution is a sodium phosphate buffer (NaH2PO4 & Na2HPO4) and a potassium phosphate buffer (K2HPO4 & KH2PO4).
[0014] Preferably, the specific steps of step (2) of water bathing in sulfuric acid solution at 70℃-90℃ for 0.5-1.5 hours are as follows: water bathing in sulfuric acid solution at 80℃ for 1 hour.
[0015] The present invention also protects a proton exchange membrane with surface wrinkles prepared by the preparation method described above, wherein the surface of the proton exchange membrane exhibits uniformly distributed wrinkles with a wrinkle size of 50-200 nm.
[0016] Preferably, the proton exchange membrane is a perfluorosulfonic acid polymer membrane or a perfluorosulfonic acid polymer reinforced membrane, and the thickness of the proton exchange membrane is 25-200 μm. More preferably, the proton exchange membrane is a Nafion 117 membrane, Nafion 115 membrane, Nafion 212 membrane, or Nafion HP reinforced membrane.
[0017] This invention also protects a water electrolysis membrane electrode, comprising a surface-wrinkled proton exchange membrane and a cathode catalyst layer and an anode catalyst layer disposed on both sides of the proton exchange membrane. The water electrolyzer membrane electrode obtained by combining the surface-wrinkled proton exchange membrane with a conventional electrode preparation method exhibits a larger active area and higher activity, effectively reducing the energy consumption for hydrogen production via electrolysis.
[0018] The present invention also protects the preparation method of the water electrolysis membrane electrode, which includes the following steps: preparing cathode catalyst ink and anode catalyst ink, and combining them with the surface-wrinkled proton exchange membrane by coating, spraying or transfer method to obtain cathode catalyst layer and anode catalyst layer disposed on both sides of the proton exchange membrane, thereby obtaining the water electrolysis membrane electrode (solid polymer water electrolysis membrane electrode).
[0019] Compared with the prior art, the beneficial effects of the present invention are:
[0020] 1. This invention provides a method for preparing a proton exchange membrane by wrinkling it. This method can increase the specific surface area of the proton exchange membrane and form an expanded three-phase reaction interface. Combined with traditional membrane electrode preparation processes, this results in better membrane electrode performance.
[0021] 2. This invention uses a simple solution impregnation method to promote wrinkling on the surface of the proton exchange membrane. This method is simpler than the traditional nanotemplate imprinting method, requires no specific equipment, and is suitable for mass production of membranes and large-scale production of membrane electrodes. Attached Figure Description
[0022] Figure 1 This is a surface morphology diagram of the proton exchange membrane with surface wrinkling obtained in Example 1;
[0023] Figure 2 Schematic diagrams of the membrane electrode prepared according to the present invention and a conventional membrane electrode;
[0024] Figure 3 The cyclic voltammetry curves of the anode of the water electrolyzer obtained in Example 1 and Comparative Example 1 are shown, where 1 represents the membrane electrode obtained in Comparative Example 1 and 2 represents the membrane electrode obtained in Example 1.
[0025] Figure 4 The water electrolysis polarization curves are prepared using the membrane electrodes of Comparative Example 1 and Example 1, where 1 represents the membrane electrode of Comparative Example 1 and 2 represents the membrane electrode obtained in Example 1. Detailed Implementation
[0026] The present invention will be further described in detail below with reference to the embodiments. These embodiments are for illustrative purposes only and are not intended to limit the scope of the invention. Experimental methods in the following embodiments that do not specify specific conditions are generally performed under conventional conditions in the art or as recommended by the manufacturer; the raw materials and reagents used, unless otherwise specified, are considered to be commercially available materials and reagents that can be obtained through conventional markets and other commercial channels.
[0027] A method for preparing a water electrolysis membrane electrode includes the following steps:
[0028] (1) Dissolve the ruthenium precursor powder in deionized water at a concentration of 0.01-0.5M, then add an oxidant, wherein the molar ratio of the oxidant to the ruthenium precursor is 1:1-8:1, and then gradually adjust the pH of the solution to 8-12 to obtain a pale yellow transparent solution;
[0029] (2) At room temperature, the proton exchange membrane was placed in the above solution and left to stand for 0.5-72 hours. After being taken out, it was rinsed in deionized water, then placed in a sulfuric acid solution at 70℃-90℃ for 0.5-1.5 hours and dried at 70℃-90℃ to obtain a proton exchange membrane with a wrinkled surface.
[0030] (3) Prepare cathode catalyst ink and anode catalyst ink, and combine them with a proton exchange membrane (solid polymer membrane) with a surface pleated by coating, spraying or transfer method to obtain a (solid polymer) water electrolysis membrane electrode.
[0031] The ruthenium precursor solution was prepared by dissolving ruthenium precursor powder in deionized water to obtain a ruthenium precursor solution with a concentration of 0.01-0.5 M. In the following examples, RuCl3 is preferred as the ruthenium precursor.
[0032] In the following embodiments, the preferred oxidant in step (1) is NaClO or H2O2, the molar ratio of the oxidant to the ruthenium precursor is 2:1-8:1, and the preferred H2O2 is an aqueous solution with a mass fraction of 30%.
[0033] In the following embodiments, it is preferred that the pH of the solution be adjusted to 8-12 by adding an alkaline solution or a phosphate buffer solution. More preferably, the alkaline solution is a sodium hydroxide solution, and the phosphate buffer solution is a sodium phosphate buffer (NaH2PO4 & Na2HPO4) and a potassium phosphate buffer (K2HPO4 & KH2PO4).
[0034] In the following embodiments, it is preferred that in step (2), the sulfuric acid solution is heated in a water bath at 80°C for 1 hour, the drying temperature is 80°C, and the concentration of the sulfuric acid solution is 0.5M.
[0035] The proton exchange membrane with surface wrinkles obtained in step (2) exhibits uniformly distributed wrinkles with a wrinkle size of 50-200 nm. The proton exchange membrane is a perfluorosulfonic acid polymer membrane or a perfluorosulfonic acid polymer reinforced membrane, and the thickness of the proton exchange membrane is 25-200 μm. More preferably, the proton exchange membrane is a Nafion 117 membrane, a Nafion 115 membrane, a Nafion 212 membrane, or a Nafion HP reinforced membrane.
[0036] In the following embodiments, conventional cathode catalyst ink and anode catalyst ink preparation processes are preferably employed. Anode catalyst is prepared by adding pure water, isopropanol, and a 5% (w / w) perfluorosulfonic acid resin solution to prepare an anode catalyst ink. The mass ratio of anode catalyst to pure water to isopropanol is 1:5:15. This ink is then applied to one side of a proton exchange membrane with a wrinkled surface using coating, spraying, or transfer methods at 60°C. Cathode catalyst is prepared by adding pure water, isopropanol, a 5% (w / w) perfluorosulfonic acid resin solution, and a 60% (w / w) polytetrafluoroethylene emulsion to prepare a cathode catalyst ink. The mass ratio of cathode catalyst, pure water, and isopropanol is 1:8:10, and the mass ratio of perfluorosulfonic acid resin to polytetrafluoroethylene is 4:9. A cathode catalyst layer is then formed on the other side of the solid polymer membrane loaded with the anode catalyst layer using coating, spraying, or transfer methods at 60°C.
[0037] The cathode catalyst is a platinum-carbon catalyst with a platinum loading of 20%, and the platinum loading of the cathode catalyst layer is 0.1 mg·cm³. -2 The anode catalyst is iridium oxide, and the iridium loading in the anode catalyst layer is 0.5 mg·cm³. -2 The cathode catalyst ink contains 15% Nafion, while the anode catalyst ink contains 10% Nafion.
[0038] In the following embodiments, coating, spraying, or transfer methods are acceptable as long as they can achieve the bonding of the cathode catalyst ink, the anode catalyst ink, and the proton exchange membrane (solid polymer membrane) with surface pleats. The specific coating, spraying, or transfer methods are not specifically limited. For example, the process parameters for spraying are as follows: spraying flow rate 6-15 mL / min, suction cup heating temperature 80℃-130℃, and nozzle height distance from suction cup height 20-40 cm. Any method that can achieve the technical objective of this invention is acceptable.
[0039] Example 1
[0040] A method for preparing a water electrolysis membrane electrode includes the following steps:
[0041] (1) Take 0.05 mol RuCl3 and add it to 100 mL of deionized water to prepare a 0.5 M solution. Then add 0.1 mol of oxidant NaClO to make the molar ratio of oxidant to ruthenium precursor 2:1. Then stir evenly.
[0042] (2) Add NaOH solution to the solution obtained in step (1) to adjust the pH to 10. After standing at room temperature for 20 minutes, a pale yellow transparent solution is obtained.
[0043] (3) Take a Nafion117 membrane with a thickness of 200 μm and immerse it directly in the solution of step (2) for 24 hours. Then take it out, wash it three times with deionized water, blow the surface with nitrogen, and finally place the Nafion117 membrane in 0.5 M H2SO4 and bathe it at 80°C for 1 hour, and dry it at 80°C.
[0044] (4) The traditional cathode catalyst ink and anode catalyst ink preparation process is adopted. The cathode uses a platinum-carbon catalyst with a platinum loading of 20% and a platinum loading of 0.1 mg·cm³. -2 The anode uses iridium oxide as a catalyst with an iridium loading of 0.5 mg·cm³. -2 The cathode catalyst ink contains 15% Nafion, and the anode catalyst ink contains 10% Nafion. The prepared ink is sprayed onto the surface of the pleated proton exchange membrane using a spraying method, and after drying, the water electrolyzer membrane electrode with expanded interface is obtained.
[0045] The single-cell electrochemical active area of the water electrolyzer is 8 cm². 2 Single-cell polarization curve testing was conducted at 80℃ and normal pressure, using a multimeter to measure steady-state voltages at different current densities. In in-situ cyclic voltammetry measurements, the anode was used as the working electrode, and the cathode as both the counter and reference electrode. The potential scan range was 0.2–1.2 V (vs RHE), and the scan rate was 20 mV / s.
[0046] Figure 1 The image shows the surface morphology of the proton exchange membrane prepared in this embodiment. It can be seen that the membrane surface is completely covered by wrinkled morphology, indicating that this method can form a large number of wrinkled structures on the membrane surface.
[0047] Figure 2 The diagram shows a cross-section of the membrane electrode. As can be seen from the figure, the contact surface between the catalyst layer and the membrane in a conventional membrane electrode is a flat structure, while the membrane prepared using this invention exhibits a wavy, textured structure, thus providing a larger catalyst layer / membrane interface per unit area.
[0048] Figure 4 Water electrolysis polarization curves prepared using conventional membrane electrodes and the membrane electrode of the present invention. Using the membrane electrode of the present invention at 1 A / cm... 2 The voltage of a single slot is only 1.666V (curve 2).
[0049] Comparative Example 1
[0050] The difference between Comparative Example 1 and Example 1 is that untreated commercial Nafion 117 membrane was used, while the other membrane electrode preparation processes and testing conditions were exactly the same as in Example 1.
[0051] Figure 3 The figures shown are the in-situ cyclic voltammetry curves of the anode in water electrolysis. Since the integral area of the cyclic voltammetry curve is positively correlated with the three-phase reaction interface of the membrane electrode, a larger integral area represents a larger reaction interface. It can be seen that the membrane electrode prepared using Example 1 (dashed line) has a larger reaction interface than the conventional membrane electrode (Comparative Example 1, solid line).
[0052] Figure 4 Curve 1 is the membrane electrode polarization curve of Comparative Example 1 using the untreated proton exchange membrane. It can be seen that under the same loading, the membrane electrode at 1 A / cm 2 The voltage of the lower single cell is 1.758V, and the energy consumption for hydrogen production is higher than that of the membrane electrode prepared in this invention.
[0053] Example 2
[0054] The difference between this embodiment and Example 1 is as follows: the concentration of the ruthenium solution prepared in step (1) is 0.01M, and the molar ratio of the oxidant NaClO to the ruthenium precursor is 8:1. In step (2), a phosphate buffer solution is used to adjust the pH to 8. In step (4), the catalyst layer is prepared using a coating process; the remaining steps and testing methods are completely consistent with Example 1. Single-cell test of the water electrolyzer membrane electrode at 1 A / cm 2 The voltage of a single cell is 1.709V, indicating that the energy consumption for hydrogen production is lower than that of a traditional membrane electrode (Comparative Example 1).
[0055] Example 3
[0056] The difference between this embodiment and Embodiment 1 is that a Nafion 115 membrane with a thickness of 120 μm is used in step (3), and the immersion time is 72 hours. All other steps and testing methods are completely consistent with Embodiment 1. Single-cell water electrolyzer test: 1 A / cm 2 The single-slot voltage is 1.645V, which is better than that of Comparative Example 1.
[0057] Example 4
[0058] The difference between this embodiment and Example 1 is that: in step (3), a 25 μm thick Nafion HP enhanced membrane is used, and the immersion time is 0.5 hours. In step (4), the catalyst layer is prepared by transfer printing. The remaining steps and testing methods are completely consistent with Example 1. Single-cell performance test 1 A / cm 2 The single-slot voltage is only 1.575V, which is better than Comparative Example 1.
[0059] Example 5
[0060] The difference between this embodiment and Embodiment 1 is that: in step (1), the concentration of the ruthenium precursor used is 0.1M, and the added oxidant is H2O2 with a mass fraction of 30%, wherein the molar ratio of H2O2 to the ruthenium precursor is 8:1. In step (2), NaOH solution is used to adjust the pH to 12. The remaining steps and testing methods are completely consistent with those of Embodiment 1. Single-tank performance test 1A / cm 2 The single-slot voltage is only 1.685V, which is better than Comparative Example 1.
[0061] The above description of the embodiments is only for the purpose of helping to understand the technical solution and core idea of the present invention. It should be noted that for those skilled in the art, several improvements and modifications can be made to the present invention without departing from the principle of the present invention, and these improvements and modifications also fall within the protection scope of the claims of the present invention.
Claims
1. A method for preparing a proton exchange membrane with a wrinkled surface, characterized in that, Includes the following steps: (1) Add an oxidant to the ruthenium precursor solution, the molar ratio of the oxidant to the ruthenium precursor is 1:1-8:1, adjust the pH of the solution to 8-12, the ruthenium precursor is RuCl3, and the oxidant is NaClO or H2O2; (2) Under room temperature conditions, the proton exchange membrane is placed in the above solution and left to stand for 0.5-72 hours. The proton exchange membrane is a perfluorosulfonic acid type polymer membrane or a perfluorosulfonic acid type polymer reinforced membrane. After rinsing, it is placed in a sulfuric acid solution at 70℃-90℃ for 0.5-1.5 hours. The concentration of the sulfuric acid solution is 0.5 M. After drying, a proton exchange membrane with a wrinkled surface is obtained.
2. The preparation method according to claim 1, characterized in that, The concentration of the ruthenium precursor solution in step (1) is 0.01-0.5 M.
3. The preparation method according to claim 1, characterized in that, The molar ratio of the oxidant to the ruthenium precursor in step (1) is 2:1-8:
1.
4. The preparation method according to claim 1 or 2, characterized in that, The specific steps for adjusting the solution pH to 8-12 in step (1) are as follows: adjust the solution pH to 8-12 by adding an alkaline solution or a phosphate buffer solution.
5. The preparation method according to claim 1 or 2, characterized in that, The specific steps of step (2) of water bathing in sulfuric acid solution at 70℃-90℃ for 0.5-1.5 hours are as follows: water bathing in sulfuric acid solution at 80℃ for 1 hour.
6. A proton exchange membrane with surface wrinkles prepared by the preparation method according to claim 1, characterized in that, The surface of the proton exchange membrane exhibits uniformly distributed wrinkles.
7. The proton exchange membrane according to claim 6, characterized in that, The proton exchange membrane is a perfluorosulfonic acid polymer membrane or a perfluorosulfonic acid polymer reinforced membrane, and the thickness of the proton exchange membrane is 25-200 μm.
8. A water electrolysis membrane electrode, characterized in that, It is composed of the proton exchange membrane with surface pleats as described in claim 6, and a cathode catalyst layer and an anode catalyst layer disposed on both sides of the proton exchange membrane.
9. A method for preparing the water electrolysis membrane electrode according to claim 8, characterized in that, The process includes the following steps: preparing cathode catalyst ink and anode catalyst ink, and combining them with the proton exchange membrane with the surface pleats described in claim 6 using coating, spraying or transfer methods to obtain a cathode catalyst layer and an anode catalyst layer disposed on both sides of the proton exchange membrane, thereby obtaining the water electrolysis membrane electrode.
Citation Information
Patent Citations
Membrane electrode and preparation method and application thereof
CN115763838A
Electrode of a wrinkle structure, display device having the same and method of fabricating the same
KR1020150088565A